Environmentally friendly carbonaceous binder for blast furnace, preparation method and blast furnace taphole mud

By using environmentally friendly carbonaceous binders for blast furnaces formulated with environmentally friendly asphalt, shale tar and other materials, the problems of high benzopyrene content and short shelf life of resin-based binders in existing blast furnace anhydrous gun mud binders have been solved, achieving better results. The environmental protection performance and usability performance meet the environmental protection and production needs of modern blast furnaces.

CN116854490BActive Publication Date: 2024-10-22TAIYUAN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310882318.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-11-14
Filing Date
2023-07-19
Publication Date
2024-10-22
Estimated Expiration
2043-07-19

AI Technical Summary

Technical Problem

The existing waterless blast furnace mud binders contain high levels of carcinogens such as benzopyrene. The resin-based binder products have short shelf life and poor practicability, and cannot meet the environmental protection and production needs of modern blast furnaces.

Method used

A blast furnace environmentally friendly carbonaceous binder formulated with environmentally friendly asphalt, shale tar, environmentally friendly asphalt powder, plasticizers and carburizers in specific proportions. It is prepared through grinding and shearing mixing processes, and is combined with petroleum coke, hydrogenated terphenyl, and resins. Substances and high aromatic carbon environmentally friendly oils are eutectic and miscible to form a high-performance environmentally friendly carbonaceous binder.

Benefits of technology

It significantly reduces the benzopyrene content, improves the plasticity and thermal stability of the binder, enhances the construction performance of the gun clay, meets environmental standards, extends the shelf life of the product, and improves the on-site operating environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004345215110000061
    Figure BDA0004345215110000061
  • Figure BDA0004345215110000071
    Figure BDA0004345215110000071
Patent Text Reader

Abstract

The present invention discloses a blast furnace environmentally friendly carbonaceous binder, each component is composed of the following mass parts: 2-25 parts of environmentally friendly asphalt, 32-63 parts of shale tar, 3-20 parts of environmentally friendly asphalt powder, 8-25 parts of plasticizer, 5-29 parts of carburizer, wherein the plasticizer is prepared by mixing hydrogenated terphenyl, resinous substances and environmentally friendly oils of high aromatic carbon by a specific process, and the carburizer is selected from petroleum coke and semi-coke, and ground to ≤2000 mesh by a grinding device, and eutectic with environmentally friendly oil and environmentally friendly asphalt by shear stirring at 150 ℃-280 ℃ to prepare. The blast furnace environmentally friendly carbonaceous binder of the present invention can enhance the plasticity of taphole mud, and has strong thermal stability, and the benzopyrene content produced by high temperature is extremely low, which can greatly improve the construction performance and on-site working environment of taphole mud.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of refractory materials for blast furnace ironmaking, and more specifically to an anhydrous taphole mud binder for blast furnaces. The present invention also relates to a preparation method of the anhydrous taphole mud binder for blast furnaces, and a blast furnace taphole mud containing the anhydrous taphole mud binder for blast furnaces. Background Art

[0002] Blast furnace taphole clay plays a very important role in the blast furnace production process, and its quality directly affects the stable operation and normal production of the blast furnace. At present, blast furnace taphole clay at home and abroad is divided into two categories: water taphole clay and waterless taphole clay. The former is only suitable for small blast furnaces, while the latter can meet the production needs of modern large and medium-sized blast furnace ironmaking. With the rapid development of my country's steel industry, large and medium-sized ironmaking blast furnaces are mostly used in steel industry production, and large and medium-sized blast furnaces are developing in the direction of large-scale, long-life, and strengthened smelting. The requirements for the taphole clay used in the blast furnace taphole are getting higher and higher. At the same time, people are paying more and more attention to environmental protection, requiring the taphole clay to be environmentally friendly and conducive to environmental protection. Therefore, the research and development of environmentally friendly high-performance blast furnace waterless taphole clay is a practical need to ensure the healthy development of my country's steel industry.

