Through the combination of softwood pulp, hardwood pulp and modified chitosan fiber, combined with the cross-linking reaction of nano-titanium dioxide, the deficiencies of medical dialysis paper in terms of strength, air permeability and antibacterial properties are solved, and high-quality medical dialysis is achieved. Paper products that meet the high standards of the medical industry.
Patent Information
- Application Number
- CN202311003981.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-10
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-08-10
AI Technical Summary
Existing medical dialysis paper has deficiencies in strength, air permeability, heat sealability and antibacterial properties. It has poor bacteriostatic effect and high cost, making it difficult to meet the medical industry's demand for high-quality products.
Using a mixture of softwood pulp and hardwood pulp, modified chitosan fiber is added, and is coated with a sizing agent to improve the strength and antibacterial performance of the paper. It is formed by the cross-linking reaction of nanometer titanium dioxide and chitosan fiber. Fiber structure with antimicrobial effect.
Medical dialysis paper that achieves high strength, good air permeability and significant antibacterial properties improves the heat resistance and service life of the paper while reducing production costs.
Smart Images

Figure BDA0004387355000000101 
Figure BDA0004387355000000111 
Figure BDA0004387355000000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of medical dialysis paper, in particular to a heat-sealed self-adhesive high-strength medical dialysis paper and a processing method thereof. Background Art
[0002] Medical dialysis paper is mostly used in medical sterilization. One side is made of plastic film materials such as high-density polyethylene and polypropylene, and the other side is dialysis paper. It is made of heat-sealed synthetic glue and is used to package medical devices for sterilization. It can effectively block the invasion of various microorganisms and avoid the possibility of bacterial infection during or after the sterilization of medical devices. With the rapid development of the medical industry and people's increasing attention to health, the requirements for medical dialysis paper are getting higher and higher. There are higher requirements for the strength, air permeability, heat sealing, antibacterial properties and other properties of dialysis paper.
[0003] Chinese patent application CN103498383A provides a medical dialysis paper, which is made of coniferous wood and hardwood as fiber raw materials according to traditional papermaking technology. Since the hardwood used in the present invention has high permeability and the coniferous wood has high strength, the medical dialysis paper produced by the present invention has good air permeability and high strength, but the medical dialysis paper has poor antibacterial effect and general strength. Chinese patent CN112501942B discloses a medical dialysis paper and a production method thereof, which includes pulping, mixing coniferous wood pulp, chitosan fiber and bamboo fiber to obtain mixed pulp; papermaking the mixed pulp to form medical dialysis paper, while ensuring the strength of the paper, the paper also has good antibacterial properties, significantly improving the quality of domestic medical dialysis paper, reducing the occurrence of medical accidents caused by poor quality of medical dialysis paper, and reducing the production cost of medical dialysis paper, but its antibacterial effect is general. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a heat-sealed self-adhesive high-strength medical dialysis paper and a processing method thereof, and provides a medical dialysis paper with high strength, good antibacterial performance and good air permeability.
[0005] In order to achieve the above object, the present invention discloses a method for processing heat-sealed self-adhesive high-strength medical dialysis paper, comprising the following steps:
[0006] Step 1, mixing and beating softwood pulp and hardwood pulp, and then adding modified chitosan fiber to mix to obtain a mixed slurry;
[0007] Step 2, adding a wet strength agent and a reinforcing agent to the mixed slurry, mixing evenly, and then forming into a sheet to obtain a semi-finished medical dialysis paper;
[0008] Step 3: Apply the sizing agent to the semi-finished medical dialysis paper and dry it to obtain heat-sealable self-adhesive high-strength medical dialysis paper.
[0009] Preferably, in step 1, the raw materials are calculated by weight, including 35-55 parts of coniferous wood pulp, 24-36 parts of hardwood pulp and 20-45 parts of modified chitosan fiber.
[0010] Preferably, in step 1, the beating time is 40-50 min, and the beating degree is 34-40° SR.
