A cobalt iron oxide composite biochar catalyst (CoFe-LDO-BC) and its preparation method
Through the hydrotalcite-like cobalt iron oxide composite biochar catalyst (CoFe-LDO-BC), the problem of difficulty in degrading dye wastewater in the existing technology has been solved, and an efficient and low-cost catalytic ozone oxidation technology has been achieved to ensure pollution control. Fully mineralized and environmentally friendly.
Patent Information
- Application Number
- CN202310685916.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-06-08
AI Technical Summary
Existing technologies cannot effectively degrade dye wastewater, especially refractory organic pollutants. Moreover, traditional methods have complex equipment, high costs, high investment in catalysts, and the impact of degradation products on the environment has not been thoroughly explored.
Cobalt-iron oxide composite biochar catalyst (CoFe-LDO-BC) derived from hydrotalcite is used to synthesize CoFe-LDH through co-precipitation method, and is combined with biochar under high-temperature reduction conditions to generate a product with high specific surface area and rich oxygen. The vacant CoFe-LDO-BC catalyst uses oxygen vacancies and biochar to accelerate ozone activation and achieve efficient degradation and mineralization of refractory organic pollutants.
A catalytic ozone oxidation technology with low cost and simple process has been realized, which can quickly degrade and completely mineralize pollutants to generate environmentally harmless carbon dioxide and water. It has low catalyst dosage and low metal ion leaching, and is environmentally friendly. Features.
Smart Images

Figure CN116850991B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of advanced oxidation of wastewater, and specifically relates to a preparation method and application of a hydrotalcite-like derived cobalt-iron oxide composite biochar catalyst. Background Art
[0002] With the continuous development of industry, the widespread use of different types of dyes has led to the discharge of a large amount of dye wastewater. Dye wastewater has bright colors and has the characteristics of toxicity, carcinogenicity, and environmental persistence, which cause serious harm to the natural environment and human body. Traditional physical and chemical and biological methods cannot effectively mineralize and degrade dye wastewater. Therefore, the development of new water treatment technology to degrade dye wastewater has become an urgent problem to be solved in the environmental field.
[0003] Advanced oxidation technology (AOPs) is a process that uses external energy such as light, heat, electricity, or catalysts to activate oxidants such as H2O2, PMS, O3, and O2 to produce highly oxidizing active oxygen free radicals (such as OH, O2 ·- 、SO4 ·- ) to degrade organic pollutants. It can quickly and indiscriminately degrade large molecular organic pollutants that are difficult to degrade into harmless or low-toxic small molecular pollutants, and even completely mineralize them into CO2 and H2O. Catalytic ozone oxidation technology is widely favored because of its simple equipment operation, no obvious secondary pollution, and low economic operation cost.
[0004] The surface of metal oxides has a large number of active centers (such as oxygen vacancies, surface acid-base centers, surface hydroxyl groups, etc.) that can activate ozone to produce different active oxygen species. Cobalt-based catalysts CoO, Co3O4 and Co(OH)2 have been widely used in catalytic ozone oxidation to remove refractory organic pollutants. However, the requirements of acidic pH, Co 3+ and Co 2+ Problems such as slow conversion rate limit the application of cobalt compounds in catalyzing ozone. Considering the price and environmental friendliness, transition metal catalysts such as iron and manganese are also used in catalytic ozone. The bimetallic synergistic system can effectively improve the catalytic performance of the catalyst. Layered double hydroxide (LDH) is considered to be a good precursor of cobalt-iron bimetallic oxide. The large specific surface area and "memory effect" of LDH make the derived layered bimetallic oxide have good adsorption and catalytic properties. Under suitable calcination temperature conditions, LDO can not only retain some lamellar structures, but also has more surface defects than general metal oxides. A large number of surface defects provide abundant acidic centers, which promote the decomposition of ozone.
[0005] Oxygen vacancies (Vo) are a typical surface defect that is often used to regulate electronic states and active sites. It can optimize the adsorption capacity of materials and enhance interfacial charge transfer and catalytic ability. Increasing oxygen vacancy defects on the catalyst surface is an effective measure to improve the efficiency of catalytic ozone generation. Generally, high-temperature reduction is an important means to produce oxygen vacancies. Different reducing agents capture lattice oxygen on the surface of metal materials and leave oxygen vacancies in the materials. Based on the synthesis of Co Fe-LDH by coprecipitation, Co Fe-LDO-BC was prepared under high-temperature reduction conditions using biochar as a reducing agent. In addition, biochar itself is an ideal carrier matrix with high dispersibility, high porosity and good electron transfer ability. With the help of composite biochar materials, the leaching and agglomeration of metal ions can be effectively controlled. So far, there is no preparation method and application of hydrotalcite-derived cobalt-iron oxide composite biochar as an ozone catalyst.
[0006] CN202211550881.5 discloses a magnetic suspension heterogeneous catalyst and its preparation method and application. Through the use of biochar and metal source, the metal atoms in the metal source can be evenly dispersed to the surface and pores of the biochar; the coordinated use of biochar and metal source, hollow glass microspheres and thickeners, the powdered material is compounded into a sphere. The hollow glass microspheres and thickeners used in the material preparation process overcome the inconvenience of powder catalysts, but the preparation steps are cumbersome and complicated, and more catalysts are invested in the experimental process, which increases the cost of practical application; its effect in the process of degrading pollutants needs to be improved, and pollutants cannot be completely degraded within 30 minutes. At the same time, its mineralization performance has not been deeply explored, and the impact of degradation products on the environment cannot be judged. Our preparation process is simple, and pollutants can be completely degraded under the condition of adding a small amount of catalyst, and it is further determined that the catalytic process can effectively mineralize pollutants and generate carbon dioxide and water that are harmless to the environment.
