Silicon-carbon anode materials for lithium-ion batteries and their preparation methods
By using a multi-layered core-shell structure for lithium-ion battery silicon-carbon anode materials, the volume expansion problem of silicon-based anode materials during charge and discharge processes has been solved, resulting in higher coulombic efficiency and cycle stability, and improved battery performance.
Patent Information
- Application Number
- CN202310880397.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-18
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-07-18
AI Technical Summary
Existing silicon-based anode materials for lithium-ion batteries suffer from severe volume expansion during charge and discharge, leading to material pulverization and contact with the electrolyte, which affects cycle stability and initial irreversible capacity.
The lithium-ion battery silicon-carbon anode material with a multi-layer core-shell structure includes a silicon-carbon matrix and graphite as the core, a vapor-deposited carbon coating layer as the shell, a porous hard carbon coating layer and a hollow interlayer, combined with elemental metals, and forms a porous structure through strong acid etching to increase conductivity and buffering effect.
It effectively suppressed the volume expansion of nano-silicon, reduced the risk of material pulverization and shedding, improved the coulombic efficiency and capacity retention of lithium-ion batteries, and enhanced electrochemical performance and cycle stability.
Smart Images

Figure CN116885186B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium battery technology, specifically relating to a silicon-carbon anode material for lithium-ion batteries and its preparation method, as well as a lithium-ion battery using the silicon-carbon anode material as the anode. Background Technology
[0002] In recent years, with the development of science and technology and the improvement of people's living standards, the standards for new green energy have been continuously raised. Currently, silicon-based anode materials in the lithium-ion battery field have been propelled onto the stage of energy storage material development due to their high capacity, low voltage, and abundant reserves. To improve the energy density and cycle stability of silicon anode materials and address the problems caused by the volume expansion (~300%) of silicon during charging and discharging, which leads to material pulverization and detachment, it is necessary to modify the material to suppress its volume expansion and avoid direct contact between the active material and the electrolyte. This will allow the active material to fully exert its electrochemical performance, reduce the initial irreversible capacity, and improve cycle stability—a pressing issue that needs to be addressed.
[0003] CN109659551.A proposes a method for preparing a low-expansion silicon anode material for lithium-ion batteries. The method involves adding hydroquinone, formaldehyde, and sodium carbonate to a silicon aqueous solution slurry to prepare a silica sol; aging the silica solution to obtain a silica gel; aging and carbonizing the silica gel to obtain a carbonized material; pulverizing and classifying the carbonized material to obtain a silicon-carbon composite material A; impregnating and coating the silicon-carbon composite material A with mesophase pitch to obtain a coating material B; and then carbonizing and sieving the coating material B to obtain the low-expansion silicon anode material for lithium-ion batteries. However, this method has high processing costs and relatively low protective layer strength. Summary of the Invention
[0004] Based on the problems of existing technologies, this invention provides a novel method for preparing silicon-carbon anode materials for lithium-ion batteries. The method employs a multi-layer core-shell structure, which can effectively suppress the volume expansion of nano-silicon, reduce the contact area with the electrolyte, increase the synergistic effect between nano-silicon and graphite, and improve the coulombic efficiency and capacity retention of lithium-ion batteries.
[0005] This invention first provides a silicon-carbon anode material for lithium-ion batteries, which has a silicon-carbon matrix and graphite as the core and a vapor-deposited carbon coating layer as the shell, forming an outer core-shell structure; the silicon-carbon matrix has nano-silicon as the core and a porous hard carbon coating layer as the shell, and the porous hard carbon coating layer has pores, and there is a hollow interlayer between the nano-silicon and the porous hard carbon coating layer, forming an inner core-double-shell structure; the porous hard carbon coating layer pores and the hollow interlayer contain a metallic element; the metallic element is at least one of Ag, Mg, and Al.
[0006] In the aforementioned silicon-carbon anode material for lithium-ion batteries, the thickness of the vapor-deposited carbon coating layer is 10–30 nm.
[0007] In the aforementioned silicon-carbon anode material for lithium-ion batteries, the porous hard carbon coating layer has micropores as its main pore type, with a pore size of less than 2 nm.
[0008] In the aforementioned silicon-carbon anode material for lithium-ion batteries, the thickness of the hollow interlayer is 1–5 nm.
[0009] The present invention also provides a method for preparing the above-mentioned silicon-carbon anode material for lithium-ion batteries, which includes the following steps:
[0010] A. Preparation of silicon-carbon matrix: Nano-silicon, hard carbon precursor material, and organic solvent are mixed, heated and stirred to remove the organic solvent, dried, and the powder is collected; the powder is carbonized under inert gas protection to obtain Si@SiO. x @C material; Si@SiO x @C material is added to a strongly acidic solution containing metal ions, and after sonication, washing and drying, a silicon-carbon matrix is obtained;
[0011] B. The silicon-carbon matrix obtained in step A is mixed with graphite in a solid phase. The resulting material is coated and carbonized under a mixed atmosphere of inert gas and carbon precursor gas. After cooling, it is sieved to obtain the Si@void@C / Gr@C composite material, which is the silicon-carbon anode material for lithium-ion batteries.