[0011] Preferably, the modified chitosan fiber in step 1 is prepared by the following steps:
[0012] S1. Evenly mix kaolin, sodium hydroxide and deionized water, then add nano titanium dioxide and polyethylene glycol, stir and mix to react, filter after the reaction, wash with deionized water, and dry in a vacuum drying oven at 60° C. for 18 h to obtain a titanium dioxide / kaolin composite material;
[0013] S2, mixing the titanium dioxide / kaolin composite material and toluene uniformly, adding deionized water and 3-aminopropyltrimethoxysilane, stirring and mixing, reacting, centrifuging after the reaction, washing with ethanol, and drying at 80° C. for 12 h to obtain an amino-modified titanium dioxide / kaolin composite material;
[0014] S3, immersing chitosan fiber in glyoxal aqueous solution, adding amino-modified titanium dioxide / kaolin composite material, stirring and mixing evenly to react, washing with deionized water after the reaction, and drying in a drying oven at 50° C. for 12 hours to obtain modified chitosan.
[0015] Furthermore, the mass ratio of kaolin, sodium hydroxide, deionized water, nano-titanium dioxide and polyethylene glycol in S1 is 100:350-550:10-18:5-15:38-55.
[0016] Furthermore, the polyethylene glycol in S1 is polyethylene glycol-1000.
[0017] Furthermore, the reaction temperature in S1 is 50-60° C., and the reaction time is 1-2 h.
[0018] Furthermore, the mass ratio of the titanium dioxide / kaolin composite material, toluene, deionized water and 3-aminopropyltrimethoxysilane in S2 is 100:2400-2800:30-45:255-315.
[0019] Furthermore, the reaction temperature in S2 is 85-95° C., and the reaction time is 24-30 hours.
[0020] Furthermore, in the S3, the mass ratio of the chitosan fiber, the glyoxal aqueous solution and the amino-modified titanium dioxide / kaolin composite material is 100:2500-3200:8-15.
[0021] Furthermore, the glyoxal aqueous solution in S3 is a glyoxal aqueous solution with a mass concentration of 4%.
[0022] Furthermore, the reaction temperature in S3 is 40-45° C., and the reaction time is 2-3 h.
[0023] Preferably, the raw materials in step 2 are calculated by weight, including 100 parts of mixed slurry, 0.2-1 parts of wet strength agent and 2-3 parts of reinforcing agent.
[0024] Preferably, the wet strength agent in step 2 comprises one of cationic polyacrylamide and polyamide polyepichlorohydrin resin.
[0025] Preferably, the reinforcing agent in step 2 comprises cationic starch.
[0026] Preferably, the papermaking in step 2 is carried out on a Fourdrinier papermaking machine.
[0027] Preferably, in step three, the sizing agent consists of neutral glue AKD, nanocellulose, polyvinyl pyrrolidone and additives, and the mass ratio of neutral glue AKD, nanocellulose, polyvinyl pyrrolidone and additives is 60:25:14:1.
[0028] Preferably, the amount of glue applied in step 3 is 15-20 g / m 2 .
[0029] Preferably, the auxiliary agent in the sizing agent in step three includes sorbitol.
[0030] Preferably, the heat-sealable self-adhesive high-strength medical dialysis paper is obtained by the processing method of the heat-sealable self-adhesive high-strength medical dialysis paper.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] In the present invention, biodegradable softwood pulp, hardwood pulp and modified chitosan fiber are used as raw materials, and a reasonable pore structure is achieved by matching different fiber components, so that the prepared dialysis paper has excellent air permeability and strength. At the same time, by coating a sizing agent on the semi-finished medical dialysis paper, a heat-sealed self-adhesive medical dialysis paper is obtained, which has good heat-sealing strength.