[0003] At present, the research ideas of environmentally friendly high-performance blast furnace anhydrous taphole mud in China mainly include two ways: developing new anhydrous taphole mud and improving or developing new anhydrous taphole mud binders. For example, the anhydrous taphole mud and preparation method for blast furnace disclosed in Chinese patent CN 110272264 A, the carbon composite anhydrous taphole mud and preparation method for large blast furnace disclosed in Chinese patent CN 110981447 A, and the environmentally friendly anhydrous taphole mud disclosed in Chinese patent CN 112374870 A belong to the first research idea. However, the modern blast furnace was invented in the mid-1850s. After more than two hundred years of operation, it is now quite mature, including the taphole mud material for the blast furnace taphole. Therefore, relatively speaking, the development of a new anhydrous taphole mud binder is lower in cost and more practical.

[0004] At present, the main types of anhydrous cannon mud binders are coal tar, coal tar, resin and a variety of additives. Coal tar and coal tar based binders have high fixed carbon content, good thermal stability and good fluidity and are widely used, but their products contain a large amount of benzopyrene, which is carcinogenic to humans. In the actual production process, they cause great pollution to the working environment, seriously endanger human health and cannot meet the environmental protection development needs under the current new situation; although the resin based blast furnace cannon mud binder can meet the environmental protection requirements in terms of environmental performance, it has poor adaptability to the site in the actual production process, and is prone to the phenomenon of being unable to be beaten and hard cannon, and the application effect is poor.

[0005] At present, the technical improvement of anhydrous taphole mud binder mainly focuses on the following two aspects:

[0006] (1) Modify the existing binder to reduce the benzopyrene content to reduce its harmfulness. For example, Chinese patent CN113149665B provides a cannon mud binder composed of low-temperature distillate oil and high-temperature distillation range asphalt of coal tar under normal pressure conditions, wherein the distillation range temperature of the low-temperature distillate oil is below 400°C, and the high-temperature distillation range asphalt is the residue after coal tar is distilled at a temperature above 500°C. Although this method can improve the performance of anhydrous cannon mud to a certain extent and increase environmental protection to a certain extent, since the modified tar or its substitute is still a macromolecular organic binder, it will inevitably produce carcinogens or pollutants such as benzopyrene or aldehydes, and the pollution and harm to the environment and furnace workers cannot be fundamentally solved.

[0007] (2) Improving the application effect of the binder by preparing a mixed binder. For example, in a binder for blast furnace taphole mud disclosed in Chinese patent CN 106145966 B, the binder includes 40-70 parts of coal tar distillation kettle bottoms, 30-60 parts of phenolic varnish resin, and 2-5 parts of surfactant. Another example is a binder for large blast furnace taphole mud provided by Chinese patent CN102875178B, which uses a compound of silicone resin, furan resin, and melamine formaldehyde resin as a curing component, and uses hydrogenated terphenyl as a synergist. It has high plasticity and a low curing rate. The reduction in the curing rate of the binder is conducive to improving the fluidity of the taphole mud at high temperature and overcoming the problem that the mud cannon is easy to agglomerate. However, the raw materials use silicone resin, furan resin, and melamine formaldehyde resin to compound three resins, which has the problems of short product shelf life and poor practicality. Summary of the invention

[0008] The technical problem to be solved by the present invention is that the coal tar-based anhydrous cannon mud binder made from modified tar or its substitutes in the prior art has a high content of carcinogens such as benzopyrene, and the resin-based anhydrous cannon mud binder has a short product shelf life and poor practicality. An environmentally friendly carbonaceous binder for large blast furnaces is provided, and the cannon mud prepared using the binder of the present invention has better environmental protection performance and usage performance.

[0009] In order to achieve the above object, the technical solution provided by the present invention is:

[0010] A large-scale blast furnace environmentally friendly carbonaceous binder, each component is composed of the following components by weight:

[0011] 2-25 parts of environmentally friendly asphalt, 32-63 parts of shale tar, 3-20 parts of environmentally friendly asphalt powder, 8-25 parts of plasticizer, and 5-29 parts of carbonizer.

[0012] Preferably, the environmentally friendly asphalt is petroleum asphalt, and the asphaltene content of the petroleum asphalt is more than 15%.

[0013] Preferably, the environmentally friendly asphalt powder is petroleum asphalt powder, and the fixed carbon content of the petroleum asphalt powder is more than 50%.

[0014] Preferably, the plasticizer is prepared by mixing 28-81 parts of hydrogenated terphenyl, 3-48 parts of resin substances and 2-55 parts of high aromatic carbon environmentally friendly oil.