[0007] CN202210996377.1 discloses a method for preparing magnetic biochar with catalytic and specific phosphorus adsorption performance, the method comprising the following steps: step 1) dissolving cobalt chloride, ferric chloride and rare earth nitrate into ethylene glycol, stirring and dissolving; step 2) adding polyethylene glycol and anhydrous sodium acetate to the solution of step 1), stirring and dissolving until uniformly dispersed; step 3) adding crab shell biochar to the solution of step 2), stirring and dispersing uniformly; step 4) transferring the solution of step 3) to a polytetrafluoroethylene liner and placing it in a reactor; step 5) placing the reactor in an oven for high temperature reaction; step 6) washing the product after the reaction with anhydrous ethanol and deionized water, drying and grinding to obtain a magnetic biochar material. However, the material is prepared by hydrothermal method, with high energy consumption and cumbersome preparation process; only the degradation at neutral pH is tested, which is not conducive to further promotion and application.
[0008] CN202111532755.2 provides a preparation of a biochar-modified cobalt-iron bimetallic composite catalyst and its application in catalytic degradation of tetracycline, based on an advanced oxidation process of transition metal-activated persulfate (PMS), using agricultural waste bagasse and Co-Fe LDH as precursors, and successfully preparing a magnetic and recyclable porous biochar-modified cobalt-iron bimetallic composite catalyst by coprecipitation and calcination methods. This material is applied to the persulfate system to only degrade and remove pollutants, without further exploring its mineralization effect on pollutants, and without exploring the impact of subsequent degradation products on the environment. We determined the mineralization capacity of the material by measuring the TOC removal rate; in the process of its mechanism research, the material only focused on the role of bimetallic synergy, that is, the role of acidic sites, ignoring the role of oxygen vacancies in the catalytic process. We determined the material through detection means that it has abundant oxygen vacancies, which accelerates the electron transfer on the catalyst surface and directly participates in the activation of oxidants; the material did not explore the specific leaching amount of metal ions in the subsequent oxidation process, which is harmful to the environment. We explored the leaching amount of metal ions in the material, which is environmentally friendly. Summary of the invention
[0009] In view of the lack of technical applications of the above-mentioned materials, one of the purposes of the present invention is to develop a low-cost, simple-process catalytic ozone oxidation catalyst. Based on the synthesis of CoFe-LDH by the co-precipitation method, the catalyst uses biochar as a reducing agent to prepare CoFe-LDO-BC under high-temperature reduction conditions; first, CoFe-LDH is synthesized by the co-precipitation method, and a reduction reaction occurs during the composite calcination of CoFe-LDH and biochar to generate CoFe-LDO-BC. After being composited with biochar, CoFe-LDO-BC has a higher specific surface area, more abundant oxygen vacancies, and more acidic sites. At the same time, with the presence of oxygen vacancies and biochar, the faster electron transfer ability on the surface of CoFe-LDO-BC can quickly activate ozone to produce a variety of active oxygen species (·OH, O2 ·- , 1 O2) oxidizes pollutants in wastewater.
[0010] Based on the above-mentioned prior art, the present invention develops a cobalt iron oxide (CoFe-LDO) composite biochar (BC) catalyst derived from hydrotalcite, which is used to catalyze and activate ozone oxidation of refractory organic matter in wastewater. The catalyst of the present invention has the advantages of high efficiency, simple preparation process, low cost, etc. and has broad application prospects.
[0011] The present invention also provides a method for preparing a catalytic material of a hydrotalcite-like derived cobalt iron oxide (CoFe-LDO) composite biochar (BC), comprising the following steps:
[0012] S1: Select biomass, wash it, and air-dry it; crush the biomass into particles using a crusher, pass the crushed biomass through a 100-mesh sieve, collect the sieved biomass powder, and dry it in an oven;
[0013] S2: Mix cobalt salt and iron salt into a beaker and add ultrapure water, ultrasonicate for 10-20 minutes to make it a uniform metal ion solution, and prepare a mixed alkaline solution of Na2CO3 and NaOH in a certain proportion.
[0014] S3: Dissolve 5 g of dried biomass in a mixed alkaline solution under stirring in a water bath. Continue stirring for 10-20 minutes, then drop the prepared metal ion solution. After the addition is complete, adjust the pH of the mixed solution to alkaline, then continue stirring. After the stirring is complete, age in a water bath to form a precipitate product.
[0015] S4: placing the precipitated product solution in a high-speed centrifuge, collecting the precipitate after centrifugation, washing and drying it, and then placing it in a planetary ball mill, and passing it through a 100-mesh molecular sieve after ball milling.
[0016] S5: The ball-milled solid powder is placed in a quartz boat, placed in a tube furnace, and calcined under an inert atmosphere to obtain a CoFe-LDO-BC catalyst.
[0017] Furthermore, the biomass in step S1 is giant grass straw.
[0018] Furthermore, in step S1, the oven drying temperature is 60-80° C., and the drying time is 12-24 hours.
[0019] Furthermore, in step S2, the cobalt salt is Co(NO3)2·6H2O, the iron salt is Fe(NO3)3·9H2O, Co:Fe=3:1; the amount of ultrapure water used is 50-100mL; and the total concentration of metal ions is 1M.
[0020] Furthermore, the ratio of the mixed alkali in step S2 is [CO3 2- ]=1.6-2.2[Fe 2+ ],[OH - ]=1.5-2[Co 2+ +Fe 3+ ], ultrapure water dosage 50-150mL. [CO3 2- ]、[OH - ]、[Fe 2+ ]、[Co 2+ +Fe 3+ ] represent the concentration of the corresponding ions.
[0021] Furthermore, in step S3, the pH value is 9-11, the temperature of the magnetic stirring water bath is 75-95°C, the stirring time is 2-5h, the aging time is 8-12h, and the aging temperature is 75-95°C.
[0022] Furthermore, the centrifugal speed in step S4 is 5000-8000 rpm.
[0023] Furthermore, in step S4, the washing is performed alternately with ethanol and ultrapure water until neutral; the drying is performed by vacuum drying, the ball milling speed is 500-700 rpm, and the ball milling is performed for 4-6 hours.
[0024] Furthermore, in step S5, the inert gas is nitrogen (N2).
[0025] Furthermore, in step S5, the calcination temperature in the tubular furnace is 300-600° C., the calcination time is 1-2 hours, and the heating rate is 5-15° C. / min.