[0033] In the preparation process of modified chitosan in the present invention, kaolin and nano-titanium dioxide are contacted in an aqueous medium, and the hydroxyl groups on the surfaces of the two are dehydrated to form a chemical bond to obtain a titanium dioxide / kaolin composite material. Then, 3-aminopropyltrimethoxysilane is used to modify the titanium dioxide / kaolin composite material, and amino groups are introduced on the surface of the titanium dioxide / kaolin composite material. The amino groups on the surface of the titanium dioxide / kaolin composite material and the amino groups on the surface of the chitosan fiber are cross-linked under the action of the cross-linking agent glyoxal to obtain modified chitosan. Kaolin and nano-titanium dioxide can improve the smoothness, opacity, printing performance, etc. of dialysis paper, improve its heat resistance, increase stability, and extend service life. The titanium dioxide / kaolin composite material is used as a filler, and the two work synergistically and can be used as a partial substitute for the fiber. Through the chemical grafting method, agglomeration is effectively avoided, and it can be evenly dispersed in the fiber to improve the strength and toughness of the dialysis paper. Nano-titanium dioxide can generate ·OH and O2 under light conditions. - , H2O2 and other strong oxidizing substances intervene in the lipid peroxidation process of bacterial cell membranes, change the concentration of various components in the cell membrane, lead to metabolic imbalance of bacterial cell membranes and subsequent degradation, photocatalytically oxidize substances in cells, promote cell death, the unreacted amino groups in the chitosan fiber molecular chain and the Schiff base groups generated after the reaction have a strong adsorption effect on negatively charged bacteria, and the large number of hydroxyl active groups in the fibers of each component enhance the adsorption and flocculation of bacteria, and the obtained dialysis paper has a strong antibacterial effect.
[0034] The neutral glue AKD in the sizing agent of the present invention can directly react with the active -OH group on the nanocellulose to generate a strong β-ketoester type covalent bond, which greatly enhances the water-resistant effect of the paper sample and effectively prevents bacteria from penetrating, making it have good antibacterial effect. The small size and large specific surface area of nanocellulose fill the gaps between the paper sheets, improve the surface properties of the paper, and improve the strength, barrier properties and smoothness of the dialysis paper. The heat-sealed self-adhesive high-strength medical dialysis paper after sizing has the advantages of good antibacterial and antibacterial properties, strong air permeability and high strength. DETAILED DESCRIPTION
[0035] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0036] Example 1
[0037] A method for preparing heat-sealed self-adhesive high-strength medical dialysis paper comprises the following steps:
[0038] Step 1: by weight, 35 parts by weight of coniferous wood pulp and 24 parts by weight of hardwood wood pulp are mixed and beaten, the beating time is 40 minutes, the beating degree is 34SR, and then 20 parts by weight of modified chitosan fiber are added and mixed to obtain a mixed slurry;
[0039] Step 2: Add 0.2 parts of wet strength agent cationic polyacrylamide and 2 parts of reinforcing agent cationic starch to 100 parts of the mixed slurry by weight, mix well, and form on a Fourdrinier paper machine to obtain a semi-finished medical dialysis paper;
[0040] Step 3: Apply the sizing agent to the semi-finished medical dialysis paper, wherein the sizing agent is composed of neutral glue AKD, nanocellulose, polyvinyl pyrrolidone and auxiliary agent sorbitol in a mass ratio of 60:25:14:1, and dry. The sizing amount is 15g / m 2 , and obtain heat-sealable self-adhesive high-strength medical dialysis paper.
[0041] The modified chitosan fiber is prepared by the following steps:
[0042] S1. Mix kaolin, sodium hydroxide and deionized water evenly, then add nano-titanium dioxide and polyethylene glycol, wherein the mass ratio of the added kaolin, sodium hydroxide, deionized water, nano-titanium dioxide and polyethylene glycol-1000 is 100:350:10:5:38, stir and mix, react at 50°C for 1h, after the reaction, filter, wash with deionized water, and dry in a vacuum drying oven at 60°C for 18h to obtain a titanium dioxide / kaolin composite material;
[0043] S2, mixing the titanium dioxide / kaolin composite material and toluene uniformly, adding deionized water and 3-aminopropyltrimethoxysilane, the mass ratio of the added titanium dioxide / kaolin composite material, toluene, deionized water and 3-aminopropyltrimethoxysilane is 100:2400:30:255, stirring and mixing, reacting at 85°C for 24h, after the reaction, centrifuging, washing with ethanol, and drying at 80°C for 12h to obtain an amino-modified titanium dioxide / kaolin composite material;
[0044] S3. Immerse the chitosan fiber in a glyoxal aqueous solution, add amino-modified titanium dioxide / kaolin composite material, wherein the mass ratio of the added chitosan fiber, glyoxal aqueous solution and amino-modified titanium dioxide / kaolin composite material is 100:2500:8, stir and mix evenly, react at 40°C for 2h, after the reaction, wash with deionized water, and dry in a drying oven at 50°C for 12h to obtain modified chitosan.
