A high-performance composite fluorescent ceramic for laser lighting and its preparation method

By coating the fluorescent ceramic with high thermal conductivity materials and coating red phosphor to form high-performance composite ceramics, the problems of reduced lighting efficiency and insufficient thermal conductivity of traditional LEDs are solved, and the laser lighting effect with high brightness and high efficiency is achieved.

CN116835983BActive Publication Date: 2024-11-22XUZHOU NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310918738.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-24
Publication Date
2024-11-22
Estimated Expiration
2043-07-24

AI Technical Summary

Technical Problem

Traditional LED lighting technology has reduced efficiency at high power, and the thermal conductivity of fluorescent ceramics is limited, resulting in difficulty in heat dissipation and complex structure, making it difficult to achieve high brightness and high efficiency laser lighting.

Method used

The cube Ce:LuAG fluorescent ceramic is coated with a high thermal conductivity coating material, and the surface is coated with red phosphor. It forms a high-performance composite fluorescent ceramic through sintering, which improves thermal conductivity and color development index, enhances thermal resistance and light scattering effect. .

Benefits of technology

Achieved small-size and high-brightness laser illumination, the thermal conductivity is increased to 28-32Wm-1K-1, the emission intensity loss is only 2.3-4.1%, the luminous efficiency can reach up to 260lm/w, and the color rendering index reaches 81-88, which is significant. Improved laser lighting effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116835983B_ABST
    Figure CN116835983B_ABST
Patent Text Reader

Abstract

The invention discloses a high-performance composite fluorescent ceramic for laser lighting and a preparation method thereof. A high thermal conductivity ceramic powder is used to coat a cubic Ce: LuAG fluorescent ceramic, wherein the side length of the cubic fluorescent ceramic is 0.5 mm-1 mm. After being sintered into a block ceramic, a red fluorescent powder is coated and sintered again to obtain a composite fluorescent ceramic. The high thermal conductivity ceramic powder is selected from Al 2 O 3 , MgO, AlN, BN, BeO, SiC. The thermal conductivity of the composite fluorescent ceramic is 28Wm ‑1 K ‑1 ‑32Wm ‑1 K ‑1 At 150°C, the emission intensity only loses 2.3%-4.1%. Using 460nm blue light LD excitation, the luminous efficiency can reach up to 260lm / w at a power of 5W, and the color rendering index is 81-88; it not only meets the requirements of small size and high brightness, but also has excellent resistance to thermal quenching, and the ceramic has good heat dissipation. After coating with red powder, a higher color rendering index can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluorescent materials, and in particular to a high-performance composite fluorescent ceramic for laser lighting and a preparation method thereof. Background Art

[0002] Laser lighting technology and LED lighting technology are both solid-state lighting technologies. Due to their advantages such as long life, low energy consumption and environmental friendliness, they are considered by academia and industry to be the most promising green lighting sources in the 21st century. However, due to the efficiency drop caused by Auger recombination, traditional LEDs can only maintain a high luminous efficiency under low current density injection. Therefore, the overall brightness can only be improved by increasing the number of LEDs, but this solution is also accompanied by disadvantages such as heat accumulation, complex structure, and increased cost. In comparison, laser lighting technology based on laser diodes can still maintain a high luminous efficiency in the field of high-power lighting, and has significant advantages such as higher brightness, smaller size, longer life, and longer search distance.

[0003] At present, the common method of obtaining white light on the market is to use a combination of blue light-emitting diodes and yellow fluorescent conversion materials. Due to high-power laser irradiation, in order to obtain good heat dissipation effects, fluorescent conversion materials must have good thermal properties, so fluorescent ceramics have received widespread attention. However, in order to obtain better thermal conductivity, high thermal conductivity composite phases such as Al2O3 (32-35w m -1 K -1 )、MgAl2O4(22w m -1 K -1 ), MgO(47.2wm -1 K -1 -53.5wm -1 K -1 ), which can both improve their thermal conductivity and increase light scattering to increase blue light absorption.