[0015] Preferably, the recarburizer is prepared by selecting 3-58 parts of petroleum coke and 5-73 parts of semi-coke, grinding them to ≤2000 mesh through grinding equipment, and then co-melting them with 6-53 parts of environmentally friendly oil and 5-62 parts of environmentally friendly asphalt through shear stirring at 150°C-280°C to prepare the recarburizer.

[0016] Preferably, the components are as follows by mass:

[0017] 9 parts of environmentally friendly asphalt, 55 parts of shale tar, 14 parts of environmentally friendly asphalt powder, 10 parts of plasticizer, and 12 parts of recarburizer.

[0018] The method for preparing the environmentally friendly carbonaceous binder for blast furnaces comprises the following steps:

[0019] (1) Weigh a certain amount of petroleum coke and semi-coke in a certain proportion and put them into a grinding device to grind them to less than 2000 meshes. Put the ground powder into a shear stirring container, melt it at 150-280° C., add a certain amount of environmentally friendly oil and environmentally friendly asphalt, and stir for shear stirring for 20-30 minutes to obtain a recarburizer;

[0020] (2) Weigh a certain amount of hydrogenated terphenyl, resinous material and high aromatic carbon environmentally friendly oil in a certain proportion, put them into a shear stirring container, shear and stir them at 110-130° C. to dissolve them, and stir for 20-30 minutes to obtain a plasticizer;

[0021] (3) Weigh environmentally friendly asphalt and carbon enhancer by weight, add them into a reactor in sequence, mix and stir them at a temperature of 90-120° C. for 20-30 minutes, then raise the temperature in the reactor to 110-130° C. at a heating rate of 1.5-5° C. / min, add a certain weight portion of environmentally friendly asphalt powder, continue to stir and mix for 20-30 minutes, and then add a certain weight portion of plasticizer and shale tar into the reactor in sequence by weight while keeping the temperature in the reactor unchanged, and continue to stir and mix for 20-30 minutes to obtain an environmentally friendly carbonaceous binder for blast furnaces;

[0022] The present invention also relates to a blast furnace taphole mud, characterized in that it contains the blast furnace environmentally friendly carbonaceous binder described in the above technical solution.

[0023] Preferably, the taphole clay for blast furnace comprises the following components in parts by weight: 10-20 parts of brown corundum, 10-25 parts of high-alumina bauxite, 15-25 parts of silicon carbide, 2-7 parts of kyanite, 3-10 parts of ferrosilicon nitride powder, 5-8 parts of sericite, 10-20 parts of ball clay and 15-20 parts of the environmentally friendly carbonaceous binder for blast furnace.

[0024] Preferably, in the taphole clay for blast furnace, the mass proportion of granular materials with a particle size greater than 70 μm in the brown corundum is 10% to 15%.

[0025] Preferably, in the taphole mud for blast furnace, the particle size of high-alumina bauxite is 40 μm to 60 μm.

[0026] Preferably, in the taphole mud for blast furnace, the particle size of ferrosilicon nitride powder is 30 μm-70 μm.

[0027] Preferably, in the taphole clay for blast furnace, the sericite particle size is 70 μm-1 mm.

[0028] Preferably, in the taphole clay for blast furnace, the silicon carbide is composed of 15% to 20% by mass of granular material with a particle size greater than 70 μm and the remainder of powdery material.

[0029] Preferably, in the taphole clay for blast furnace, the particle size of the ball clay is 48 μm-70 μm.

[0030] Compared with the existing known technologies, the technical solution provided by the present invention has the following significant effects:

[0031] (1) The present invention is an environmentally friendly carbonaceous binder for large blast furnaces, wherein petroleum asphalt and shale tar are used as base materials, and a mixed solution prepared by mixing hydrogenated terphenyl, resinous substances and high aromatic carbon environmentally friendly oils through a specific process is used as a plasticizer, and petroleum coke and semi-coke are selected and ground to ≤2000 mesh through grinding equipment, and then sheared and stirred at 150°C-280°C to co-melt with environmentally friendly oils, environmentally friendly asphalt, etc. to prepare a carburizer, so that the cannon mud adhesive has better plasticity and better thermal stability.