[0045] Example 2
[0046] A method for preparing heat-sealed self-adhesive high-strength medical dialysis paper comprises the following steps:
[0047] Step 1: by weight, 42 parts by weight of coniferous wood pulp and 28 parts by weight of hardwood wood pulp are mixed and beaten, the beating time is 45 minutes, the beating degree is 38°SR, and then 30 parts by weight of modified chitosan fiber are added and mixed to obtain a mixed slurry;
[0048] Step 2: Add 0.5 parts of wet strength agent cationic polyacrylamide and 2.5 parts of reinforcing agent cationic starch to 100 parts of the mixed slurry by weight, mix well, and form on a Fourdrinier paper machine to obtain a semi-finished medical dialysis paper;
[0049] Step 3: Apply the sizing agent to the semi-finished medical dialysis paper, wherein the sizing agent is composed of neutral glue AKD, nanocellulose, polyvinyl pyrrolidone and auxiliary agent sorbitol in a mass ratio of 60:25:14:1, and dry. The sizing amount is 18g / m 2 , and obtain heat-sealable self-adhesive high-strength medical dialysis paper.
[0050] The modified chitosan fiber is prepared by the following steps:
[0051] S1. Mix kaolin, sodium hydroxide and deionized water evenly, then add nano-titanium dioxide and polyethylene glycol, wherein the mass ratio of the added kaolin, sodium hydroxide, deionized water, nano-titanium dioxide and polyethylene glycol-1000 is 100:420:14:10:45, stir and mix, react at 55°C for 1.5h, after the reaction, filter, wash with deionized water, and dry in a vacuum drying oven at 60°C for 18h to obtain a titanium dioxide / kaolin composite material;
[0052] S2, mixing the titanium dioxide / kaolin composite material and toluene evenly, adding deionized water and 3-aminopropyltrimethoxysilane, the mass ratio of the added titanium dioxide / kaolin composite material, toluene, deionized water and 3-aminopropyltrimethoxysilane is 100:2550:38:280, stirring and mixing, reacting at 90°C for 28h, after the reaction, centrifuging, washing with ethanol, and drying at 80°C for 12h to obtain an amino-modified titanium dioxide / kaolin composite material;
[0053] S3. Immerse the chitosan fiber in a glyoxal aqueous solution, add an amino-modified titanium dioxide / kaolin composite material, wherein the mass ratio of the added chitosan fiber, the glyoxal aqueous solution and the amino-modified titanium dioxide / kaolin composite material is 100:2800:12, stir and mix evenly, react at 42°C for 2.5h, and after the reaction, wash with deionized water and dry in a drying oven at 50°C for 12h to obtain modified chitosan.
[0054] Example 3
[0055] A method for preparing heat-sealed self-adhesive high-strength medical dialysis paper comprises the following steps:
[0056] Step 1: by weight, 42 parts by weight of coniferous wood pulp and 28 parts by weight of hardwood wood pulp are mixed and beaten, the beating time is 45 minutes, the beating degree is 38°SR, and then 30 parts by weight of modified chitosan fiber are added and mixed to obtain a mixed slurry;
[0057] Step 2: Add 0.5 parts of wet strength agent cationic polyacrylamide and 2.5 parts of reinforcing agent cationic starch to 100 parts of the mixed slurry by weight, mix well, and form on a Fourdrinier paper machine to obtain a semi-finished medical dialysis paper;
[0058] Step 3: Apply the sizing agent to the semi-finished medical dialysis paper, wherein the sizing agent is composed of neutral glue AKD, nanocellulose, polyvinyl pyrrolidone and auxiliary agent sorbitol in a mass ratio of 60:25:14:1, and dry. The sizing amount is 18g / m 2 , and obtain heat-sealable self-adhesive high-strength medical dialysis paper.