[0004] However, the thermal conductivity improved by this method of adding two phases is limited. The method of using a high thermal conductivity coating material to wrap fluorescent ceramics can improve the thermal conductivity to a greater extent, and can limit the divergence of light, playing a role of convergence, which is very suitable for application in laser lighting and display. For example, patent CN 111285680 A proposes a fluorescent ceramic device with a edging structure: the fluorescent ceramic and the non-luminescent ceramic are sintered separately, and then combined together for application in laser lighting systems. However, in order to maintain the stable operation of fluorescent ceramics, additional heat dissipation devices are still needed; on the other hand, the two-step sintering process is complicated, and there are certain difficulties in achieving a close fit between the edging arc and the wafer, which makes it difficult for the fluorescent ceramic to conduct and radiate heat. Summary of the invention

[0005] In view of the above-mentioned technical deficiencies, the purpose of the present invention is to provide a high-performance composite fluorescent ceramic for laser lighting and a preparation method thereof. The composite fluorescent ceramic adopts a coating material to coat the fluorescent ceramic, which can not only achieve the requirements of small size and high brightness, but also has excellent resistance to thermal quenching, and the ceramic has good heat dissipation. After coating with red powder, a higher color rendering index can be achieved.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] One object of the present invention is to provide a high-performance composite fluorescent ceramic for laser lighting, wherein a cubic Ce: LuAG fluorescent ceramic is coated with a high thermal conductivity coating material, wherein the cubic ceramic has a side length of 0.5-1 mm, and after sintering to form a block ceramic, a red fluorescent powder is coated, wherein the red fluorescent powder is selected from nitride red powder CaAlSiN3: Eu 2+ or fluoride K2(Si / Ge / Ti)F6:Mn 4+ and sintering again to obtain the composite fluorescent ceramic.

[0008] Furthermore, the high thermal conductivity ceramic powder is selected from any one of Al2O3, MgO, AlN, BN, BeO, and SiC.

[0009] Furthermore, the thermal conductivity of the composite fluorescent ceramic is 28-32Wm -1 K -1 At 150℃, the emission intensity only loses 2.3-4.1%. Using 460nm blue light LD excitation, the luminous efficiency can reach up to 260lm / w at a power of 5W, and the color rendering index is 81-88.

[0010] Another object of the present invention is to provide a method for preparing a high-performance composite fluorescent ceramic for laser lighting, comprising the following steps:

[0011] S1: Preparation of Ce:LuAG;

[0012] S1-1 ingredients: Lutetium oxide, aluminum oxide, and cerium oxide are weighed according to the stoichiometric ratio of each element in Ce:LuAG, and 0.3wt.%-1wt.% MgO and TEOS are added as sintering aids, and the mixture is ball-milled;

[0013] S1-2 tableting: drying and sieving the mixed powder, and using a steel mold to dry and press the sieved powder into a tablet;

[0014] S1-3 vacuum sintering: placing the pressed green billet into a vacuum sintering furnace to sinter the green billet;

[0015] S1-4 polishing and cutting: polishing and cutting the upper and lower surfaces of the sintered ceramic to obtain cubic Ce: LuAG ceramics;

[0016] S2: Preparation of composite fluorescent ceramics;

[0017] S2-1 Preparation of coated green blank: weigh 3-5g of coating material and put it into a mold, dry and press the steel mold to obtain a coated ceramic green blank;

[0018] S2-2 performs coating: taking out the ejector pin of the die casting mold, placing the cubic Ce: LuAG ceramic cut in step S1 in the center of the coated ceramic blank, and pressing the cubic Ce: LuAG ceramic into the coated ceramic blank;

[0019] S2-3 sintering: sintering the coated ceramic and double-sided polishing to obtain a bulk ceramic;

[0020] S2-5 coating red powder: using PIG to mix red phosphor, wherein the mass ratio of PIG to red phosphor is 10:1-3:1, and the coating thickness is 70-150 μm; sintering again to obtain a composite fluorescent ceramic.

[0021] Furthermore, in step S1-1, the ball milling time is 24-48 hours; and the ball milling speed is 140-150 r / min.

[0022] Furthermore, in step S1-2, the drying temperature is 40-65°C, the drying time is 15-20h; the sieving mesh number is 100-200 mesh; and the pressure of the steel mold drying and pressing is 15-25MPa.

[0023] Furthermore, in step S1-3, the vacuum sintering temperature is 1760-1800°C, and the holding time is 8-20h.

[0024] Furthermore, in step S2-1, the pressure of the steel mold drying and pressing is 3-5 MPa.