[0026] The present invention also provides a cobalt iron oxide composite biochar catalyst (CoFe-LDO-BC) obtained by the above method. The specific surface area of the catalyst is 35.8 to 36.0 m 2 / g; More preferably, the specific surface area of the catalyst is 35.89m 2 / g and more abundant oxygen vacancies and more acidic sites (see Fig.10 At the same time, with the presence of oxygen vacancies and biochar, the faster electron transfer ability on the surface of CoFe-LDO-BC can quickly activate ozone to produce a variety of active oxygen species (·OH, O2 ·- , 1 O2) oxidizes pollutants in wastewater.
[0027] The CoFe-LDO-BC catalyst has an amorphous graphite carbon structure with the (220) crystal plane of CoFe2O4 and the (111), (200), (220) and (222) crystal planes and (002) crystal plane of CoO. The infrared spectrum of the catalyst CoFe-LDO-BC is 563 cm -1 、694cm -1 、871cm -1 、979cm -1 There are characteristic peaks. The two peaks of CoFe-LDO-BC at 563cm-1 and 694cm-1 are confirmed to be the Co-O bonds in Co(Ⅱ,Ⅱ) oxide; 871cm-1 and 979cm-1 are the characteristic absorption peaks of iron oxide / hydroxide.
[0028] The pHzpc of CoFe-LDO-BC is 9.1 to 9.2. Preferably, the pHzpc of CoFe-LDO-BC is about 9.17.
[0029] The oxygen vacancy ratio of CoFe-LDO-BC is 0.7-0.75, and Co 2+ and Fe 2+ Preferably, the oxygen vacancy ratio of CoFe-LDO-BC is 0.72, and the Co 2+ and Fe 2+ They are 0.45 and 0.70 respectively.
[0030] The third object of the present invention is to provide a hydrotalcite-derived cobalt iron oxide composite biochar catalyst (CoFe-LDO-BC) for use in activating ozone to oxidize organic pollutants in water.
[0031] Specifically, the CoFe-LDO-BC catalyst is added to organic wastewater, ultrasonicated for 5 to 10 minutes to fully disperse the particles, and ozone is introduced to mechanically stir the system to degrade pollutants through advanced oxidation reactions.
[0032] Furthermore, the pollutants are refractory organic pollutants. Refractory organic pollutants refer to organic matter that cannot be degraded by untamed activated sludge, but can be degraded to a certain extent after a certain period of taming. There are mainly two categories: one is toxic macromolecular organic matter, such as organic chlorides, organophosphorus pesticides, organic heavy metal compounds, polycyclic and other long-chain organic compounds represented by aromatics; the other is inert organic matter that cannot be degraded by microorganisms at all. More preferably, the refractory organic pollutant is methylene blue.
[0033] Further, the catalyst dosage is 0.05-0.20 g / L, more preferably, the catalyst dosage is from 0.05 g / L to 0.10 g / L. The system temperature is 15-35°C. The pH is 3.5-11, preferably, pH=3.5-9; more preferably, pH=7-9.
[0034] Furthermore, the O3 flow rate is 1.75 to 5.25 mg / min; more preferably, the O3 flow rate is 3.5 to 5.25 mg / min.
[0035] Furthermore, the reaction time is 5 to 60 min; more preferably, the reaction time is 30 to 60 min.
[0036] Furthermore, the catalyst prepared by the present invention can effectively limit the leaching of metal ions, see Fig.18 Analysis, no secondary pollution, and environmentally friendly.
[0037] Compared with the prior art, the technical effects of the present invention are as follows:
[0038] (1) The entire preparation process of the present invention is simple, convenient, easy to operate, and can be applied to industrial mass production.
[0039] (2) The catalyst prepared by the present invention uses hydrotalcite as a precursor. The large specific surface area and "memory effect" of LDH (layered double metal hydroxide) make its derived LDO (layered double metal oxide) have good adsorption and catalytic properties. Under suitable calcination temperature conditions, LDO can not only retain some flaky structures, but also have more surface defects than general metal oxides. A large number of acidic centers on the metal surface can effectively activate ozone to produce active oxygen species.
[0040] (3) The catalyst prepared by the present invention uses biochar as a reducing agent and successfully composites LDO with biochar through high-temperature calcination. The effective composite of biochar not only significantly increases the specific surface area of the catalyst and forms more abundant oxygen vacancies and acidic sites, but also effectively inhibits metal agglomeration and accelerates electron transfer between Co(III) / Co(II) and Fe(III) / Fe(II) metal pairs.
[0041] (4) The catalyst prepared by the present invention is applied to heterogeneous ozone oxidation technology, has an excellent removal effect on pollutants in wastewater, and has good stability.
[0042] (5) The catalyst prepared by the present invention can still have good removal ability for pollutants in different pH ranges.
[0043] (6) The catalyst prepared by the present invention is environmentally friendly and has no metal leaching (see Fig.18 ) and other secondary pollution, and the amount of catalyst added is small. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 The scanning electron microscope images of different catalysts in Example 1 of the present invention are shown.
[0045] Figure 2 1 is the X-ray diffraction pattern of different catalysts in Example 1 of the present invention.
[0046] Figure 3 IR spectra of biochar and CoFe-LDO-BC in Example 1 of the present invention.
[0047] Figure 4 Specific surface area and pore distribution of different catalysts in Example 1 of the present invention.
[0048] Figure 5 is the pH of CoFe-LDO-BC in Example 1 of the present invention zpc .
[0049] Figure 6This is an EPR oxygen vacancy data diagram of different catalysts in Example 1 of the present invention.
[0050] Figure 7 Cyclic voltammetry curves of different catalysts in Example 1 of the present invention
[0051] Figure 8 1 is the electrochemical impedance spectrum of different catalysts in Example 1 of the present invention.
[0052] Fig. 9 This is a diagram of the NH3 temperature-programmed desorption of different catalysts in Example 1 of the present invention.
[0053] Fig.10 pyridine infrared images of different catalysts in Example 1 of the present invention.
[0054] Fig.11 This is the XPS spectrum of CoFe-LDO and CoFe-LDO-BC when they are not used in Example 1 of the present invention (a);
[0055] XPS spectrum of CoFe-LDO-BC after use (b), where (1) O1s, O Ⅰ : Lattice oxygen peak; O Ⅱ : oxygen vacancy peak; O Ⅱ : Hydroxyl oxygen peak; (2) Co2p; (3) Fe2p.
