Liquid composition, film, and article having the film
By using the liquid composition prepared by spray coating method on electronic equipment and industrial products, combining the concave and convex and convex of a specific proportion and particle size to form particles, the problem of difficult formation of black coating films with high design in the prior art is solved, and the problem of achieving the goal of achieving high design is achieved. The film with low gloss, low reflectivity and high light-shielding properties has been improved, and the product design and functional performance is improved.
Patent Information
- Application Number
- CN202280015362.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-02-16
- Filing Date
- 2022-02-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-02-09
AI Technical Summary
It is difficult for the prior art to form a black coating film with high designability on electronic equipment and industrial products, especially in the context of improving designability requirements, and the gloss and reflectivity of the existing films are difficult to meet the high designability requirements.
The liquid composition is prepared by spray coating method. The composition contains a specific proportion of resin components, concave-convex forming particles and diluted solvent. The concave-convex forming particles are mainly inorganic particles of 0.05 μm to 0.4 μm and 2 μm to 6 μm. By adjusting The particle ratio and particle size distribution form a film with low gloss, high light shielding and high blackness.
It has achieved the formation of a film with high designability on electronic equipment and industrial products, with low gloss, low reflectivity and high light shading, which is suitable for improving the designability and functionality of electronic equipment and industrial products.
Smart Images

Figure BDA0004397345330000191 
Figure BDA0004397345330000091
Abstract
Description
Technical Field
[0001] The present invention relates to a liquid composition, a film, and an article having the film. Specifically, the present invention relates to a liquid composition for forming a film, a film formed by the composition, and an article having the film on a coated object. Background Art
[0002] In electronic devices such as smartphones, tablet computers, and computers, a black coating is applied to part or all of the frame (either the outside or the inside) or to the non-viewing part (e.g., the edge of the frame) of a cover glass disposed and fixed on the viewing side of a touch panel in order to improve design, shield internal wiring, and block light. In recent years, such a demand has also been applied to part (e.g., the outer edge of the lens) or all of electronic device components such as lenses installed in various camera units.
[0003] For example, the technology disclosed in Patent Document 1 is to form a film by directly screen printing a film made of an insulating material on a housing of a portable electronic device such as a smartphone, or to form a film by forming a thin film in a mold after screen printing.
[0004] Prior art literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2007-285093 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] However, with the demand for improving the design of industrial products in recent years, there is a demand for applying a black coating film (for example, a concave-convex film) with higher design to such products.
[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a liquid composition that can form a film with high design properties, and the film can be preferably applied to various industrial products such as electronic devices or electronic device components.
[0009] Solutions to the problem
[0010] As a result of intensive research, the present inventors have found that a film with high design properties can be effectively formed by satisfying the following requirements.
[0011] As a film forming method (coating method), a spray coating method is used.
[0012] The liquid composition used for film formation has a specific composition (containing unevenness-forming particles at a specified ratio, and the unevenness-forming particles contain inorganic particles having a specified particle size range at a specified mass ratio range).
[0013] The present inventors have completed the invention provided below based on this new finding and have solved the above-mentioned problems.
[0014] In the following, (A) is a resin component, (B) is a concave-convex particle, (B1) is an inorganic small particle having a particle size (d1) of 0.05 μm to 0.4 μm, (B2) is an inorganic large particle having a particle size (d2) of 2 μm to 6 μm, and (C) is a diluent solvent.
[0015] According to the present invention, there is provided a composition which is a liquid composition for forming a film by spraying, wherein:
[0016] At least (A), (B) and (C),
[0017] The composition contains 20% by mass or more and 60% by mass or less of (B) in 100% by mass of the total solid content of the composition,
[0018] (B) contains 90 mass % or more of (B1) and (B2), and the mass ratio of (B2) to (B1):1 is 1.8 to 3.3.
[0019] The above liquid composition may include the following aspects:
[0020] (B2) preferably contains silicon dioxide.
[0021] The silica preferably includes composite silica that has been blackened by a colorant.
[0022] (B1) preferably contains carbon black.
[0023] The viscosity at 25°C is preferably from 1 mPa·s to 30 mPa·s.
[0024] According to the present invention, there is provided a film formed by spraying the above-mentioned liquid composition. In addition, according to the present invention, there is provided an article having the above-mentioned film.
[0025] The above items may include the following:
[0026] The outermost surface of the film-forming surface preferably has a glossiness of less than 2% for incident light at an incident angle of 60° (hereinafter also referred to as “glossiness”), a reflectivity of less than 4% for light with a wavelength of 550 nm (hereinafter also referred to as “reflectivity”), and an L value of less than 22 in the CIELAB colorimetric system measured by the SCE method.
[0027] When the film is required to have light-shielding properties while being transparent, the optical density of the outermost surface of the film-forming surface is preferably 1.5 or more.
[0028] ·Preferably, the maximum height Rz (hereinafter also referred to as “Rz”) of the outermost surface of the film-forming surface in JIS B0601:2001 is 7 μm or more, the length average Rsm (hereinafter also referred to as “Rsm”) of the profile curve elements is 80 μm or more, the skewness Rsk (hereinafter also referred to as “Rsk”) of the profile curve is 0.3 or less, and the kurtosis Rku (hereinafter also referred to as “Rku”) of the profile curve is 3 or more.
[0029] Effects of the Invention
[0030] According to the present invention, a liquid composition capable of forming a highly designed film can be provided, and the film can be preferably applied to various industrial products such as electronic devices or electronic device components. DETAILED DESCRIPTION
[0031] The following describes the best embodiment of the present invention. However, the present invention is not limited to the following embodiments. Without departing from the spirit of the present invention, any appropriate changes or improvements made to the following embodiments by those skilled in the art based on their general knowledge obviously also fall within the scope of the present invention.