[0059] The modified chitosan fiber is prepared by the following steps:
[0060] S1. Mix kaolin, sodium hydroxide and deionized water evenly, then add nano-titanium dioxide and polyethylene glycol, wherein the mass ratio of the added kaolin, sodium hydroxide, deionized water, nano-titanium dioxide and polyethylene glycol-1000 is 100:500:16:12:50, stir and mix, react at 55°C for 1.5h, after the reaction, filter, wash with deionized water, and dry in a vacuum drying oven at 60°C for 18h to obtain a titanium dioxide / kaolin composite material;
[0061] S2, mixing the titanium dioxide / kaolin composite material and toluene uniformly, adding deionized water and 3-aminopropyltrimethoxysilane, the mass ratio of the added titanium dioxide / kaolin composite material, toluene, deionized water and 3-aminopropyltrimethoxysilane is 100:2700:42:305, stirring and mixing, reacting at 90°C for 28h, after the reaction, centrifuging, washing with ethanol, and drying at 80°C for 12h to obtain an amino-modified titanium dioxide / kaolin composite material;
[0062] S3. Immerse the chitosan fiber in a glyoxal aqueous solution, add amino-modified titanium dioxide / kaolin composite material, wherein the mass ratio of the added chitosan fiber, glyoxal aqueous solution and amino-modified titanium dioxide / kaolin composite material is 100:3000:14, stir and mix evenly, react at 42°C for 2.5h, after the reaction, wash with deionized water, and dry in a drying oven at 50°C for 12h to obtain modified chitosan.
[0063] Example 4
[0064] A method for preparing heat-sealed self-adhesive high-strength medical dialysis paper comprises the following steps:
[0065] Step 1: by weight, 50 parts by weight of coniferous wood pulp and 32 parts by weight of hardwood wood pulp are mixed and beaten for 48 minutes at a beating degree of 38°SR, and then 40 parts by weight of modified chitosan fiber are added and mixed to obtain a mixed slurry;
[0066] Step 2: Add 0.8 parts of wet strength agent cationic polyacrylamide and 2.8 parts of reinforcing agent cationic starch to 100 parts of the mixed slurry by weight, mix well, and form on a Fourdrinier paper machine to obtain a semi-finished medical dialysis paper;
[0067] Step 3: Apply the sizing agent to the semi-finished medical dialysis paper, wherein the sizing agent is composed of neutral glue AKD, nanocellulose, polyvinyl pyrrolidone and auxiliary agent sorbitol in a mass ratio of 60:25:14:1, and dry. The sizing amount is 18g / m 2 , and obtain heat-sealable self-adhesive high-strength medical dialysis paper.
[0068] The preparation method of the modified chitosan fiber is the same as that in Example 3.
[0069] Example 5
[0070] A method for preparing heat-sealed self-adhesive high-strength medical dialysis paper comprises the following steps:
[0071] Step 1: by weight, 55 parts by weight of coniferous wood pulp and 36 parts by weight of hardwood wood pulp are mixed and beaten, the beating time is 50 minutes, the beating degree is 40°SR, and then 45 parts by weight of modified chitosan fiber are added and mixed to obtain a mixed slurry;
[0072] Step 2: Add 1 part of wet strength agent cationic polyacrylamide and 3 parts of reinforcing agent cationic starch to 100 parts of the mixed slurry by weight, mix well, and form on a Fourdrinier paper machine to obtain a semi-finished medical dialysis paper;
[0073] Step 3: Apply the sizing agent to the semi-finished medical dialysis paper, wherein the sizing agent is composed of neutral glue AKD, nanocellulose, polyvinyl pyrrolidone and auxiliary agent sorbitol in a mass ratio of 60:25:14:1, and dry. The sizing amount is 20g / m 2 , and obtain heat-sealable self-adhesive high-strength medical dialysis paper.