[0032] (2) The cannon clay is prepared by adding the binder of the present invention, and the construction performance of the cannon clay is better. The content of benzopyrene is lower than 300 ppm, which is lower and meets the environmental protection standards, and the working environment on site is better. DETAILED DESCRIPTION

[0033] In order to further understand the content of the present invention, the present invention is further described below in conjunction with embodiments.

[0034] Example 1

[0035] The environmentally friendly carbonaceous binder for blast furnaces in this embodiment is composed of the following components by weight: 4 parts of environmentally friendly asphalt, 60 parts of shale tar, 13 parts of environmentally friendly asphalt powder, 9 parts of plasticizer, and 14 parts of recarburizer; the preparation method is as follows:

[0036] (1) Weigh 20 parts of semi-coke and 18 parts of petroleum coke, put them into a grinding device and grind them to less than 2000 meshes, put the ground powder into a shear stirring container, melt it at 200°C, add 30 parts of environmentally friendly oil and 32 parts of environmentally friendly asphalt, and stir for shear stirring. After stirring for 30 minutes, a recarburizer is obtained.

[0037] (2) Weigh 70 parts of hydrogenated terphenyl, 22 parts of resinous substances and 8 parts of environmentally friendly oil with high aromatic carbon content, put them into a shear stirring container, and perform shear stirring at 120° C. to dissolve them. After stirring for 20 minutes, a plasticizer is obtained.

[0038] (3) Environmentally friendly asphalt and recarburizer are weighed in parts by mass, added to a reactor in sequence, and mixed and stirred at a temperature of 100°C for 30 minutes. Then, the temperature in the reactor is raised to 116°C at a heating rate of 2°C / min, and a certain amount of environmentally friendly asphalt powder is added. After stirring and mixing for 20 minutes, a certain amount of plasticizer and shale tar are added to the reactor in sequence in accordance with their mass while maintaining the temperature in the reactor unchanged. The mixture is stirred and mixed for 25 minutes to obtain an environmentally friendly carbonaceous binder for blast furnaces of a certain viscosity.

[0039] (4) Raw materials for taphole mud: 18 parts of brown corundum, 20 parts of high-alumina bauxite, 15 parts of silicon carbide, 5 parts of kyanite, 6 parts of iron silicon nitride powder, 8 parts of sericite, 13 parts of ball clay and 15 parts of binder. A large-scale blast furnace environmentally friendly anhydrous taphole mud is prepared according to the above formula through a specific taphole mud processing process.

[0040] Example 2

[0041] The environmentally friendly carbonaceous binder for blast furnaces in this embodiment is composed of the following components by weight: 6 parts of environmentally friendly asphalt, 58 parts of shale tar, 5 parts of environmentally friendly asphalt powder, 11 parts of plasticizer, and 10 parts of recarburizer; the preparation method is as follows:

[0042] (1) Weigh 23 parts of semi-coke and 9 parts of petroleum coke, put them into a grinding device and grind them to less than 2000 mesh, put the ground powder into a shear stirring container, melt it at 208°C, add 35 parts of environmentally friendly oil and 33 parts of environmentally friendly asphalt, and stir them for shear stirring. After stirring for 28 minutes, a recarburizer is obtained.

[0043] (2) Weigh 68 parts of hydrogenated terphenyl, 8 parts of resinous substances and 24 parts of environmentally friendly oil with high aromatic carbon content, put them into a shear stirring container, and perform shear stirring at 116° C. to dissolve them. After stirring for 25 minutes, a plasticizer is obtained.

[0044] (3) Environmentally friendly asphalt and recarburizer are weighed in parts by mass, added to a reactor in sequence, and mixed and stirred at a temperature of 105°C for 30 minutes. Then, the temperature in the reactor is raised to 118°C at a heating rate of 2.5°C / min, and a certain amount of environmentally friendly asphalt powder is added. After stirring and mixing for 20 minutes, a certain amount of plasticizer and shale tar are added to the reactor in sequence in accordance with their mass while maintaining the temperature in the reactor unchanged. The mixture is stirred and mixed for 25 minutes to obtain an environmentally friendly carbonaceous binder for blast furnaces of a certain viscosity.

[0045] (4) Raw materials for spare taphole mud: 13 parts of brown corundum, 24 parts of high-alumina bauxite, 18 parts of silicon carbide, 6 parts of kyanite, 4 parts of iron silicon nitride powder, 6 parts of sericite, 12 parts of ball clay and 17 parts of binder. A large-scale blast furnace environmentally friendly anhydrous taphole mud is prepared according to the above formula through a specific taphole mud processing process.