[0032] In the numerical ranges described in this specification, the upper limit or lower limit of some numerical ranges may be replaced by the numerical values shown in the examples.
[0033] In the present specification, the content rate or content of each component in the composition means the total content rate or content of the plurality of substances present in the composition, unless otherwise specified, when the composition contains a plurality of substances corresponding to the components.
[0034] <Liquid Composition>
[0035] The liquid composition (hereinafter, also referred to as "composition") according to one embodiment of the present invention is used to form a film on the surface of a coated object, and comprises (A) a resin component, (B) concave-convex forming particles, and (C) a diluting solvent. (B) used to form the composition comprises: (B1) small particles having a particle size (d1) of 0.05 μm to 0.4 μm, and (B2) large particles having a particle size (d2) of 2 μm to 6 μm, and may also comprise components other than (B1) and (B2). That is, the composition according to one embodiment of the present invention comprises (A), (B1), (B2), and (C). When applying the composition according to one embodiment on the surface of the coated object, spraying can be appropriately used.
[0036] Hereinafter, the composition according to one embodiment of the present invention will be described in detail.
[0037] -(A)-
[0038] (A) used to form the composition becomes the adhesive of (B). The material of (A) is not particularly limited, and any one of a thermoplastic resin and a thermosetting resin can be used. As a thermosetting resin, for example, acrylic resin, ethyl formate resin, phenolic resin, melamine resin, urea resin, diallyl phthalate resin, unsaturated polyester resin, epoxy resin, alkyd resin, etc. can be cited. As a thermoplastic resin, for example, polyacrylate resin, polyvinyl chloride resin, butyral resin, styrene-butadiene copolymer resin, etc. can be cited. From the viewpoint of heat resistance, moisture resistance, solvent resistance, and surface hardness of the formed concave-convex film, a thermosetting resin is preferably used as (A). As a thermosetting resin, when considering the softness and toughness of the formed film, an acrylic resin is particularly preferred. (A) can be used alone or in combination of two or more.
[0039] The content (total amount) of (A) is not particularly limited, but considering the ratio with other ingredients, the total amount relative to the total solid amount of the composition (100 mass %) is preferably 5 mass % or more, 15 mass % or more is preferably, 25 mass % or more is more preferably, 50 mass % or less is preferably, 45 mass % or less is preferably, and 40 mass % or less is more preferably.
[0040] -(B)-
[0041] (B) used to form the composition must be composed of a plurality of concave-convex particles of different sizes. As (B), the main feature is the combination of (B1) small particles and (B2) large particles. For example, when only two concave-convex particles of different sizes (i.e., (B1) and (B2)) are used to form (B), the particle size (d2) of (B2) is preferably 10 times or more, preferably 15 times or more, preferably 40 times or less, and preferably 35 times or less than the particle size (d1) of (B1). As (B), when three or more concave-convex particles of different sizes are used, the relationship between the particle size (dmax) of the concave-convex particles representing the maximum particle size and the particle size (dmin) of the concave-convex particles representing the minimum particle size can be adjusted to the above relationship, that is, (dmax) is preferably 10 times or more, preferably 15 times or more, preferably 40 times or less, and preferably 35 times or less than (dmin).
[0042] In one embodiment, (d1) is preferably 0.05 μm or more, more preferably 0.1 μm or more, preferably 0.4 μm or less, and more preferably 0.3 μm or less. (d2) is preferably 2 μm or more, more preferably 3 μm or more, preferably 6 μm or less, preferably 5 μm or less, and even more preferably 4 μm or less.
[0043] The particle diameter (d1) of (B1) and the particle diameter (d2) of (B2) are measured by a laser diffraction / scattering particle size distribution measuring device, and the volume basis thereof is the median diameter.
[0044] In one embodiment, the mass ratio of (B2) in (B) is relative to (B1):1, preferably 1.5, preferably 1.8 or more, preferably 3.5 or less, and preferably 3.3 or less. Within this mass ratio range, by combining (B1) and (B2) having the above-mentioned specific particle size range, it is easy to embed one (B1) between two adjacent (B2) in the formed film. As a result, the inventors have found that in addition to achieving low gloss and low reflectivity on the film surface, the blackness can also be improved (L value becomes lower).
[0045] The total content (total amount) of (B1) and (B2) in (B) is preferably 90% by mass or more, more preferably 95% by mass or more. The upper limit is not particularly limited, but is 100% by mass. That is, in one embodiment, (B1) and (B2) preferably contain 90% by mass or more in 100% by mass of (B).
[0046] The content (total amount) of (B) is preferably 20% by mass or more, more preferably 25% by mass or more, more preferably 30% by mass or more, preferably 60% by mass or less, more preferably 50% by mass or less, more preferably 45% by mass or less, and particularly preferably 40% by mass or less, relative to the total amount of the total solids of the composition (100% by mass). When the total amount of (B) is less than 20% by mass, problems such as increased gloss and insufficient optical density will occur. When it exceeds 60% by mass, the amount of (A) in the formed coating film will be relatively small, and as a result, the coating film will fall off from the coated object.
[0047] As (B2), any of resin particles and inorganic particles may be used. Examples of the resin particles include melamine resin, benzoguanidine (Benzoguanamine) resin, phenylguanidine / melamine / formalin condensate, acrylic resin, ethyl formate resin, styrene resin, fluororesin, silicone resin, etc. On the other hand, inorganic particles include, for example, silicon dioxide, aluminum oxide, calcium carbonate, barium sulfate, titanium oxide, carbon, etc. These may be used alone or in combination of two or more.