[0074] The modified chitosan fiber is prepared by the following steps:
[0075] S1. Mix kaolin, sodium hydroxide and deionized water evenly, then add nano-titanium dioxide and polyethylene glycol, wherein the mass ratio of the added kaolin, sodium hydroxide, deionized water, nano-titanium dioxide and polyethylene glycol-1000 is 100:550:18:15:55, stir and mix, react at 60°C for 2h, after the reaction, filter, wash with deionized water, and dry in a vacuum drying oven at 60°C for 18h to obtain a titanium dioxide / kaolin composite material;
[0076] S2, mixing the titanium dioxide / kaolin composite material and toluene uniformly, adding deionized water and 3-aminopropyltrimethoxysilane, the mass ratio of the added titanium dioxide / kaolin composite material, toluene, deionized water and 3-aminopropyltrimethoxysilane is 100:2800:45:315, stirring and mixing, reacting at 95°C for 30h, after the reaction, centrifuging, washing with ethanol, and drying at 80°C for 12h to obtain an amino-modified titanium dioxide / kaolin composite material;
[0077] S3. Immerse the chitosan fiber in a glyoxal aqueous solution, add amino-modified titanium dioxide / kaolin composite material, wherein the mass ratio of the added chitosan fiber, glyoxal aqueous solution and amino-modified titanium dioxide / kaolin composite material is 100:3200:15, stir and mix evenly, react at 45°C for 3h, after the reaction, wash with deionized water, and dry in a drying oven at 50°C for 12h to obtain modified chitosan.
[0078] Comparative Example 1
[0079] A method for preparing heat-sealed self-adhesive high-strength medical dialysis paper comprises the following steps:
[0080] Step 1: by weight, 50 parts by weight of coniferous wood pulp and 32 parts by weight of hardwood wood pulp are mixed and beaten for 48 minutes at a beating degree of 38°SR, and then 5 parts by weight of titanium dioxide / kaolin composite material and 35 parts of chitosan fiber are added and mixed to obtain a mixed slurry;
[0081] Step 2: Add 0.8 parts of wet strength agent cationic polyacrylamide and 2.8 parts of reinforcing agent cationic starch to 100 parts of the mixed slurry by weight, mix well, and form on a Fourdrinier paper machine to obtain a semi-finished medical dialysis paper;
[0082] Step 3: Apply the sizing agent to the semi-finished medical dialysis paper, wherein the sizing agent is composed of neutral glue AKD, nanocellulose, polyvinyl pyrrolidone and auxiliary agent sorbitol in a mass ratio of 60:25:14:1, and dry. The sizing amount is 18g / m 2 , and obtain heat-sealable self-adhesive high-strength medical dialysis paper.
[0083] The titanium dioxide / kaolin composite material is prepared by the following steps:
[0084] Kaolin, sodium hydroxide and deionized water are mixed evenly, and then nano-titanium dioxide and polyethylene glycol are added, wherein the mass ratio of the added kaolin, sodium hydroxide, deionized water, nano-titanium dioxide and polyethylene glycol-1000 is 100:500:16:12:50. The mixture is stirred and reacted at 55°C for 1.5 hours. After the reaction, the mixture is filtered, washed with deionized water, and dried in a vacuum drying oven at 60°C for 18 hours to obtain a titanium dioxide / kaolin composite material.
[0085] The softwood pulp used in the embodiments and comparative examples of the present invention is bleached kraft softwood pulp; the hardwood pulp is bleached hardwood; chitosan fiber (CS) was purchased from Qingdao Marine Bioengineering Co., Ltd.; kaolin was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., and its chemical composition formula is (Si 1.95 Al 0.05 )(Al 1.94 Mg 0.02 Fe 0.04 )O5(OH)4Na 0.04 K 0.04 , with an average particle size of 1.32 μm; nano titanium dioxide was purchased from Xuancheng Jingrui New Materials Co., Ltd., model JR05, with an average particle size of 5 nm; cationic polyacrylamide and neutral gum AKD were purchased from Zhejiang Longyou Futian Paper Refining Co., Ltd.; cationic starch was purchased from Jiangxi Hongda Chemical Co., Ltd., and nanocellulose was purchased from Funa New Materials Technology (Shanghai) Co., Ltd.; other raw materials and reagents were commercially available.