[0056] Fig.12 This is a diagram showing the effect of different catalysts activating O3 to degrade methylene blue in water in Example 1 of the present invention.
[0057] Fig.13 This is a diagram showing the effects of different catalysts activating O3 to mineralize methylene blue in water in Example 1 of the present invention, as well as the effect of different catalyst adsorption on the mineralization rate in the upper right illustration.
[0058] Fig.14 The effect diagram (a) of the CoFe-LDO-BC catalyst in Example 1 of the present invention on activating methylene blue in O3 mineralized water at different ozone dosages and its corresponding pseudo-first-order degradation kinetic diagram (b).
[0059] Fig.15 The effect diagram of the CoFe-LDO-BC catalyst in Example 1 of the present invention at different pH values for activating methylene blue in O3 mineralized water (a) and its corresponding pseudo-first-order degradation kinetic diagram (b); the effect diagram of ozone alone at different pH values for activating methylene blue in O3 mineralized water (a1).
[0060] Fig.16The effect diagram (a) of the CoFe-LDO-BC catalyst in Example 1 of the present invention on activating methylene blue in O3 mineralized water at different catalyst dosages and its corresponding pseudo-first-order degradation kinetic diagram (b).
[0061] Fig.17 This is a diagram showing the effect of the CoFe-LDO-BC catalyst in Example 1 of the present invention activating methylene blue in O3 mineralized water after multiple cycles.
[0062] Fig.18 This is a diagram showing the amount of ions leached into the solution after the CoFe-LDO-BC catalyst in Example 1 of the present invention has been recycled. DETAILED DESCRIPTION
[0063] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The described embodiments are only part of the embodiments of the present invention, and the present invention can be embodied through many different forms of embodiments. Based on the embodiments of the present invention, all other embodiments obtained without creative work belong to the protection scope of the present invention.
[0064] In the following examples, the present invention selects methylene blue dye wastewater as a typical refractory organic wastewater for simulation experiments. Methylene blue is not a limitation for refractory organics, and all pollutants within the scope of refractory organics are within the protection scope of the present invention.
[0065] Example 1
[0066] Preparation method of CoFe-LDO-BC catalyst
[0067] S1: Select biomass (giant grass straw), wash and air-dry; crush the biomass into particles using a crusher, pass the crushed biomass through a 100-mesh sieve, collect the sieved biomass powder and dry it in an oven;
[0068] S2: Mix Co(NO3)2·6H2O and Fe(NO3)3·9H2O metal salts and add them to 50mL ultrapure water, Co:Fe=3:1, and ultrasonicate for 15min to make it a uniform metal ion solution with a total metal ion concentration of 1M. At the same time, prepare 100mL of [CO3 2- ]=2[Fe 2+ ],[OH - ]=1.6[Co 2+ +Fe 3+ ] mixed alkaline solution of Na2CO3 and NaOH.
[0069] S3: Dissolve 5 g of dried biomass in a mixed alkaline solution under stirring in an 80°C water bath. After continuous stirring for 15 minutes, add the prepared metal ion solution dropwise. After the addition is complete, adjust the pH of the mixed solution to 10. Then, continue stirring for 3 hours. After the stirring is complete, age the mixed solution in an 80°C water bath for 12 hours to form a precipitated product.
[0070] S4: Place the precipitated product solution in a high-speed centrifuge at a centrifugal speed of 6000rpm. After centrifugation, collect the precipitate, wash it alternately with alcohol and ultrapure water until it is neutral, and place it in a planetary ball mill after drying at a ball milling speed of 600rpm for 4h. After ball milling, pass it through a 100-mesh molecular sieve.
[0071] S5: The ball-milled solid powder was placed in a quartz boat, placed in a tube furnace, and calcined in a nitrogen atmosphere at a temperature of 500° C. for 2 h at a heating rate of 10° C. / min to obtain a CoFe-LDO-BC catalyst.
[0072] BC catalyst preparation method
[0073] The BC catalyst is obtained by the same method as S1 and S5 for preparing the CoFe-LDO-BC catalyst.
[0074] Preparation method of CoFe-LDO catalyst
[0075] The same as the CoFe-LDO-BC catalyst preparation method S2, S3, S4, S5, no biomass is added in step S3, and the CoFe-LDO catalyst is obtained.
[0076] CoFe-LDH catalyst
[0077] The same as the preparation method S2, S3 and S4 of the CoFe-LDO-BC catalyst, no biomass is added in step S3, and the CoFe-LDH catalyst is obtained.
[0078] Figure 1 The scanning electron microscope images of different catalysts in Example 1 of the present invention are shown in Figure 1, where (a) BC, (b) CoFe-LDO, and (c) CoFe-LDO-BC. Figure 1 The microstructure of the CoFe-LDO-BC catalyst can be observed. The red arrows point to the pore structure of biochar, and the yellow circles are metal oxide particles, which confirms that the synthesis of CoFe-LDO-BC is successful and has the dual advantages of biochar and metal oxides.
[0079] Figure 2 is the X-ray diffraction pattern of different catalysts in Example 1 of the present invention. Figure 2It can be concluded that the CoFe-LDO-BC catalyst has an amorphous graphite carbon structure with the (220) crystal plane of CoFe2O4 and the (111), (200), (220) and (222) crystal planes of CoO and the (002) crystal plane, which fully demonstrates that CoFe-LDO and BC are successfully composited.
[0080] Figure 3 The infrared spectra of biochar and CoFe-LDO-BC in Example 1 of the present invention are shown in Figure 1. It can be concluded that both materials have CO stretching vibration peaks, and CoFe-LDO-BC has a stronger intensity. CoFe-LDO-BC has a peak at 563 cm -1 and 694cm -1 The two peaks at 871 cm -1 ,979cm -1 It is the characteristic absorption peak of iron oxide / hydroxide.