[0012] In the preparation method of the silicon-carbon anode material for lithium-ion batteries, in step A, the organic solvent is at least one of methanol, ethanol, ethylene glycol, propanol, isopropanol, n-butanol, acetone, toluene, and xylene.
[0013] In the preparation method of the silicon-carbon anode material for lithium-ion batteries, in step A, the median particle size of the nano-silicon is 40–150 nm, and the surface has SiO₂. x(1<x<2) Passivation layer.
[0014] Preferably, in the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, the thickness of the passivation layer in step A is 1-5 nm.
[0015] In the preparation method of the silicon-carbon anode material for lithium-ion batteries, in step A, the hard carbon precursor material is at least one of polyaniline, polypyrrole, polystyrene, polyacrylonitrile, polyimide, polyvinylidene chloride, sucrose, glucose, and phenolic resin.
[0016] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, in step A, the mass ratio of the organic solvent to the hard carbon precursor material is 10-40:1.
[0017] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, in step A, the mass ratio of nano-silicon to hard carbon precursor material is 5-10:1-2.
[0018] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, in step A, the temperature for heating and stirring to remove organic solvent is 50–200°C.
[0019] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, in step A, the time for heating and stirring to remove organic solvent is 3 to 12 hours.
[0020] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, in step A, the rotation speed for heating and stirring to remove organic solvent is 100-1000 rpm.
[0021] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, in step A, the drying temperature is 50–200°C.
[0022] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, the drying time in step A is 3 to 12 hours.
[0023] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, in step A, the carbonization temperature is 700-1300℃ and the heating rate is 2-15℃ / min.
[0024] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, in step A, the carbonization holding time is 1 to 10 hours.
[0025] In the preparation method of the silicon-carbon anode material for lithium-ion batteries, in step A, the inert gas is nitrogen or argon, and the gas flow rate is 10-50 L / min.
[0026] In the preparation method of the silicon-carbon anode material for lithium-ion batteries, in step A, the strong acid solution is at least one of sulfuric acid, nitric acid, hydrofluoric acid, and hydrochloric acid, and the hydrogen ion concentration in the solution is 1-10 mol / L.
[0027] In the preparation method of the silicon-carbon anode material for lithium-ion batteries, in step A, the metal ions in the strongly acidic solution containing metal ions are Ag. + Mg 2+ Al 3+ At least one of them.
[0028] In the preparation method of the silicon-carbon anode material for lithium-ion batteries, in step A, the concentration of metal ions in the strongly acidic solution containing metal ions is 0.1–0.5 mol / L.
[0029] In the above-mentioned method for preparing silicon-carbon anode materials for lithium-ion batteries, in step A, the Si@SiO x The mass ratio of the @C material to the volume ratio of the strongly acidic solution containing metal ions is 1g: 2.5~6mL.
[0030] In the preparation method of the silicon-carbon anode material for lithium-ion batteries, in step B, the graphite is artificial graphite or natural graphite.
[0031] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, in step B, the mass ratio of graphite to silicon-carbon matrix is 1 to 1.5:1.
[0032] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, in step B, the median particle size of the graphite is 3-20 μm.
[0033] In the preparation method of the silicon-carbon anode material for lithium-ion batteries, in step B, the inert gas is nitrogen or argon.
[0034] In the preparation method of the silicon-carbon anode material for lithium-ion batteries, in step B, the carbon precursor gas is at least one of methane, ethane, propane, ethylene, propylene, and acetylene.
[0035] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, in step B, the flow rate of the carbon precursor gas is 2-10 L / min.
[0036] In the preparation method of the silicon-carbon anode material for lithium-ion batteries, in step B, the inlet gas flow rate ratio of the inert gas to the carbon precursor gas is 1-10:99-90.
[0037] In the preparation method of the silicon-carbon anode material for lithium-ion batteries, in step B, the rotation speed of the solid-phase mixing is 2000-3000 rpm.
[0038] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, in step B, the solid-phase mixing time is 10-60 min.
[0039] In the above-mentioned method for preparing silicon-carbon anode material for lithium-ion batteries, in step B, the vapor deposition carbonization temperature is 700–1300℃, and the heating rate is 2–15℃ / min.
[0040] In the preparation method of the silicon-carbon anode material for lithium-ion batteries, step B involves sieving through a 325-mesh sieve and taking the material passing through the sieve.
[0041] Based on the above-mentioned silicon-carbon anode material, the present invention also provides a lithium-ion battery anode, which is prepared from the above-mentioned silicon-carbon anode material or the silicon-carbon anode material prepared by the above method.
[0042] Based on the aforementioned silicon-carbon anode material or anode, the present invention also provides a lithium-ion battery, which uses the aforementioned lithium-ion battery anode as the anode.