[0046] Example 3

[0047] The environmentally friendly carbonaceous binder for blast furnaces in this embodiment is composed of the following components by weight: 9 parts of environmentally friendly asphalt, 55 parts of shale tar, 14 parts of environmentally friendly asphalt powder, 310 parts of plasticizer B, and 312 parts of recarburizer A; the preparation method is as follows:

[0048] (1) Weigh 29 parts of semi-coke and 24 parts of petroleum coke, put them into a grinding device and grind them to less than 2000 meshes, put the ground powder into a shear stirring container, melt it at 203°C, add 26 parts of environmentally friendly oil and 21 parts of environmentally friendly asphalt, and stir them for shear stirring. After stirring for 22 minutes, a recarburizer is obtained.

[0049] (2) Weigh 64 parts of hydrogenated terphenyl, 6 parts of resinous substances and 30 parts of environmentally friendly oil with high aromatic carbon content, put them into a shear stirring container, and perform shear stirring at 122° C. to dissolve them. After stirring for 20 minutes, a plasticizer is obtained.

[0050] (3) Environmentally friendly asphalt and recarburizer are weighed in parts by mass, added to a reactor in sequence, and mixed and stirred at a temperature of 110°C for 30 minutes. Then, the temperature in the reactor is raised to 120°C at a heating rate of 3°C / min, and a certain amount of environmentally friendly asphalt powder is added. After stirring and mixing for 20 minutes, a certain amount of plasticizer and shale tar are added to the reactor in sequence in accordance with their mass while maintaining the temperature in the reactor unchanged. The mixture is stirred and mixed for 25 minutes to obtain an environmentally friendly carbonaceous binder for blast furnaces with a certain viscosity.

[0051] (4) Raw materials for spare taphole mud: 20 parts of brown corundum, 15 parts of high-alumina bauxite, 23 parts of silicon carbide, 3 parts of kyanite, 5 parts of iron silicon nitride powder, 6 parts of sericite, 10 parts of ball clay and 18 parts of binder. A large-scale blast furnace environmentally friendly anhydrous taphole mud is prepared according to the above formula through a specific taphole mud processing process.

[0052] Example 4

[0053] The environmentally friendly carbonaceous binder for blast furnaces in this embodiment is composed of the following components by weight: 12 parts of environmentally friendly asphalt, 49 parts of shale tar, 10 parts of environmentally friendly asphalt powder, 14 parts of plasticizer, and 15 parts of recarburizer; the preparation method is as follows:

[0054] (1) Weigh 30 parts of semi-coke and 20 parts of petroleum coke, put them into a grinding device and grind them to less than 2000 meshes, put the ground powder into a shear stirring container, melt it at 195°C, add 28 parts of environmentally friendly oil and 22 parts of environmentally friendly asphalt, and stir for 30 minutes to obtain a recarburizer.

[0055] (2) Weigh 60 parts of hydrogenated terphenyl, 18 parts of resinous substances and 22 parts of environmentally friendly oil with high aromatic carbon content, put them into a shear stirring container, and perform shear stirring at 118° C. to dissolve them. After stirring for 26 minutes, a plasticizer is obtained.

[0056] (3) Environmentally friendly asphalt and recarburizer A4 were weighed in parts by mass, added to a reactor in sequence, and mixed and stirred at a temperature of 108°C for 30 minutes. Then, the temperature in the reactor was raised to 118°C at a heating rate of 3.5°C / min, and a certain amount of environmentally friendly asphalt powder was added. After stirring and mixing for 20 minutes, a certain amount of plasticizer B4 and shale tar were added to the reactor in sequence in parts by mass while keeping the temperature in the reactor unchanged. The mixture was stirred and mixed for 25 minutes to obtain an environmentally friendly carbonaceous binder for blast furnaces with a certain viscosity.

[0057] (4) Raw materials for spare taphole mud: 10 parts of brown corundum, 13 parts of high-alumina bauxite, 20 parts of silicon carbide, 4 parts of kyanite, 8 parts of iron silicon nitride powder, 7 parts of sericite, 18 parts of ball clay and 20 parts of binder. A large-scale blast furnace environmentally friendly anhydrous taphole mud is prepared according to the above formula through a specific taphole mud processing process.