[0081] Figure 4 is the specific surface area and pore distribution of different catalysts in Example 1 of the present invention. Figure 4 It can be seen that the pores with the largest adsorption capacity of BC, CoFe-LDO, and CoFe-LDO-BC are distributed at 40nm, 25nm, and 4nm pores. Since the smaller the average pore size of the material adsorbed, the larger the specific surface area of adsorption. Therefore, their specific surface areas are 1.37m 2 / g, 17.91m 2 / g, 35.89m 2 / g. It can be found that the specific surface area of CoFe-LDO-BC is 26 times that of BC and 2 times that of CoFe-LDO.
[0082] Figure 5 is the pH of CoFe-LDO-BC in Example 1 of the present invention zpc .from Figure 5 It can be seen that the pH of CoFe-LDO-BC zpc The pH is about 9.17. zpc It represents the Zeta potential of CoFe-LDO-BC material. Since the pH of the solution plays an important role in catalysis, CoFe-LDO-BC is neutral when the solution pH is 9.17. When the pH is lower than 9.17, the surface of CoFe-LDO-BC presents a positive charge. Since it is more conducive to activating ozone to produce active oxygen free radicals under neutral and positive charge conditions, it can be confirmed that the catalyst has a relatively wide pH application range.
[0083] Figure 6 Figure 1 is the EPR oxygen vacancy data of different catalysts in Example 1 of the present invention. Figure 6It can be seen that after being composited with biochar, CoFe-LDO-BC has more abundant oxygen vacancy defects. Figure 6 The electron paramagnetic signal intensity in the CoFe-LDO-BC was used to confirm the number of oxygen vacancies in the two materials. CoFe-LDO-BC obviously has a sharper electron paramagnetic signal peak and therefore has more abundant oxygen vacancies.
[0084] Figure 7 1 is a cyclic voltammetry curve of different catalysts in Example 1 of the present invention. Figure 7 It can be seen that, under the same voltage condition of -0.55V to 0.5V, the highest current densities of BC, CoFe-LDO and CoFe-LDO-BC are 0.42mA / cm 2 , 0.55mA / cm 2 , 0.94mA / cm 2 Therefore, the redox ability of CoFe-LDO-BC is stronger after biochar composite modification.
[0085] Figure 8 The electrochemical impedance spectra of different catalysts in Example 1 of the present invention are shown in FIG. Figure 8 It can be seen that CoFe-LDO-BC has the smallest Nyquist curve radius, and the smaller the radius, the smaller the resistance. That is, the presence of oxygen vacancies accelerates the electron transfer on the CoFe-LDO-BC surface.
[0086] Fig. 9 The NH3 programmed temperature desorption diagram of different catalysts in Example 1 of the present invention is shown in FIG. Fig. 9 It can be seen that the total acid amount of CoFe-LDO quantified by NH3 is 219 μmol / g, and the total acid amount of CoFe-LDO-BC obtained after biochar composite is 293 μmol / g, and the amount of surface acid increases.
[0087] Fig.10 : is the infrared image of pyridine of different catalysts in Example 1 of the present invention. Fig.10 It can be seen that Lewis acid accounts for 83.7% of the total acid content and Bronsted acid accounts for 16.3%, that is, Lewis acid is the main acid site. Ozone can be regarded as a strong Lewis base that is easily activated by CoFe-LDO-BC to produce more active oxygen free radicals.
[0088] Fig.11 The XPS spectra of CoFe-LDO and CoFe-LDO-BC before use in Example 1 of the present invention (a) and the XPS spectra of CoFe-LDO-BC after use (b), wherein (1) O1s O Ⅰ : Lattice oxygen peak; O Ⅱ : oxygen vacancy peak; O Ⅱ : Hydroxyl oxygen peak; (2) Co2p; (3) Fe2p. Fig.11 It can be seen that the oxygen vacancy ratio of CoFe-LDO-BC obtained by compounding biochar with CoFe-LDO is increased to 0.72, and Co 2+ and Fe 2+ The ratio of oxygen vacancies and metal acid sites on the surface of the material were increased to 0.45 and 0.70 respectively. It can be seen that the material surface has abundant oxygen vacancies and metal acid sites. Subsequently, the material after oxidation was collected and tested, and the results were compared with those before use. It can be found that the oxygen vacancy ratio dropped to 0.51 after the catalyst was used, and Co 2+ and Fe 2 They dropped to 0.38 and 0.54, respectively. Therefore, it can be confirmed that both oxygen vacancies and metal acid sites are involved in activating ozone and mineralizing pollutants.
[0089] Example 2
[0090] The CoFe-LDO-BC catalyst was prepared in the same manner as in Example 1, except that the reaction conditions were different. The reaction conditions are shown in the following table:
[0091] Example 1 Example 2-1 Example 2-2 Example 2-3 Embodiment 2-4 <![CDATA[[CO3 2- ] / [Fe 2+ ]]]> 2 1.6 1.8 2 2.2 <![CDATA[[OH - ] / [Co 2+ +Fe 3+ ]]>> 1.6 1,5 1.7 1.8 2 Stirring time (h) 3 2 5 3 4 pH 10 9 11 10 10 Aging(℃) 80 75 95 85 90 Aging (h) 12 8 10 11 9 Ball mill (rpm) 600 500 700 650 550 Ball milling (h) 4 6 5 4 5 Calcination(℃) 500 300 600 400 500 Calcination (h) 2 1 1.5 2 2 Heating rate (℃ / min) 10 5 15 10 10
[0092] After testing, various parameters of the CoFe-LDO-BC catalyst obtained in Example 2 are substantially the same as those of the CoFe-LDO-BC catalyst obtained in Example 1.
[0093] Example 3
[0094] The effects of different types of catalysts (BC, CoFe-LDO, CoFe-LDO-BC, blank) prepared in Example 1 of the present invention on activating ozone to oxidize methylene blue in water were tested.
[0095] Different types of catalysts were added into methylene blue dye wastewater, ultrasonicated for 5 minutes to fully disperse the particles, then 3.5 mg / min of ozone was introduced, the reaction system was mechanically stirred, and a concentration removal experiment was conducted for 10 minutes. During the advanced oxidation reaction, 5 mL of samples were taken at regular intervals (reaction time 0, 1, 3, 5, 8, 10 minutes) and filtered with a 0.45 μm nylon filter membrane. The absorbance of the filtered clear liquid was measured at a wavelength of 664 nm by an ultraviolet-visible spectrophotometer to determine the concentration removal rate of methylene blue, thereby obtaining the catalytic effect of different materials on methylene blue. The results are shown in FIG. Fig.12 As shown, among which, methylene blue, 20 mg / L; catalyst, 0.10 g / L; O3, 3.5 mg / min; wastewater volume, 100 mL.