[0048] In order to obtain more superior properties, (B2) preferably uses inorganic particles. As (B2), by using inorganic particles, it is easy to form a highly light-shielding film with lower gloss. As the inorganic particles used in (B2), silicon dioxide is preferred. Although the shape of (B2) is not particularly limited, in order to achieve further low gloss, low reflection, and low L value on the surface of the formed film, it is preferred to use particles (sharp-edge products) with a narrower particle size distribution (CV (Coefficient of Variation) value is, for example, less than 15). The CV value is a value that quantifies the degree of diffusion (unevenness of particle size) of the particle size distribution relative to the average value of the particle size (arithmetic mean particle size). By using such particles, the contact opportunity between (B2) and (B1) in the formed film will be increased, and it will be easy to achieve further low gloss, low reflection, and low L value on the surface of the film.
[0049] In order to further reduce the glossiness of the film-forming surface, it is preferred to use amorphous particles as (B2). Among these, porous amorphous silica particles are particularly preferred as (B2). By using such particles as (B2), the glossiness of the film surface can be further reduced due to repeated refraction of light on the surface and inside of (B2) during film formation.
[0050] In one embodiment, in order to suppress light reflection on the film-forming surface, (B2) may be colored black with an organic or inorganic colorant. Examples of such materials include composite silica, conductive silica, and black silica.
[0051] Examples of composite silica include nano-scale composites of carbon black (hereinafter also referred to as "CB") and silica. Examples of conductive silica include conductive particles such as CB coated on silica particles. Examples of black silica include natural ore containing stone mill in silica rock.
[0052] On the other hand, like (B2), the material of (B1) is not particularly limited, and either resin particles or inorganic particles can be used. Examples of the resin particles include melamine resin, benzoguanidine, Resin, benzoguanidine / melamine / formalin condensate, acrylic resin, ethyl formate resin, styrene resin, fluororesin, silicone resin, etc. On the other hand, inorganic particles include silicon dioxide, aluminum oxide, calcium carbonate, barium sulfate, titanium oxide, CB, etc. These may be used alone or in combination of two or more.
[0053] As (B1), for example, CB added as a coloring agent or a conductive agent can be used. By using CB as (B1), the formed film is colored, so that the antireflection effect can be enhanced and a good antistatic effect can be obtained.
[0054] -(C)-
[0055] The (C) used to form the composition is blended for the purpose of dissolving (A) and adjusting the viscosity of the composition as a whole. By using (C), it will be easier to mix (A) and even other components added as needed, thereby improving the uniformity of the composition. In addition, since the viscosity of the composition can be appropriately adjusted, when a film is formed on the surface of the coated object, the operability of the composition and the uniformity of the coating thickness can be improved, which will greatly help to improve the design of the final article.
[0056] As (C), there is no particular limitation as long as it is a solvent that can dissolve (A), and examples thereof include organic solvents and water. As organic solvents, for example, butanone, toluene, propylene glycol monomethyl ether acetate, ethyl acetate, butyl acetate, methanol, ethanol, isopropanol, butanol, etc. (C) can be used alone or in combination of two or more.
[0057] In order to obtain the above-mentioned effect obtained by blending (C), the content (total amount) of (C) in the composition is preferably 1 mass part or more, more preferably 3 mass parts or more, and preferably 20 mass parts or less, relative to 100 mass parts of (A).
[0058] -(D) Optional ingredients-
[0059] In addition to the above-mentioned components ((A), (B), (C)), the composition may also contain (D) to the extent that the effects of the present invention are not impaired. Examples of (D) include leveling agents, thickeners, pH adjusters, lubricants, dispersants, defoamers, hardeners, reaction catalysts, and the like.
[0060] In particular, when a thermosetting resin is used as (A), the crosslinking of (A) can be promoted by adding a curing agent. Examples of the curing agent include urea compounds, melamine compounds, isocyanate compounds, epoxy compounds, aziridine compounds, Azoline compounds, etc. As the curing agent, isocyanate compounds are preferred among these. The curing agent may be used alone or in combination of two or more.
[0061] The ratio of the curing agent to be added to the composition is preferably 10 to 50 parts by mass relative to 100 parts by mass of (A). By adding the curing agent within this range, the hardness of the formed film can be increased, and as a result, even if the film is placed in an environment where it slides with other members, the properties of the film surface can be maintained for a long time, and low gloss, high light shielding, low reflection and high blackness can be easily maintained.
[0062] When a hardener is added to the composition, a reaction catalyst may be used in combination to promote the reaction between (A) and the hardener. Examples of the reaction catalyst include ammonia and ammonium chloride. The ratio of the reaction catalyst added to the composition is preferably 0.1 mass part or more and 10 mass parts or less relative to 100 mass parts of the hardener.
[0063] Based on the reason of maintaining the smoothness of the composition on the surface of the coated object and applying (spraying) by spraying, the composition involved in one embodiment has a viscosity of 1 mPa·s or more at 25°C, preferably 30 mPa·s or less, and preferably 20 mPa·s or less. When the viscosity of the composition is too low, it is likely that a film with a thickness sufficient to express the improvement of the design will not be formed. When the viscosity of the composition is too high, it is likely that the composition cannot be sprayed uniformly on the surface of the coated object, and as a result, it is likely that a film with a uniform thickness that improves the design will not be formed.
[0064] The above viscosity varies depending on the components contained in the composition, that is, the type or molecular weight of (A) and (B) used. Furthermore, when (D) is blended in addition to (A) and (B), the viscosity also varies depending on the type or molecular weight of (D). However, it can be easily adjusted by adjusting the content of (C) in the composition within the above range.
[0065] The composition according to one embodiment of the present invention can be prepared by adding (A) and (B) to (C), and optionally adding (D), and mixing and stirring. The order of mixing the components is not particularly limited as long as the components can be uniformly mixed.