[0058] Example 5

[0059] The environmentally friendly carbonaceous binder for blast furnaces in this embodiment is composed of the following components by weight: 15 parts of environmentally friendly asphalt, 50 parts of shale tar, 7 parts of environmentally friendly asphalt powder, 12 parts of plasticizer, and 16 parts of recarburizer; the preparation method is as follows:

[0060] (1) Weigh 24 parts of semi-coke and 16 parts of petroleum coke, put them into a grinding device and grind them to less than 2000 meshes, put the ground powder into a shear stirring container, melt it at 210°C, add 30 parts of environmentally friendly oil and 18 parts of environmentally friendly asphalt, etc., and stir for shear stirring. After stirring for 20 minutes, a recarburizer is obtained.

[0061] (2) Weigh 72 parts of hydrogenated terphenyl, 15 parts of resinous substances and 13 parts of environmentally friendly oil with high aromatic carbon content, put them into a shear stirring container, and perform shear stirring at 115° C. to dissolve them. After stirring for 30 minutes, a plasticizer is obtained.

[0062] (3) Environmentally friendly asphalt and recarburizer are weighed in parts by mass, added to a reactor in sequence, and mixed and stirred at a temperature of 108°C for 30 minutes. Then, the temperature in the reactor is raised to 122°C at a heating rate of 4°C / min, and a certain amount of environmentally friendly asphalt powder is added. After stirring and mixing for 20 minutes, a certain amount of plasticizer and shale tar are added to the reactor in sequence in accordance with their mass while maintaining the temperature in the reactor unchanged. The mixture is stirred and mixed for 25 minutes to obtain an environmentally friendly carbonaceous binder for blast furnaces of a certain viscosity.

[0063] (4) Raw materials for spare taphole mud: 15 parts of brown corundum, 17 parts of high-alumina bauxite, 20 parts of silicon carbide, 2 parts of kyanite, 10 parts of iron silicon nitride powder, 5 parts of sericite, 15 parts of ball clay and 16 parts of binder. A large blast furnace environmentally friendly anhydrous taphole mud is prepared according to the above formula through a specific taphole mud processing process.

[0064] The performance indicators of the blast furnace environmentally friendly carbonaceous binders prepared in Examples 1 to 5 are shown in Table 1 below.

[0065] Table 1

[0066]

[0067]

[0068] As can be seen from Table 1, the environmentally friendly binder configured by environmentally friendly asphalt, shale tar, environmentally friendly asphalt powder, plasticizer and recarburizer in the present invention is combined with the aggregate in the present invention to prepare blast furnace taphole mud, which helps to improve the plasticity, flexural strength, compressive strength and resistance to slag iron erosion and scouring of blast furnace taphole mud, and the filling effect is more compact. Compared with the existing coal tar and coal tar binders, the binder in the present invention is more prominent in environmental protection performance, the on-site working environment has been greatly improved, and the health hazards to on-site workers have been greatly reduced. Compared with the existing resin-based binders, the binder in the present invention is more convenient to store, not easy to solidify and has lower cost. Therefore, the recarburizer in the present invention has better uniformity after mixing with other components in the binder; when combined with raw materials such as brown corundum, silicon carbide, and high-alumina bauxite in the aggregate, it has better bonding performance and is easy to form, and has better construction performance. At the same time, compared with the existing coal tar and coal tar binders, the binder in the present invention has a significantly lower benzopyrene content. In the blast furnace environmentally friendly carbonaceous binder product provided in the embodiment, the maximum benzopyrene content is 432 ppm, while in the best embodiment it can be reduced to 269 ppm. Therefore, the furnace working environment can be greatly improved.