[0096] like Fig.12As shown in the figure, at 10 min, the four systems of blank (only O3 added), BC, CoFe-LDO, and CoFe-LDO-BC can completely degrade methylene blue. Since methylene blue is a phenothiazine derivative with high electron delocalization, it is more easily degraded by direct attack of ozone molecules. Therefore, the color removal and degradation of MB is mainly attributed to ozone rather than ozone-derived reactive oxygen radicals. However, the pseudo-first-order degradation kinetic rate of ozone alone is 0.116 min -1 The pseudo-first-order degradation kinetic rate of the CoFe-LDO-BC+O3 system is 0.668min -1 , it can be found that after adding CoFe-LDO-BC, the degradation rate of the system increased by about 5.76 times.
[0097] Example 4
[0098] Different types of catalysts were added to methylene blue dye wastewater, and ultrasound was applied for 5 minutes to fully disperse the particles. Subsequently, 3.5 mg / min of ozone was introduced, and the reaction system was mechanically stirred. A 60-minute concentration removal experiment was conducted. During the advanced oxidation reaction, 5 mL of samples were taken at regular intervals (reaction time 0, 5, 15, 30, 45, 60 min) and filtered with a 0.45 μm nylon filter membrane. The filtered clear liquid was analyzed for TOC concentration by a TOC analyzer to obtain the mineralization effect of different materials on methylene blue. At the same time, the catalyst was added for analysis as in the above steps, but ozone was not introduced. The reaction time (0, 1, 2, 5, 15, 30, 45, 60 min) was changed to take samples and filter for adsorption experiments to determine the effect of different catalyst adsorption on TOC removal. The results of the catalytic and adsorption experiments are shown in the figure. Fig.13 As shown, among which, methylene blue, 20 mg / L; catalyst, 0.10 g / L; O3, 3.5 mg / min; wastewater volume, 100 mL.
[0099] like Fig.13As shown, the illustration shows that the TOC removal rate of methylene blue by different catalysts within 60 minutes is less than 10%, that is, the role of adsorption in TOC removal: this represents that under the condition of not adding O3, only adding three different catalysts, the TOC removal rate after 60 minutes is less than 10%. It can be confirmed that the catalyst itself has little effect on TOC removal. The reason for the increase in TOC removal rate is that the catalyst activates ozone to produce more active oxygen free radicals. It is believed that catalytic ozone oxidation plays a leading role in the mineralization process. Within 60 minutes, the TOC removal rates of the four systems of blank (only O3 added), BC, CoFe-LDO, and CoFe-LDO-BC were significantly different, 30%, 32%, 51.3%, and 57.9%, respectively. CoFe-LDO-BC catalyst has the best mineralization effect. At the same time, it can be found that when the reaction time increases from 30 minutes to 60 minutes, the TOC removal rate only increases by about 2%. Therefore, ventilation for 30 minutes is selected as the subsequent experimental conditions. Fig.10 The figure in the upper right corner shows the TOC removal effect of three catalysts after adsorption for 60 minutes.
[0100] Example 5
[0101] The CoFe-LDO-BC catalyst prepared in Example 1 of the present invention was tested to explore the mineralization effect of methylene blue in water at different ozone ventilation rates.
[0102] CoFe-LDO-BC was added to methylene blue dye wastewater, and ultrasonic treatment was performed for 5 minutes to fully disperse the particles. Subsequently, ozone with different flow rates was introduced, and the reaction system was mechanically stirred. A mineralization experiment was performed for 30 minutes. During the advanced oxidation reaction, 5 mL of samples were taken at regular intervals (reaction time 0, 5, 10, 15, 20, 30 minutes) and filtered with a 0.45 μm nylon filter membrane. The TOC concentration of the filtered clear liquid was analyzed by a TOC analyzer, thereby obtaining the mineralization effect of different ozone dosages on methylene blue. The results are shown in FIG. Fig.14 As shown, methylene blue, 20 mg / L; catalyst, 0.10 g / L; O3 flow, 1.75, 3.5, 5.25 mg / min; wastewater volume, 100 mL.
[0103] like Fig.14 As shown in the figure, when the ozone flow rate increased from 1.75 mg / min to 5.25 mg / min, the TOC removal rate increased from 37% to 56.6%. With the continuous increase of ozone flow rate, the amount of ozone dissolved and the number of derived free radicals increased, and the TOC removal rate increased significantly in the early stage. However, from the perspective of the kinetic constant K, 5.25 mg / min (2.7×10 -2 min -1 ) and 3.5mg / min (2.6×10-2 min -1 ), the TOC removal effect is not significantly improved. The possible reason is that the ozone is saturated and cannot be further dissolved in the pollutant solution. In addition, excessive ozone molecules are not conducive to improving the TOC removal rate. Ozone molecules may form a competitive relationship with pollutants and consume the generated active oxygen free radicals. Therefore, when the amount of ozone reaches saturation, further addition cannot significantly improve the TOC removal rate.
[0104] Example 6
[0105] The CoFe-LDO-BC catalyst prepared in Example 1 of the present invention was tested to explore the mineralization effect of methylene blue in water at different pH values.
[0106] The pH of the methylene blue wastewater was adjusted to 3.5, 5.18, 7, 9, and 11 by dropping 0.1M HCl or 0.1M NaOH. CoFe-LDO-BC was added to the methylene blue dye wastewater, and the particles were fully dispersed by ultrasound for 5 minutes. Then, 3.5 mg / min of ozone was introduced, the reaction system was mechanically stirred, and a mineralization experiment was carried out for 30 minutes. During the advanced oxidation reaction, 5 mL of the sample was taken at regular intervals (reaction time 0, 5, 10, 15, 20, 30 min) and filtered with a 0.45 μm nylon filter membrane. The filtered clear liquid was analyzed by a TOC analyzer for TOC concentration, thereby obtaining the mineralization effect of different pH on methylene blue. At the same time, under the conditions of pH 3.5, 5.18, 7, 9, and 11, only 3.5 mg / min of ozone was introduced, the reaction system was mechanically stirred, and a mineralization experiment was carried out for 30 minutes to explore the effect of different pH on the mineralization of the ozone system alone. The results of the two are as follows Fig.15 As shown, methylene blue, 20 mg / L; catalyst, 0.10 g / L; O3 flow rate, 3.5 mg / min; wastewater volume, 100 mL.