[0066] The composition according to one embodiment of the present invention may be a one-component type or a two-component type. When a hardener is added to the composition as (D), the composition according to one embodiment may be a two-component type, for example, comprising: a first liquid containing components other than the hardener, and a second liquid containing the hardener.
[0067] <Coating method, film, and article>
[0068] The composition according to one embodiment of the present invention can be used to form a film, and an article having the film can be manufactured.
[0069] The film forming method is not particularly limited, and can be any method such as spray coating (e.g., air spray, airless spray, electrostatic spray, etc.), brush coating, curtain flow coating, roller brush coating, rod coating, kiss-roll, metering roller, gravure roller, reverse roller, dip coating, die-cast coating, etc., or can be used by an apparatus to form a film on any object to be coated.
[0070] In particular, the composition according to one embodiment is preferably used to form a film by spraying, where droplets must be sprayed from a relatively small nozzle hole. That is, the composition according to one embodiment is preferably used to form a film by spraying, and the formed film is a sprayed film.
[0071] When the composition according to one embodiment is sprayed, the droplets formed by the composition gradually adhere to the surface of the object to be coated, and at the same time, (C) in the droplets already attached to the object to be coated will also volatilize. As a result, the solid amount (particles) that have been removed from the droplets (C) gradually accumulate on the surface of the object to be coated to form a solid particle stack. According to one embodiment, this solid particle stack constitutes a film.
[0072] When a thermosetting resin is used as (A) and a composition mixed with a curing agent is used as (D), it is preferred that the solid particle layered product is attached to the surface of the coated object and then heated to cure the layered product. In this case, even if a small amount of (C) remains in the layered product before heating, (C) can be completely volatilized by the heating.
[0073] The heating conditions may be appropriately adjusted depending on the thickness of the laminate before heating or the heat resistance of the coated object, etc. An example of the heating conditions is 70°C to 150°C for 1 minute to 10 minutes, preferably 100°C to 130°C for 2 minutes to 5 minutes.
[0074] The coating object (coated object) of the composition involved in one embodiment of the present invention is not particularly limited, as long as it is an object with a hard surface, such as a hard surface made of glass, resin, metal, ceramic, wood, etc. The shape of the coated object is also not particularly limited, and examples thereof include a plate-like, (hollow) cylindrical, and thin-film-like.
[0075] Examples of the coating object include:
[0076] ·Electrical and electronic equipment such as mobile phones, smartphones, tablet computers, computers, computer peripherals (keyboards, printers, external hard disks, etc.), watches, audio equipment, various OA equipment, etc.
[0077] ·Household appliances such as refrigerators, vacuum cleaners, microwave ovens, televisions, and video equipment.
[0078] Stairs, floors, tables, chairs, cabinets, other furniture, woodworking products.
[0079] Various building materials, wooden floors, interior decoration of buildings , exterior walls, etc.
[0080] Vehicles such as automobiles and motorcycles, or their components: specifically, vehicle bodies, interior components (dashboards, instrument panels, steering wheels, etc.), bumpers, spoilers, door handles, headlights, taillights, aluminum wheels, motorcycle fuel tanks, etc.
[0081] Optical applications, such as optical components such as lenses installed in various camera units.
[0082] · Glasses, goggles, and similar products.
[0083] In this specification, the article refers to an object in which a film formed of the composition according to one embodiment of the present invention is formed directly on an object to be coated, or formed on a previously formed positioning layer.
[0084] As the positioning layer, for example, urea resin layer, melamine resin layer, ethyl formate resin layer, polyester resin, etc. can be listed. For example, the ethyl formate resin layer can be obtained by applying a solution containing polyisocyanate and active hydrogen compounds such as diamine and diol on the surface of the object to be coated, and then hardening it. In addition, in the case of urea resin and melamine resin, a solution containing water-soluble urea resin or water-soluble melamine resin can be applied on the surface of the object to be coated, and then hardened. Polyester resin is obtained by applying a solution dissolved or diluted with an organic solvent (such as butanone, toluene, etc.) on the surface of the object to be coated, and then drying it.
[0085] Alternatively, a film of the composition according to one embodiment may be formed on an object other than the object to be coated (such as a plastic film), and then the entire object may be attached to the object to be coated, thereby providing a film of the composition according to one embodiment on the surface of the object.
[0086] The thickness of the film formed by the composition involved in one embodiment is not particularly limited and can be appropriately adjusted according to the use of the article, etc. The average film thickness of the film includes the height of the portion protruding from the surface of the coated object more than (B2) and (B1) of the film. The average film thickness of the film can be measured according to the method of JIS K7130.
[0087] <Film Characteristics>
[0088] The properties of a film formed from the composition according to one embodiment are as follows.
[0089] (Glossiness, reflectivity, L value, optical density, adhesion)
[0090] The film formed from the composition involved in one embodiment preferably has a glossiness of less than 2%, a reflectance of 4% or less, and an L value of 22 or less on the film surface. When the film formed from the composition involved in one embodiment is required to have light-shielding properties during transmission, in addition to the above-mentioned characteristics (glossiness of less than 2%, reflectance of 4% or less, and L value of 22 or less on the film surface), it is also preferred that the optical density of the film surface is 1.5 or more.
[0091] Here, if the film formed by the composition involved in one embodiment is configured to be exposed on the outermost surface, the glossiness, reflectivity, L value and optical density of the film surface are preferably within the above ranges as described in the text. When other films are coated on the film formed by the composition involved in one embodiment, the glossiness, reflectivity, L value and optical density of the surface of the other film (i.e., the outermost surface of the article) are preferably within the above ranges. Hereinafter, these surfaces are collectively referred to as "film outermost surfaces".