[0025] Furthermore, in step S2-3, the sintering method is to place the mixture in a muffle furnace or an atmosphere furnace for sintering, the sintering temperature is 1300-1650°C, and the temperature is kept for 8-12 hours.

[0026] The beneficial effects of the present invention are:

[0027] 1. The composite fluorescent ceramic provided in this application has a center size of only 0.25 mm 2 -1mm 2 Compared with the fluorescent surface of existing lighting devices, it has a smaller light-emitting area and higher efficiency, up to 260lm / w;

[0028] 2. The composite fluorescent ceramic obtained by the preparation method of the present invention is tightly coated with a high thermal conductivity coating material, the coating material and the fluorescent ceramic are tightly fitted, the heat dissipation performance is better, and the opaque coating material improves the thermal conductivity to a greater extent, can effectively converge the spot size, and the laser lighting effect is better;

[0029] 3. The composite fluorescent ceramic provided in the present application uses Ce: LuAG coated thermal conductive material, which has better resistance to thermal quenching, and the emission intensity only loses 2.3%-4.1% at 150°C;

[0030] 4. The composite fluorescent ceramic provided in the present application adopts Ce:LuAG to coat the red fluorescent powder, which has a significant effect of supplementing red light and a color rendering index of 81-88. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0032] Figure 1 This is a test temperature-dependent spectrum data diagram of the composite fluorescent ceramic prepared in Example 1;

[0033] Figure 2 This is a graph showing the lighting efficiency versus test power of the composite fluorescent ceramic prepared in Example 1. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] A high-performance composite fluorescent ceramic for laser lighting and a preparation method thereof, specifically comprising the following steps:

[0037] (1) Preparation of Ce:LuAG;

[0038] According to (Ce 0.002 Lu 0.998 )3Al5O 12 The stoichiometric ratio of each element was 41.9711 g of lutetium oxide, 17.95952 g of aluminum oxide, 0.07276 g of cerium oxide, and 0.6 g of MgO and 330 μl of 1.0 wt.% TEOS were added as sintering aids;

[0039] The raw material powders were mixed by ball milling with alumina balls at a speed of 140 r / min for 24 h;

[0040] The mixed powder is dried and sieved at 40°C for 20 hours and the sieve size is 200 meshes.

[0041] The sieved powder is pressed into shape using a steel dry press at a pressure of 15 MPa;

[0042] The pressed green billet is placed in a vacuum sintering furnace and sintered at a vacuum sintering temperature of 1760°C for 20 hours.

[0043] The upper and lower surfaces of the vacuum-sintered ceramics are polished and cut to a size of 1mm*1mm*1mm;

[0044] (2) Preparation of composite fluorescent ceramics (taking Al2O3 as an example);

[0045] Weigh 4g of coating material and put it into the mold, press it into shape, and the pressure is 5MPa; since the size of the coated ceramic designed in this application is relatively small, with a side length of only 0.5-1mm, if the coating is to be completed, only not much powder is needed, 3-5g is more appropriate, less than 3 grams is not easy to shape, and more than 5g is easy to cause waste.

[0046] Take out the ejector pin, place the cut Ce:LuAG ceramic in the center of the green body, and press the ceramic into the coated ceramic green body at a pressure of 10MPa;

[0047] Place in a muffle furnace for sintering at a sintering temperature of 1300°C and a holding time of 12h;

[0048] Double-sided polishing;

[0049] PIG was used to mix commercial red phosphor, where the mass ratio of PIG to red phosphor was 10:1, and the red phosphor used was CaAlSiN3:Eu 2+ , and sintered again.

[0050] The thermal conductivity of the prepared fluorescent ceramic is 29.3Wm -1 K -1 When not coated with red powder, the emission intensity only loses 4.1% at 150°C. After coating with red powder, using 460nm blue light LD excitation, the luminous efficiency is 253lm / w at a power of 5W, and the color rendering index is 85.

[0051] Example 2

[0052] A high-performance composite fluorescent ceramic for laser lighting and a preparation method thereof, specifically comprising the following steps:

[0053] (1) Preparation of Ce:LuAG

[0054] According to (Ce 0.003 Lu 0.997 )3Al5O 12 The stoichiometric ratio of each element was 41.93419 g of lutetium oxide, 17.96173 g of aluminum oxide, 0.10915 g of cerium oxide, and 0.6 g of MgO and 330 μl of 1.0 wt.% TEOS were added as sintering aids;

[0055] The raw material powders were mixed by ball milling with alumina balls at a speed of 145 r / min for 30 h;

[0056] The mixed powder is dried and sieved at 60°C for 18 hours and the sieve size is 200 meshes.