[0107] like Fig.15 As shown in the figure, in the range of pH = 3.5-11, the TOC removal rate of the single ozone system increased from 16.68% to 33.50%. zpc =9.17, the CoFe-LDO-BC+O3 system decreased at pH=11, but its TOC removal rate in the process of pH=3.5-9 increased from 56.26% to 68.25%, and the mineralization effect was significantly better than that of the single ozone system. Even under acidic conditions, the mineralization rate was better than that of single ozone at pH=11. In addition, in actual application, excessive pH adjustment will increase economic costs. The good mineralization effect of the CoFe-LDO-BC+O3 system in neutral and weak alkaline conditions makes it unnecessary to further adjust the high pH, and has good economic applicability.
[0108] Example 7
[0109] The CoFe-LDO-BC catalyst prepared in Example 1 of the present invention was tested to explore the mineralization effect of methylene blue in water at different catalyst dosages.
[0110] Different amounts of CoFe-LDO-BC were added to the methylene blue dye wastewater, and the particles were fully dispersed by ultrasound for 5 minutes. Then 3.5 mg / min of ozone was introduced, and the reaction system was mechanically stirred. The mineralization experiment was carried out for 30 minutes. During the advanced oxidation reaction, 5 mL of samples were taken at intervals (reaction time 0, 5, 10, 15, 20, 30 minutes) and filtered with a 0.45 μm nylon filter membrane. The TOC concentration of the filtered clear liquid was analyzed by a TOC analyzer, thereby obtaining the mineralization effect of different catalyst dosages on methylene blue. The results are shown in Fig.16 As shown. Among them, methylene blue, 20 mg / L; catalyst, respectively 0.05, 0.10, 0.15, 0.20 g / L; O3, 3.5 mg / min; pH = 9; wastewater volume, 100 mL.
[0111] like Fig.16 As shown in the figure, when the catalyst dosage gradually increases from 0.05g / L to 0.20g / L, even the worst catalytic ozone group has a higher TOC removal rate than single ozone. However, with the increase of catalyst dosage, the improvement of catalytic ozone TOC removal rate is not obvious. After 30 minutes of reaction, the final TOC removal rates of 0.15g / L and 0.20g / L are both lower than 0.10g / L. Fig.13 The pseudo-first-order degradation kinetics further verified that when the dosage was 0.15 g / L and 0.20 g / L, Kobs was 2.2×10 -3 min -1 and 1.7×10 -2 min -1 , below 3.7×10 when 0.10g / L -2 min -1 , even lower than 2.7×10 at 0.05g / L -2 min -1 . A large number of active centers (such as vacancy defects) on the catalyst surface can activate ozone to produce different active oxygen species, which has a positive significance for the TOC removal of MB. However, since the function of the excess catalyst is limited by the insufficient ozone dosage, the TOC removal rate is no longer significantly improved. At the same time, the excess Co(II) / Fe(II) in the catalytic system reacts with hydroxyl radicals, resulting in a poor mineralization effect of MB. Therefore, an excess of catalyst will reduce the mineralization efficiency. Based on the above results, it is reasonable to choose a 0.10g / L catalyst.
[0112] Experimental Example 8
[0113] The CoFe-LDO-BC catalyst prepared in Example 1 of the present invention was tested for its effect of activating O3 to oxidize methylene blue in water after multiple cycles and regeneration treatments.
[0114] CoFe-LDO-BC was added to methylene blue dye wastewater, and the agglomerated particles were dispersed in the water by ultrasonic treatment for 5 minutes. Then, 3.5 mg / min of ozone was introduced, and the reaction system was mechanically stirred. A mineralization experiment was conducted for 30 minutes. During the advanced oxidation reaction, 5 mL of samples were taken at regular intervals (reaction time 0, 5, 10, 15, 20, 30 min) and filtered with a 0.45 μm nylon filter membrane. The filtered clear liquid was analyzed for TOC concentration by a TOC analyzer to determine the mineralization rate of methylene blue, thereby obtaining the catalytic effect of CoFe-LDO-BC on methylene blue. The catalyst in the water was collected by an external magnetic field and dried in an oven at 80°C. After drying, the above oxidation experimental steps were repeated for five cycles. The above experimental results are shown in Fig.17 As shown, wherein, methylene blue, 20 mg / L; catalyst, 0.10 g / L; O3, 3.5 mg / min; wastewater volume, 100 mL.
[0115] like Fig.17 As shown in the figure, the mineralization efficiency of methylene blue decreases with the increase of reaction time, which may be due to the blockage and deactivation of oxygen vacancies and acidic sites on the catalyst surface. Even so, CoFe-LDO-BC still maintains good reusability and stability, and the mineralization efficiency only decreases by 7.9% after five cycles.
[0116] Example 9
[0117] The CoFe-LDO-BC catalyst prepared in Example 1 of the present invention was tested for the amount of metal ions leached into the aqueous solution after multiple cycles of O3 activation.
[0118] CoFe-LDO-BC was added to methylene blue dye wastewater, and ultrasonic treatment was performed for 5 minutes to disperse the agglomerated particles in the water. Subsequently, 3.5 mg / min of ozone was introduced, the reaction system was mechanically stirred, and a mineralization experiment was performed for 30 minutes. The catalyst in the water was then collected by an external magnetic field and placed in an 80°C oven for drying. After drying, fresh methylene blue dye wastewater was added to repeat the above oxidation experimental steps, and the cycle was repeated five times in total. 5 mL of the fifth water sample was taken and filtered through a 0.45 μm nylon filter membrane, and the clear liquid obtained by filtration was used to detect the leaching amount of Co and Fe ions using ICP-MS. The above experimental results are as follows: Fig.18As shown, wherein, methylene blue, 20 mg / L; catalyst, 0.10 g / L; O3, 3.5 mg / min; wastewater volume, 100 mL.