[0092] The film formed from the composition involved in one embodiment preferably has a glossiness of less than 2%, a reflectivity of 4% or less, and an L value of 22 or less on the outermost surface of the film. When the film formed from the composition involved in one embodiment is required to have light-shielding properties during transmission, in addition to the above-mentioned characteristics (glossiness of the outermost surface of the film is less than 2%, reflectivity is less than 4%, and L value is less than 22), it is also preferred that the optical density of the outermost surface of the film is 1.5 or more. By setting the glossiness, reflectivity, L value and optical density of the outermost surface of the film within the above ranges, low glossiness, low reflectivity, high blackness and high light-shielding properties of the outermost surface of the film can be achieved.
[0093] The upper limit of glossiness is preferably less than 1.5%, and more preferably less than 1%. By adjusting the glossiness within the above range, flare and ghosting caused by diffuse reflection of light can be effectively prevented. The lower limit of glossiness is not particularly limited, and the lower the better.
[0094] The upper limit of the reflectivity is preferably below 3%, and below 2.5% is more preferred. The lower limit of the reflectivity is not particularly limited, and the lower the better. By adjusting the reflectivity within the above range, flare and ghosting caused by diffuse reflection of light can be more effectively prevented.
[0095] The upper limit of the L value (blackness) is preferably 20 or less, and more preferably 18 or less. The lower limit of the L value is not particularly limited, but from the perspective of requiring a darker appearance, the lower the better. By adjusting the L value within the above range, the blackness is improved, the blackness is more obvious, and the design is excellent, so it can be applied to camera units of mobile phones such as smartphones.
[0096] The above L value is the lightness L* value in the CIE 1976 L*a*b* (CIELAB) color system measured by the SCE method on the outermost surface of the film. The so-called SCE method is a method of removing regular reflected light, which means a method of measuring color by removing regular reflected light. The definition of the SCE method is stipulated in JIS Z 8722 (2009). Since the SCE method removes regular reflected light for measurement, the color is close to the color actually seen by the human eye.
[0097] CIE is the abbreviation of Commission internationale de l'éclairage, which means International Commission on Illumination. CIELAB color space is an equal color space specified in JIS Z8781 (2013) and recommended in 1976 to measure color differences caused by differences in perception and equipment. The three coordinates of CIELAB are represented by L* value, a* value, and b* value. L* value represents lightness and is represented by 0 to 100. When the L* value is 0, it means black, and when the L* value is 100, it means diffuse white. The a* value represents the color between red and green. If the a* value is negative, it means that the color is close to green, and if it is positive, it means that the color is close to red. The b* value represents the color between yellow and blue. If the b* value is negative, it means that the color is close to blue, and if it is positive, it means that the color is close to yellow.
[0098] When the film formed by the composition is required to have light-shielding properties during transmission, the lower limit of the optical density is preferably 2 or more, and more preferably 2.5 or more. By adjusting the optical density within the above range, the light-shielding properties can be further improved. The upper limit of the optical density is not particularly limited, and the higher the better.
[0099] The glossiness, reflectance, L value and optical density mentioned above can be measured by a post-processing method.
[0100] The film formed by the composition preferably has good adhesion to the surface of the coated object in addition to the above-mentioned properties (gloss, reflectivity, L value, and optical density as required). The adhesion of the film formed by the composition to the surface of the coated object is preferably such that the coating film residue is 75% or more as shown in the adhesion evaluation in the examples described below.
[0101] (Rz, Rsm, Rsk, Rku, Ra)
[0102] The film formed from the composition according to one embodiment preferably has a maximum height Rz of 7 μm or more on the outermost surface of the film, a length average Rsm of the profile curve elements of 80 μm or more, a skewness Rsk of the profile curve of 0.3 or less, and a peak Rku of the profile curve of 3 or more. By setting Rz, Rsm, Rsk, and Rku of the outermost surface of the film to the above ranges, and by setting the glossiness, optical density, reflectivity, and L value of the outermost surface of the film to the above ranges (glossiness less than 2%, reflectivity 4% or less, L value 22 or less, and optical density 1.5 or more as required), low glossiness, low reflectivity, high blackness, and high light shielding properties as required on the outermost surface of the film can be achieved.
[0103] The lower limit of Rz is preferably 10 μm or more. By setting the lower limit of Rz to the above value, low glossiness, low reflectivity, and high light shielding properties can be more easily adjusted.
[0104] The upper limit of Rz is not particularly limited, but is preferably 50 μm or less, more preferably 30 μm or less. By setting the upper limit of Rz to the above value, low gloss, high light shielding properties, low reflectivity, and high blackness of the outermost surface of the film can be more easily achieved.
[0105] Rsm is the average length of the contour curve element in the reference length. The lower limit of Rsm is preferably 100 μm or more, and more preferably 120 μm or more. By setting the lower limit of Rsm to the above value, the advantage of low gloss can be obtained more easily. Although the upper limit of Rsm is not particularly limited, it is preferably 160 μm or less. Within the above range, a more superior adhesion can be obtained between the coated object and the film formed thereon.
[0106] Rsk is an index that represents the cube of the height Z(x) in the dimensionless reference length averaged by the cube of the root mean square height (Zq), and represents the deviation of the average line of the concave and convex shape of the outermost surface of the film, that is, an index representing the degree of deformation. If the value of Rsk is positive (Rsk>0), the concave and convex shape tends to be concave and sharpened. If it is negative (Rsk<0=, the concave and convex shape tends to be convex and blunted. When the protrusion of the contour curve is blunt, its haze is lower than when it is sharp.
[0107] The upper limit of Rsk is preferably below 0.2. By setting the upper limit of Rsk to the above value, the advantage of low gloss can be obtained more easily. Although the lower limit of Rsk is not particularly limited, it is preferably above 0. By setting the lower limit of Rsk to the above value, the advantage of low gloss can be easily obtained.