Claims

1. A blast furnace environmentally friendly carbonaceous binder, characterized in that: It is composed of the following components by mass: 2-25 parts of petroleum asphalt; 32-63 parts of shale tar; 3-20 parts of petroleum asphalt powder; 8-25 parts of plasticizer; 5-29 parts of carburizer; Wherein, the asphaltene content in the petroleum asphalt is more than 15%; The petroleum asphalt powder has a fixed carbon content of more than 50%; The plasticizer is prepared by mixing 28-81 parts of hydrogenated terphenyl, 3-48 parts of resinous substances and 2-55 parts of environmentally friendly oil with high aromatic carbon content; The recarburizer is a product obtained by selecting 3-58 parts of petroleum coke and 5-73 parts of semi-coke, grinding them to ≤2000 meshes through a grinding device, and then melting them with 6-53 parts of environmentally friendly oil and 5-62 parts of environmentally friendly asphalt by shear stirring at 150°C-280°C; The method for preparing the environmentally friendly carbonaceous binder for blast furnaces comprises the following steps: (1) Weigh a certain amount of petroleum coke and semi-coke in a certain proportion and put them into a grinding device to grind them to less than 2000 meshes. Put the ground powder into a shear stirring container and melt it at 150-280 °C. Then add a certain amount of environmentally friendly oil and environmentally friendly asphalt to shear and stir. After stirring for 20-30 minutes, the recarburizer is obtained; (2) Weigh a certain amount of hydrogenated terphenyl, resinous substances and high aromatic carbon environmentally friendly oil in a certain proportion, put them into a shear stirring container, shear and stir them at 110-130° C. to dissolve them, and stir for 20-30 minutes to obtain a plasticizer; (3) Weigh petroleum asphalt and the recarburizer obtained in step (1) in parts by mass, add them into a reactor in sequence, mix and stir them at a temperature of 90-120° C. for 20-30 minutes, then raise the temperature in the reactor to 110-130° C. at a heating rate of 1.5-5° C. / min, add a certain amount of petroleum asphalt powder in parts by mass, continue to stir and mix for 20-30 minutes, and then, while keeping the temperature in the reactor unchanged, add a certain amount of the plasticizer and shale tar obtained in step (2) in parts by mass into the reactor in sequence, continue to stir and mix for 20-30 minutes, and prepare an environmentally friendly carbonaceous binder for blast furnaces.

2. A method for preparing the blast furnace environmentally friendly carbonaceous binder according to claim 1, comprising the following steps: (1) Weigh a certain amount of petroleum coke and semi-coke in a certain proportion and put them into a grinding device to grind them to less than 2000 meshes. Put the ground powder into a shear stirring container and melt it at 150-280 °C. Then add a certain amount of environmentally friendly oil and environmentally friendly asphalt to shear and stir. After stirring for 20-30 minutes, the recarburizer is obtained; (2) Weigh a certain amount of hydrogenated terphenyl, resinous substances and high aromatic carbon environmentally friendly oil in a certain proportion, put them into a shear stirring container, shear and stir them at 110-130° C. to dissolve them, and stir for 20-30 minutes to obtain a plasticizer; (3) Weigh petroleum asphalt and the recarburizer obtained in step (1) in parts by mass, add them into a reactor in sequence, mix and stir them at a temperature of 90-120° C. for 20-30 minutes, then raise the temperature in the reactor to 110-130° C. at a heating rate of 1.5-5° C. / min, add a certain amount of petroleum asphalt powder in parts by mass, continue to stir and mix for 20-30 minutes, and then, while keeping the temperature in the reactor unchanged, add a certain amount of the plasticizer and shale tar obtained in step (2) in parts by mass into the reactor in sequence, continue to stir and mix for 20-30 minutes, and prepare an environmentally friendly carbonaceous binder for blast furnaces.

3. A blast furnace taphole mud, characterized in that Contains the blast furnace environmentally friendly carbonaceous binder according to claim 1.

4. The blast furnace taphole clay according to claim 3, characterized in that: The taphole clay for blast furnace comprises the following components in parts by weight: 10-20 parts of brown corundum, 10-25 parts of high-alumina bauxite, 15-25 parts of silicon carbide, 2-7 parts of kyanite, 3-10 parts of ferrosilicon nitride powder, 5-8 parts of sericite, 10-20 parts of ball clay and 15-20 parts of blast furnace environmentally friendly carbonaceous binder.

5. The blast furnace taphole clay according to claim 4, characterized in that: The mass proportion of granular materials with a particle size greater than 70 μm in the brown corundum is 10% to 15%.

6. The blast furnace taphole clay according to claim 4, characterized in that: The silicon carbide is composed of granular materials with a particle size greater than 70 μm accounting for 15% to 20% by mass and the remainder is powdery material.