[0086] The heat-sealable self-adhesive high-strength medical dialysis papers in Examples 1-5 and Comparative Example 1 were used as samples for performance tests, and the relevant performance tests are as follows:
[0087] (1) Burst resistance test: The heat-sealable self-adhesive high-strength medical dialysis paper prepared in Examples 1-5 and Comparative Example 1 was subjected to a burst resistance test. The test method adopted the test standard of GB / T 454-2020 "Determination of burst resistance of paper". The test results are recorded as shown in Table 1:
[0088] Table 1
[0089]
[0090] According to the test results in Table 1, it can be seen that the heat-sealable self-adhesive high-strength medical dialysis paper in Examples 1-5 of the present invention has excellent burst resistance, wherein the burst resistance index corresponding to Example 4 is 8.7 kPa·m 2 / g. With the different components of softwood pulp, hardwood pulp and modified chitosan fiber, the bursting index shows an upward trend from Examples 1 to 4. In Comparative Example 1, the titanium dioxide / kaolin composite material is not modified, and the titanium dioxide / kaolin composite material is not cross-linked with the chitosan fiber. The strength of the dialysis paper is reduced, and the bursting index is reduced to 7.2 kPa·m 2 / g.
[0091] (2) Air permeability test: The heat-sealable self-adhesive high-strength medical dialysis paper prepared in Examples 1-5 and Comparative Example 1 was tested for air permeability. The test method adopted the test standard of GB / T 458-2008 "Determination of air permeability of paper and paperboard". The test results are recorded as shown in Table 2:
[0092] Table 2
[0093]
[0094] According to the test results in Table 2, it can be seen that the heat-sealable self-adhesive high-strength medical dialysis paper in Examples 1-5 of the present invention achieves a reasonable pore structure by matching different fiber components, and the prepared dialysis paper has excellent air permeability. With the increase of the amount of sizing, the air permeability decreases. The air permeability of the corresponding heat-sealable self-adhesive high-strength medical dialysis paper in Example 1 can reach 6.3 μm·Pa- 1 ·s- 1 In Comparative Example 1, the chitosan fiber and titanium dioxide / kaolin composite material were not cross-linked, which had a certain effect on the air permeability, which was 5.4 μm·Pa- 1 ·s- 1 .
[0095] (3) Bacterial barrier test: The heat-sealable self-adhesive high-strength medical dialysis paper prepared in Examples 1-5 and Comparative Example 1 was subjected to a bacterial barrier test. The paper substrates were cut into squares with a side length of 50 mm, and 5 paper substrates in each group were used as parallel samples. The test bacteria were sterilized. The test bacteria were Bacillus subtilis, which was purchased from the China Industrial Microbiological Culture Collection Center. A nutrient agar medium was prepared: 3 g beef extract, 5 g peptone, 5 g sodium chloride, 15 g agar, and 1000 mL distilled water. The pH was adjusted to 7.0. 5 mg of MnSO4·H2O was added to the nutrient agar medium. Bacillus subtilis was cultured for 24 h. The cultured Bacillus subtilis was diluted to obtain 10 7 cfu / mL of Bacillus subtilis suspension, transfer the sterilized sample to a sterile plate, and take 10 7 5 drops of Bacillus subtilis suspension with a concentration of 1.5 cfu / mL, 0.1 mL per drop, were evenly dropped on the outer surface of the sample without contacting each other. After drying for 12 hours at a temperature of 25°C and a relative humidity of 50%, the inner surface of the infected sample was completely spread on the surface of the nutrient agar culture medium. After 5 seconds, the infected sample was discarded; the nutrient agar culture medium was cultured at 37°C for 24 hours, the bacterial growth was observed, and the number of bacteria grown was recorded. The test results are shown in Table 3:
[0096] Table 3
[0097]
[0098] According to the test results in Table 3, it can be seen that the heat-sealed self-adhesive high-strength medical dialysis papers corresponding to Examples 1-5 and Comparative Example 1 of the present invention all have excellent antibacterial properties. Nano-titanium dioxide and chitosan fiber have excellent antibacterial effects. After the cross-linking reaction, the unreacted amino groups in the chitosan fiber molecular chain and the Schiff base groups generated after the reaction have a strong adsorption effect on negatively charged bacteria.