[0108] Rku is an index that represents the fourth power average of the height Z(x) in the dimensionless reference length through the fourth power of the root mean square height (Zq), and represents the sharpness of the front end of the concave and convex portion of the film. As Rku increases, the front end of more concave and convex portions will become sharper, so the inclination angle near the front end of the concave and convex portion will increase, but the inclination angle of other parts will decrease, resulting in a tendency to easily produce background reflections. In addition, as Rku decreases, the front end of more concave and convex portions will become flat, so the inclination angle of the front end of the concave and convex portion will decrease, resulting in a tendency to easily produce background reflections.
[0109] The lower limit of Rku is preferably 3.3 or more. By setting the lower limit of Rku to the above value, the advantage of low gloss can be more easily obtained. The upper limit of Rku is not particularly limited, but is preferably 5 or less. By setting the upper limit of Rku to the above value, the advantage of low gloss can be more easily obtained.
[0110] The film formed from the composition according to one embodiment has an arithmetic mean roughness (Ra) of the outermost surface of the film of preferably 0.5 μm or more, more preferably 1.0 μm or more, and even more preferably 1.5 μm or more.
[0111] In addition, Rz, Rsm, Rsk, Rku and Ra of the outermost surface of the film as described above can be measured and calculated in accordance with JIS B0601:2001.
[0112] [Example]
[0113] Hereinafter, although the present invention is specifically described based on experimental examples (including embodiments and comparative examples), the present invention is not limited to these experimental examples. In the following description, "part" means "part by mass" and "%" means "% by mass".
[0114] [Composition components]
[0115] As A (resin component), the following items were prepared.
[0116] A1: Thermosetting acrylic resin
[0117] (ACRYDIC A801, manufactured by DIC Corporation, solid content 50%)
[0118] As B1 (small particles) belonging to B (concavoconvex-shaped particles), the following items were prepared.
[0119] B1a: Carbon black (CB) (particle size 150nm)
[0120] (MH black #273, manufactured by Mikoku Color Co., Ltd., CB content 9.5%)
[0121] B1b: Transparent silica (particle size 58nm)
[0122] (ACEMATT R972, manufactured by EVONIK)
[0123] As B2 (large particles) belonging to B, the following items are prepared.
[0124] B2a: Composite silica (particle size 3 μm)
[0125] (BECSIA ID, manufactured by FUJI SILYSIA Chemical Co., Ltd.)
[0126] B2b: Black acrylic beads (particle size 3μm)
[0127] (RUBCOULEUR 224SMD black, manufactured by Dainichi Seika Industries, Ltd.)
[0128] B2c: Transparent silica (particle size 4.1 μm)
[0129] (SYLYSIA 430, manufactured by FUJI SILYSIA CHEMICAL CO., LTD.)
[0130] B2d: Transparent silica (particle size 8 μm)
[0131] (SYLYSIA 450, manufactured by FUJI SILYSIA CHEMICAL CO., LTD.)
[0132] B2e: Transparent acrylic beads (particle size 3μm)
[0133] (Uni powder-NMB-0320C, manufactured by JX Nippon Oil & Energy Corporation)
[0134] In addition, the BECSIAID used in B2a (composite silica) is a composite particle of CB and silica with CB / silica = about 25 / 75 (mass ratio). The MHI black #273 used in B1a (CB) is a CB dispersion, of which 9.5% is CB and the remaining 8.5% is other compounds out of a total solid content of 18%. Of the 8.5% other compounds, 3% are copper compounds and 5.5% are acrylic resins.
[0135] As D (optional ingredient), the following items were prepared.
[0136] ·D1: Isocyanate compound
[0137] (TAKENATE D110N, manufactured by Mitsui Chemicals, Inc., solid content 75%)
[0138] [Object to be painted]
[0139] As an object to be coated, a smartphone frame (plastic casing) was prepared.
[0140] [Experimental Examples 1 to 16]
[0141] 1. Preparation of the composition
[0142] In order to make the solid content ratio as shown in Table 1, so that the total solid content is about 25% by mass, the components of each experimental example are placed in a required amount of a mixed solvent (methyl ethyl ketone: butyl acetate = 50:50) as (C) a diluent solvent, and stirred and mixed to prepare a liquid composition (hereinafter also referred to as "liquid").
[0143] 2. Production of items (evaluation samples)
[0144] The liquid obtained in each experimental example was sprayed using the coating method described below (3-3). After spraying toward the outer surface of the object to be coated, it was dried by heating at 120°C for 3 minutes. The resulting article was a coating film (hereinafter referred to as "coating film") having an average film thickness of 20 μm formed on the surface of the object to be coated by heating the solid particle accumulation layer obtained by spraying.
[0145] 3. Evaluation
[0146] The liquid obtained in each experimental example was evaluated for various properties (viscosity, injectability, coating property, liquid sliding property) by the following method (liquid evaluation). In addition, the coating film formed on the article obtained in each experimental example was evaluated for various properties (properties, surface properties) by the following method (article evaluation). The results are shown in Table 1.
[0147] [Liquid agent evaluation]
[0148] (3-1) Viscosity
[0149] The viscosity of each liquid was measured using an E-type viscometer (VISCOMETER TV-35, manufactured by Toki Sangyo Co., Ltd.) at 25° C., 1 rpm, after 1 minute, with a standard cone rotor and rotor number: 01. The evaluation criteria were as follows.
[0150] ○: Viscosity is 1 mPa·s or more and 30 mPa·s or less (good viscosity)
[0151] ×: Viscosity is more than 30 mPa·s (viscosity is too high)
[0152] (3-2) Injectability
[0153] The injectability of the liquid agent is evaluated by observing the injection of the gas spray.