[0119] like Fig.18 As shown, after multiple cycles, the leaching amounts of Co and Fe ions in the solution were 0.543 mg / L and 0.527 mg / L, respectively, accounting for about 0.5% of the catalyst dosage. Therefore, it can be determined that CoFe-LDO-BC has good stability and environmental friendliness.
Claims
1. A method for preparing a cobalt-iron oxide composite biochar catalyst CoFe-LDO-BC, characterized in that: The CoFe-LDO-BC has an amorphous graphite carbon structure having a (220) crystal plane of CoFe2O4 and (111), (200), (220) and (222) crystal planes and a (002) crystal plane of CoO; The preparation method comprises the following steps: S1: Select biomass, wash it, and air-dry it; crush the biomass into particles using a crusher, pass the crushed biomass through a 100-mesh sieve, collect the sieved biomass powder, and dry it in an oven; S2: Mix cobalt salt and iron salt in a beaker and add ultrapure water, ultrasonicate for 10-20 minutes to make it a uniform metal ion solution, and prepare a mixed alkaline solution of Na2CO3 and NaOH at the same time; S3: Dissolve 5 g of dried biomass in a mixed alkaline solution under stirring in a water bath, continue stirring for 10-20 min, then drop the prepared metal ion solution, adjust the pH of the mixed solution to alkaline after the addition is complete, then continue stirring, and after the stirring is complete, age in a water bath to form a precipitate product; S4: placing the precipitated product solution in a high-speed centrifuge, collecting the precipitate after centrifugation, washing and drying it, and then placing it in a planetary ball mill, and passing it through a 100-mesh molecular sieve after ball milling; S5: putting the ball-milled solid powder into a quartz boat, placing it in a tube furnace, and calcining it under an inert atmosphere to obtain a CoFe-LDO-BC catalyst; The biomass in step S1 is giant grass straw.
2. The method for preparing the cobalt iron oxide composite biochar catalyst CoFe-LDO-BC according to claim 1, characterized in that: In step S1, the oven drying temperature is 60-80°C and the drying time is 12-24h; In step S2, the cobalt salt is Co(NO3)2·6H2O, the iron salt is Fe(NO3)3·9H2O, Co:Fe=3:1; the amount of ultrapure water is 50-100 mL; the total concentration of metal ions is 1 M; The mixed alkali ratio in step S2 is [CO3 2- ]=1.6-2.2[Fe 2+ ],[OH - ]=1.5-2[Co 2+ +Fe 3+ ], ultrapure water dosage 50-150mL, [CO3 2- ]、[OH - ]、[Fe 2+ ]、[Co 2+ +Fe 3+ ] represent the concentration of the corresponding ions.
3. The method for preparing the cobalt iron oxide composite biochar catalyst CoFe-LDO-BC according to claim 1, characterized in that: In step S3, the pH value is 9-11, the temperature of the magnetic stirring water bath is 75-95°C, the stirring time is 2-5h, the aging time is 8-12h, and the aging temperature is 75-95°C; The centrifugal speed in step S4 is 5000-8000 rpm; In step S4, washing is performed alternately with ethanol and ultrapure water until neutral; drying is performed by vacuum drying, the ball milling speed is 500-700 rpm, and the ball milling is performed for 4-6 hours; In step S5, the inert atmosphere is nitrogen; In step S5, the calcination temperature in the tubular furnace is 300-600° C., the calcination time is 1-2 hours, and the heating rate is 5-15° C. / min.
4. The cobalt iron oxide composite biochar catalyst CoFe-LDO-BC obtained by the method according to any one of claims 1 to 3.
5. The cobalt iron oxide composite biochar catalyst CoFe-LDO-BC according to claim 4, characterized in that: The specific surface area of the catalyst is 35.8-36.0 m 2 / g; The infrared spectrum of the catalyst CoFe-LDO-BC shows that at 563 cm -1 、694cm -1 、871cm -1 、979cm -1 There are characteristic peaks.
6. The cobalt iron oxide composite biochar catalyst CoFe-LDO-BC according to claim 4, characterized in that: The pHzpc of CoFe-LDO-BC is 9.1~9.
2.
7. The cobalt iron oxide composite biochar catalyst CoFe-LDO-BC according to claim 4, characterized in that: The pHzpc of CoFe-LDO-BC is about 9.
17.
8. The cobalt iron oxide composite biochar catalyst CoFe-LDO-BC according to claim 4, characterized in that: For CoFe-LDO-BC, the oxygen vacancy ratio is 0.7~0.
75.
9. The cobalt iron oxide composite biochar catalyst CoFe-LDO-BC according to claim 4, characterized in that: CoFe-LDO-BC, the oxygen vacancy ratio is 0.
72.
10. Use of the cobalt iron oxide composite biochar catalyst CoFe-LDO-BC according to any one of claims 4 to 9, or use of the catalyst prepared by the preparation method according to any one of claims 1 to 3, characterized in that: Application of activated ozone in the oxidation of organic pollutants in water.
11. The use according to claim 10, characterized in that The CoFe-LDO-BC catalyst is added into organic wastewater, ultrasonicated for 5 to 10 minutes to fully disperse the particles, ozone is introduced, the system is mechanically stirred, and pollutants are degraded through advanced oxidation reactions.
12. The use according to claim 11, characterized in that The pollutants are difficult-to-degrade organic pollutants; The catalyst dosage is 0.05-0.20 g / L; The system temperature is 15-35°C; pH 3.5-11; O3 flow rate is 1.75~5.25mg / min; The reaction time is 5~60min.
13. The use according to claim 12, characterized in that The refractory organic pollutant is methylene blue; Catalyst dosage ranges from 0.05 g / L to 0.10 g / L; pH = 3.5-9; O3 flow rate is 3.5~5.25mg / min; The reaction time is 30~60min.
14. The use according to claim 13, characterized in that pH=7-9.