[0099] Can generate OH and O2 under light conditions - , H2O2 and other strong oxidizing substances intervene in the lipid peroxidation process of the bacterial cell membrane, change the concentration of each component in the cell membrane, cause the metabolic imbalance of the bacterial cell membrane and subsequent degradation, photocatalytically oxidize the substances in the cell, and promote cell death. The unreacted amino groups in the chitosan fiber molecular chain and the Schiff base groups generated after the reaction have a strong adsorption effect on negatively charged bacteria. At the same time, a large number of hydroxyl active groups in the fibers of each component strengthen the adsorption and flocculation of bacteria, and the obtained dialysis paper has a strong antibacterial effect. No cross-linking treatment was performed in Comparative Example 1, but the chitosan fiber contained a large number of amino groups, and the positive charge interacted with the negative charge on the bacterial cell membrane, effectively changing the permeability of the bacterial cells and promoting the death of the bacterial cells.
[0100] Although the embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that all equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A method for processing heat-sealed self-adhesive high-strength medical dialysis paper, characterized in that: The steps include: Step 1, mixing and beating softwood pulp and hardwood pulp, and then adding modified chitosan fiber to mix to obtain a mixed slurry; The raw materials are calculated by weight, including 35-55 parts of coniferous wood pulp, 24-36 parts of hardwood pulp and 20-45 parts of modified chitosan fiber; Step 2, adding a wet strength agent and a reinforcing agent to the mixed slurry, mixing evenly, and then forming into a sheet to obtain a semi-finished medical dialysis paper; The raw materials are calculated by weight, including 100 parts of mixed slurry, 0.2-1 parts of wet strength agent and 2-3 parts of reinforcing agent; Step 3, applying the sizing agent to the semi-finished medical dialysis paper, and drying, to obtain heat-sealed self-adhesive high-strength medical dialysis paper; The modified chitosan fiber in step 1 is prepared by the following steps: S1. Evenly mix kaolin, sodium hydroxide and deionized water, then add nano titanium dioxide and polyethylene glycol, stir and mix to react, filter after the reaction, wash with deionized water, and dry in a vacuum drying oven at 60° C. for 18 h to obtain a titanium dioxide / kaolin composite material; S2, mixing the titanium dioxide / kaolin composite material and toluene uniformly, adding deionized water and 3-aminopropyltrimethoxysilane, stirring and mixing, reacting, centrifuging after the reaction, washing with ethanol, and drying at 80° C. for 12 h to obtain an amino-modified titanium dioxide / kaolin composite material; S3, immersing chitosan fiber in glyoxal aqueous solution, adding amino-modified titanium dioxide / kaolin composite material, stirring and mixing evenly to react, washing with deionized water after the reaction, and drying in a drying oven at 50° C. for 12 hours to obtain modified chitosan; In the step 3, the sizing agent is composed of neutral glue AKD, nanocellulose, polyvinyl pyrrolidone and an auxiliary agent, and the mass ratio of neutral glue AKD, nanocellulose, polyvinyl pyrrolidone and the auxiliary agent is 60:25:14:1; The amount of glue applied in step 3 is 15-20g / m 2 The mass ratio of kaolin, sodium hydroxide, deionized water, nano-titanium dioxide and polyethylene glycol in S1 is 100:350-550:10-18:5-15:38-55, and the mass ratio of chitosan fiber, glyoxal aqueous solution and amino-modified titanium dioxide / kaolin composite material in S3 is 100:2500-3200:8-15.
2. The method for processing a heat-sealable self-adhesive high-strength medical dialysis paper according to claim 1, characterized in that: The wet strength agent in step 2 includes one of cationic polyacrylamide and polyamide polyepichlorohydrin resin.
3. The method for processing a heat-sealable self-adhesive high-strength medical dialysis paper according to claim 1, characterized in that: The reinforcing agent in step 2 includes cationic starch.
4. A heat-sealable self-adhesive high-strength medical dialysis paper obtained by the processing method of a heat-sealable self-adhesive high-strength medical dialysis paper according to any one of claims 1 to 3.