[0154] The injectability was evaluated by visually observing the state of each liquid agent entering the nozzle from the cup of the air brush using an air sprayer in which an air brush (SPRAY-WORK HG single air brush, manufactured by TAMIYA) was attached to an air can (SPRAY-WORK AIR CAN 420D, manufactured by TAMIYA). The evaluation criteria were as follows.
[0155] ○: No clogging at all, the liquid enters the nozzle smoothly
[0156] △: Although there is no clogging, the speed at which the liquid enters the nozzle is a little slow
[0157] ×: Liquid is clogged and cannot enter the nozzle
[0158] (3-3) Coating properties
[0159] The coating properties of the liquid agent were evaluated by observing the coating unevenness after spray coating.
[0160] Each liquid agent was injected into an air spray using the above (3-2), and sprayed toward the outer surface of the object to be coated from the tip of the air brush to a distance of 10 cm for 10 seconds, and then the formed solid particle layer was visually evaluated for coating unevenness. The evaluation criteria were as follows.
[0161] ○: Uneven coating (uneven thickness) was not observed.
[0162] △: Local uneven coating was observed
[0163] ×: Uneven coating was observed in most areas
[0164] (3-4) Liquid Sliding Properties
[0165] The liquid slippage of a liquid agent is evaluated by observing the liquid sliding off the coated object after being sprayed.
[0166] As in the coating property described in (3-3), each liquid agent was injected into the air spray using the method described in (3-2), and sprayed toward the outer surface of the object to be coated from the tip of the air brush at a distance of 10 cm for 10 seconds, and then the liquid sliding property of the attached droplets from the object to be coated was evaluated. The evaluation criteria were as follows.
[0167] ○: When the coated object is placed vertically, it is confirmed that the liquid does not slide off at all.
[0168] △: When the coated object is placed vertically, the liquid gradually slides off.
[0169] ×: When the coated object is placed vertically, the liquid immediately slides off.
[0170] [Item Evaluation]
[0171] (3-5) Characteristics
[0172] -Glossiness-
[0173] The glossiness of the coating film formed on the surface of each article at a relative incident angle of 60° (60° specular glossiness) was measured at 9 points using a gloss meter (VG 7000, manufactured by Nippon Denshoku Industries Co., Ltd.) according to the method of JIS Z8741, and the average value was defined as the glossiness. The evaluation criteria were as follows.
[0174] ◎: Glossiness is less than 1.5% (extremely good low gloss)
[0175] ○: Glossiness 1.5% or more, less than 2% (good low glossiness)
[0176] ×: Glossiness 2% or more (low glossiness is insufficient)
[0177] -Reflectivity-
[0178] The reflectance of light with a wavelength of 550 nm (550 nm reflectance) formed on the coating surface of each article was measured at 9 points using a spectrophotometer (CM-5, manufactured by Konica Minolta, Inc.) according to JIS Z8722, and the average value was defined as the reflectance. The evaluation criteria were as follows.
[0179] ◎: Reflectivity 3% or less (extremely good low reflectivity)
[0180] ○: Reflectivity is more than 3% and less than 4% (good low reflectivity)
[0181] ×: Reflectivity exceeds 4% (low reflectivity is insufficient)
[0182] -Blackness-
[0183] The blackness of the coating surface formed on each article was evaluated by measuring the lightness L* value of the coating surface in the CIE 1976 L*a*b* (CIELAB) color system using the SCE method. The lightness L* value was measured using a spectrophotometer (CM-5, manufactured by KONICAMINOLTA) in accordance with the method of JIS Z8781-4:2013. The evaluation criteria are as follows.
[0184] In the measurement, CIE standard illuminant D65 was used as the light source, the viewing angle was 10°, and the L* value was calculated using the CIELAB color expression method using the SCE method. CIE standard illuminant D65 is specified in JIS Z 8720 (2000) "Standard light (illuminate) and standard light source for color measurement", and the same is also specified in ISO 10526 (2007). CIE standard illuminant D65 is used to express the color of objects illuminated by daylight. Regarding the viewing angle of 10°, it is specified in JIS Z 8723 (2009) "Visual comparison method of surface color", and the same is also specified in ISO / DIS 3668.
[0185] ◎: L value 20 or less (extremely high blackness)
[0186] ○: L value is more than 20 and less than 22 (high blackness)
[0187] ×: L value exceeds 22 (blackness is insufficient)
[0188] -Light blocking properties-
[0189] The light-shielding property of the coating formed on each object is evaluated by calculating the optical density of the coating. The optical density of the coating formed on each object is calculated by using an optical densitometer (X-rite 361T (Ortho filter), manufactured by Japan Flatbed Machinery Co., Ltd.) to irradiate the coating side of the object with a vertically transmitted light beam, and the ratio to the non-coating state is expressed as log (logarithm). The optical density of 6.0 or above is the upper limit of the detection limit of the measurement. The evaluation criteria are as follows. In addition, in this evaluation, it is assumed that the coated object itself has transmittance and the light-shielding property of the coating formed thereon is required. When the coating is not required to have light-shielding properties, this evaluation will not affect the comprehensive evaluation.
[0190] ◎: Optical density 2 or more (extremely good light shielding properties)
[0191] ○: Optical density 1.5 or more, less than 2 (good light shielding properties)
[0192] ×: Optical density is less than 1.5 (light shielding property is insufficient)
[0193] The adhesion of the coating film formed on each article to the surface of the coated object was evaluated by scoring the coating film with a commercially available utility knife into a checkered pattern, sticking a transparent tape (Cellotape, manufactured by NICHIBAN) on it, and then removing it to visually confirm the remaining state of the coating film. The evaluation criteria were as follows.