[0057] The sieved powder is pressed into shape using a steel dry press at a pressure of 15 MPa;

[0058] The pressed green billet is placed in a vacuum sintering furnace and sintered at a vacuum sintering temperature of 1780°C for 16 hours.

[0059] The upper and lower surfaces of the vacuum-sintered ceramics are polished and cut to a size of 1mm*1mm*1mm;

[0060] (2) Preparation of composite fluorescent ceramics (taking Al2O3 as an example)

[0061] Weigh 4g of coating material and put it into the mold, and press it into shape at a pressure of 5MPa;

[0062] Take out the ejector pin, place the cut Ce:LuAG ceramic in the center of the green body, and press the ceramic into the coated ceramic green body at a pressure of 10MPa;

[0063] Place in a muffle furnace for sintering at a sintering temperature of 1400°C and a holding time of 10 hours;

[0064] Double-sided polishing;

[0065] PIG was used to mix commercial red phosphor, where the mass ratio of PIG to red phosphor was 5:1, and the red phosphor used was K2SiF6:Mn 4+ , and sintered again.

[0066] The thermal conductivity of the prepared fluorescent ceramic is 30Wm -1 K -1 When not coated with red powder, the emission intensity only loses 2.3% at 150°C. After coating with red powder, using 460nm blue light LD excitation, the luminous efficiency is 260lm / w at a power of 5W, and the color rendering index is 87.

[0067] Example 3

[0068] A high-performance composite fluorescent ceramic for laser lighting and a preparation method thereof, specifically comprising the following steps:

[0069] (1) Preparation of Ce:LuAG

[0070] According to (Ce 0.004 Lu 0.996 )3Al5O 12 In the stoichiometric ratio of each element, 41.89728 g of lutetium oxide, 17.96393 g of aluminum oxide, 0.14555 g of cerium oxide were weighed, and 0.6 g of MgO and 350 μl of 1.0 wt.% TEOS were added as sintering aids;

[0071] The raw material powders were mixed by ball milling with alumina balls at a speed of 150 r / min for 20 h;

[0072] The mixed powder is dried and sieved at 65°C for 24 hours and the sieve size is 200 meshes.

[0073] The sieved powder is pressed into shape using a steel dry press at a pressure of 15 MPa;

[0074] The pressed green blank is placed in a vacuum sintering furnace and sintered at a vacuum sintering temperature of 1800°C for 8 hours.

[0075] The upper and lower surfaces of the vacuum-sintered ceramics are polished and cut to a size of 0.5mm*0.5mm*0.5mm;

[0076] (2) Preparation of composite fluorescent ceramics (taking Al2O3 as an example)

[0077] Weigh 3-5g of coating material and put it into the mold, and press it into shape at a pressure of 5MPa;

[0078] Take out the ejector pin, place the cut Ce:LuAG ceramic in the center of the green body, and press the ceramic into the coated ceramic green body at a pressure of 10MPa;

[0079] Place in a muffle furnace for sintering at a sintering temperature of 1600°C and a holding time of 12h;

[0080] Double-sided polishing;

[0081] PIG was used to mix commercial red phosphor, where the mass ratio of PIG to red phosphor was 3:1, and the red phosphor used was K2GeF6:Mn 4+ , and sintered again.

[0082] The thermal conductivity of the prepared fluorescent ceramic is 32Wm-1 K -1 When not coated with red powder, the emission intensity only loses 2.3% at 150°C. After coating with red powder, using 460nm blue light LD excitation, the luminous efficiency is 258lm / w at a power of 5W, and the color rendering index is 83.

[0083] Comparative Example 1

[0084] Preparation of Ce:LuAG

[0085] According to (Ce 0.004 Lu 0.996 )3Al5O 12 In the stoichiometric ratio of each element, 41.89728 g of lutetium oxide, 17.96393 g of aluminum oxide, 0.14555 g of cerium oxide were weighed, and 0.6 g of MgO and 350 μl of 1.0 wt.% TEOS were added as sintering aids;

[0086] The raw material powders were mixed by ball milling with alumina balls at a speed of 150 r / min for 20 h;

[0087] The mixed powder is dried and sieved at 65°C for 24 hours and the sieve size is 200 meshes.