[0194] ◎: 100% coating residue (extremely high adhesion)
[0195] ○: The coating film remains 75% or more and less than 100% (high adhesion)
[0196] ×: The coating film remains less than 75% (insufficient adhesion)
[0197] - Comprehensive Assessment -
[0198] The glossiness, reflectivity, blackness, and adhesion were comprehensively evaluated. The evaluation criteria were as follows. In addition, as described above, the light-shielding property was excluded from the comprehensive evaluation because its necessity depends on the situation.
[0199] ◎: Glossiness, reflectivity, blackness, and adhesion are all ◎
[0200] ○: At least one of the evaluation of glossiness, the evaluation of reflectivity, the evaluation of blackness, and the evaluation of adhesion is ○, and none of them is ×
[0201] ×: At least one of the evaluation of glossiness, the evaluation of reflectivity, the evaluation of blackness, and the evaluation of adhesion was ×
[0202] (3-6) Surface properties
[0203] -Rz value, Rsm value, Rsk value, Rku value, Ra value-
[0204] The properties (Rz value, Rsm value, Rsk value, Rku value, Ra value) of the coating film surface formed on each article were measured using a surface roughness measuring machine (SURFCOM480B, manufactured by Tokyo Seimitsu Co., Ltd.) in accordance with the method of JIS B0601: 2001. The evaluation criteria are as follows.
[0205] (Rz)
[0206] ◎: Rz is 10 μm or more (extremely good)
[0207] ○: Rz is 7 μm or more and less than 10 μm (good)
[0208] ×: Rz is less than 7 μm (defective)
[0209] (Rsm)
[0210] ◎: Rsm is 120 μm or more (extremely good)
[0211] ○: Rsm is 80 μm or more and less than 120 μm (good)
[0212] ×: Rsm is less than 80 μm (defective)
[0213] (Rsk)
[0214] ◎: Rsk is 0.2 or less (extremely good)
[0215] ○: Rsk is more than 0.2 and less than 0.3 (good)
[0216] ×: Rsk is more than 0.3 (defective)
[0217] (Rku)
[0218] ◎: Rku is 3.3 or more (extremely good)
[0219] ○: Rku is 3 or more and less than 3.3 (good)
[0220] ×: Rku is less than 3 (bad)
[0221] (Ra)
[0222] ◎: Ra is 1.5 μm or more (extremely good)
[0223] ○: Ra is 0.5 μm or more and less than 1.5 μm (good)
[0224] ×: Ra is less than 0.5 μm (poor)
[0225] [Table 1]
[0226]
[0227] 4. Investigation
[0228] As shown in Table 1, when the liquid does not contain one or more of (B1) and (B2) as (B) (Experimental Examples 6, 7, 9, 11, and 12), glossiness, reflectivity, L value, and adhesion of one or more film characteristics cannot be satisfied. On the other hand, even if both (B1) and (B2) are contained in the liquid as (B) (Experimental Examples 1 to 5, 8, and 10), if the mass ratio of (B2) relative to (B1):1 is less than 1.8 (Experimental Example 1) or exceeds 3.3 (Experimental Example 5), L value and adhesion of one or more film characteristics cannot be satisfied. Even if both (B1) and (B2) are included, and the mass ratio of (B2) to (B1):1 is in an appropriate range (above 1.8 and below 3.3) (Experimental Examples 2 to 4, 13 to 17), when the (B) content (total amount) in the total solid content of 100 mass% is less than 20 mass% (Experimental Example 13) or exceeds 60 mass% (Experimental Example 17), it will not be possible to meet the viscosity of more than one liquid and the glossiness, reflectivity, L value, and adhesion of the film properties.
[0229] In contrast, when the mass ratio of (B2) relative to (B1):1 is greater than 1.8 and less than 3.3, and the total amount of (B) contained in the composition with respect to 100 mass% of the total solid amount is greater than 20 mass% and less than 60 mass% (Experimental Examples 2 to 4, 8, 10, 14 to 16), all membrane properties and membrane characteristics can be met.
Claims
1. A composition, which is a liquid composition for forming a film by spraying, wherein: At least (A), (B) and (C), The composition contains 20% by mass or more and 60% by mass or less of (B) in 100% by mass of the total solid content of the composition, (B) contains 90% by mass or more of (B1) and (B2), and the mass ratio of (B2) to (B1):1 is 1.8 to 3.3; (A) is a resin component, (B) is a concavoconvex forming particle, (B1) is an inorganic small particle having a particle size (d1) of 0.05 μm or more and 0.4 μm or less, (B2) is an inorganic large particle having a particle size (d2) of 3 μm or more and 6 μm or less, (C) is a dilution solvent, The particle size (d2) of (B2) is 20 to 40 times the particle size (d1) of (B1), and (B2) contains composite silica that is blackened by a colorant.
2. The composition according to claim 1, wherein (B1) contains carbon black.
3. The composition according to claim 1 or 2, wherein The viscosity at 25°C is 1 mPa·s or more and 30 mPa·s or less. 4 . A film formed by spraying the composition according to claim 1 . An article comprising the film according to claim 4.
6. The article of claim 5, wherein: The outermost surface of the film-formed surface has a glossiness of less than 2% for incident light at an incident angle of 60°, a reflectivity of less than 4% for light of a wavelength of 550 nm, and an L value of less than 22 in the CIELAB colorimetric system measured using the SCE method.
7. The article of claim 6, wherein: When the film is required to have light-shielding properties during transmission, the optical density of the outermost surface on which the film is formed is 1.5 or more.
8. The article according to any one of claims 5 to 7, wherein The maximum height Rz of the outermost surface of the film-formed surface in JIS B0601:2001 is 7 μm or more, the length average Rsm of the profile curve elements is 80 μm or more, the skewness Rsk of the profile curve is 0.3 or less, and the kurtosis Rku of the profile curve is 3 or more.