[0088] The sieved powder is pressed into shape using a steel dry press at a pressure of 15 MPa;

[0089] The pressed green blank is placed in a vacuum sintering furnace and sintered at a vacuum sintering temperature of 1800°C for 8 hours.

[0090] The upper and lower surfaces of the vacuum sintered ceramic are polished.

[0091] The thermal conductivity of the prepared fluorescent ceramic is 9Wm -1 K -1 , the emission intensity loses 5.8% at 150℃. Using 460nm blue light LD excitation, the luminous efficiency is 267lm / w at a power of 5W, and the color rendering index is 49.

[0092] The above description of the disclosed embodiments enables those skilled in the art to implement and use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest range consistent with the principles and novel features disclosed herein.

Claims

1. A high-performance composite fluorescent ceramic for laser lighting, characterized in that: A cubic Ce: LuAG fluorescent ceramic is coated with a high thermal conductivity ceramic powder, the side length of the cubic fluorescent ceramic is 0.5-1 mm, and after sintering to form a block ceramic, a red fluorescent powder is coated and sintered again to obtain the composite fluorescent ceramic; the high thermal conductivity ceramic powder is selected from any one of Al2O3, MgO, AlN, BN, BeO, and SiC; the red fluorescent powder is selected from nitride red powder CaAlSiN3: Eu 2+ or fluoride K2 (Si / Ge / Ti) F6: Mn 4+ One of; The preparation method of the composite fluorescent ceramic comprises the following steps: S1: Preparation of Ce:LuAG; S1-1 ingredients: Lutetium oxide, aluminum oxide, and cerium oxide are weighed according to the stoichiometric ratio of each element in Ce:LuAG, 0.3-1wt.% MgO and TEOS are added as sintering aids, and the mixture is ball-milled; S1-2 tableting: drying and sieving the mixed powder, and using a steel mold to dry and press the sieved powder into a tablet; S1-3 Vacuum sintering: Place the pressed green billet into a vacuum sintering furnace and sinter the green billet; the vacuum sintering temperature is 1760-1800℃, and the holding time is 8-20 h; S1-4 polishing and cutting: polishing and cutting the upper and lower surfaces of the sintered ceramic to obtain cubic Ce: LuAG ceramics; S2: Preparation of composite fluorescent ceramics; S2-1 Preparation of coated green blank: weigh 3-5g of coating material and put it into a mold, dry and press the steel mold to obtain a coated ceramic green blank; S2-2 performs coating: taking out the ejector pin of the die casting mold, placing the cubic Ce: LuAG ceramic cut in step S1 in the center of the coated ceramic blank, and pressing the cubic Ce: LuAG ceramic into the coated ceramic blank; S2-3 sintering: sintering the coated ceramics, double-sided polishing, to obtain block ceramics; sintering method is to place in a muffle furnace or an atmosphere furnace for sintering, the sintering temperature is 1300-1650℃, and the temperature is kept for 8-12 hours; S2-4 coating red powder: using PIG to mix red phosphor, wherein the mass ratio of PIG to red phosphor is 10:1-3:1, and the coating thickness is 70-150 μm; sintering again to obtain a composite fluorescent ceramic.

2. A high-performance composite fluorescent ceramic for laser lighting according to claim 1, characterized in that: The composite fluorescent ceramic has a thermal conductivity of 28-32 Wm -1 K -1 At 150°C, the emission intensity only loses 2.3-4.1%. Using 460 nm blue light LD excitation, the luminous efficiency can reach up to 260 lm / w at a power of 5 W, and the color rendering index is 81-88.

3. The high-performance composite fluorescent ceramic for laser lighting according to claim 1, characterized in that: In step S1-1, the ball milling time is 20-48 h; and the ball milling speed is 140-150 r / min.

4. The high-performance composite fluorescent ceramic for laser lighting according to claim 1, characterized in that: In step S1-2, the drying temperature is 40-65°C, the drying time is 15-24h, the sieve mesh is 100-200 mesh, and the steel mold drying and pressing pressure is 15-25 MPa.

5. The high-performance composite fluorescent ceramic for laser lighting according to claim 1, characterized in that: In step S2-1, the pressure of the steel mold dry pressing is 3-5 MPa.