[0043] The beneficial effects of this invention are:
[0044] This invention first employs a hollow sandwich layer and a porous hard carbon coating layer as a buffer layer for silicon volume expansion, reducing the risk of material pulverization and detachment. The strong acid solution etches away the SiO₂... x While passivating the layer, it also chemically activates the hard carbon coating, increasing its pore count. After etching, Ag... + Mg 2+ Al 3+ Metal ions increase the electrical contact between the core and shell, improving conductivity and lithium-ion insertion / extraction rates. Then, because the molecular structure of the hard carbon coating layer is similar to that of graphite, it is easier to combine to form a silicon-graphite composite material. Simultaneously, graphite can also buffer the expansion of the nano-silicon active material. Finally, a carbon coating layer is deposited using vapor deposition to achieve a uniform external carbon layer, avoiding the formation of a large amount of SEI film due to contact between the active material and the electrolyte. The entire process is simple, straightforward, and easy to implement. Battery performance tests demonstrated excellent physical and electrochemical properties, with significant improvements in the cycle stability and initial charge / discharge efficiency of the active material. Attached Figure Description
[0045] Figure 1 This is a schematic diagram of the silicon-carbon anode material of the present invention.
[0046] Figure 2 This is a TEM image of the silicon-carbon matrix of the present invention.
[0047] Figure 3 This is a SEM image of the negative electrode active material of the present invention. Detailed Implementation
[0048] Specifically, the silicon-carbon anode material for lithium-ion batteries has an outer core-shell structure consisting of a silicon-carbon matrix and graphite as the core, and a vapor-deposited carbon coating layer as the shell. The silicon-carbon matrix has a nano-silicon core and a porous hard carbon coating layer as the shell, with channels in the porous hard carbon coating layer. There is a hollow interlayer between the nano-silicon and the porous hard carbon coating layer, forming an inner core-double-shell structure. A metallic element exists in the channels and hollow interlayer of the porous hard carbon coating layer. The metallic element is at least one of Ag, Mg, and Al.
[0049] In the silicon-carbon anode material of lithium-ion batteries, the graphite particles are larger than the silicon-carbon matrix, and the molecular structure of the carbon material has already been formed. Therefore, the graphite is not a single layer and does not form a coating on silicon. Instead, it is a composite material formed by mutual adsorption with the silicon-carbon matrix due to weak interaction forces. The metal element is produced by the reduction of metal ions in strong acid solution with Si-H bonds on the silicon surface or water molecules.
[0050] In the silicon-carbon anode material for lithium-ion batteries of this invention, the thickness of the vapor-deposited carbon coating layer is 10–30 nm; the porous hard carbon coating layer has micropores as its main pore type, with a pore size of less than 2 nm; the thickness of the hollow interlayer is 1–5 nm, and this hollow interlayer is formed by etching away SiO2 with a strongly acidic solution. x The passivation layer remains.
[0051] This invention also provides a method for preparing the above-mentioned silicon-carbon anode material for lithium-ion batteries, comprising the following steps:
[0052] A. Preparation of silicon-carbon matrix: Nano-silicon, hard carbon precursor material, and organic solvent are mixed, heated and stirred to remove the organic solvent, dried, and the powder is collected; the powder is carbonized under inert gas protection to obtain Si@SiO. x @C material; Si@SiO x @C material is added to a strongly acidic solution containing metal ions, and after sonication, washing and drying, a silicon-carbon matrix is obtained;
[0053] B. The silicon-carbon matrix obtained in step A is mixed with graphite in a solid phase. The resulting material is coated and carbonized under a mixed atmosphere of inert gas and carbon precursor gas. After cooling, it is sieved to obtain the Si@void@C / Gr@C composite material, which is the silicon-carbon anode material for lithium-ion batteries.
[0054] In step A of the preparation method of this invention, the median particle size of the nano-silicon is 40-150 nm, and the surface has SiO₂. x(1<x<2) Passivation layer; by controlling the thickness of the passivation layer to 1–5 nm, a hollow sandwich layer with a thickness of 1–5 nm between the nano-silicon and the porous hard carbon coating layer is obtained.
[0055] In step A of the preparation method of the present invention, the organic solvent is at least one selected from methanol, ethanol, ethylene glycol, propanol, isopropanol, n-butanol, acetone, toluene, and xylene; the hard carbon precursor material is at least one selected from polyaniline, polypyrrole, polystyrene, polyacrylonitrile, polyimide, polyvinylidene chloride, sucrose, glucose, and phenolic resin; the mass ratio of the organic solvent to the hard carbon precursor material is 10-40:1; and the mass ratio of the nano-silicon to the hard carbon precursor material is 5-10:1-2.
[0056] In step A of the preparation method of this invention, an organic solvent is first added to dissolve the hard carbon precursor, and then the organic solvent is removed by heating and stirring in a reaction vessel. The temperature for heating and stirring to remove the organic solvent is 50-200°C, the time is 3-12 hours, and the rotation speed is 100-1000 rpm. Then the material after removing the organic solvent is dried at a temperature of 50-200°C for 3-12 hours.
[0057] In step A of the preparation method of the present invention, the carbonization temperature is controlled at 700-1300℃, the heating rate is 2-15℃ / min, and the carbonization holding time is 1-10h; the carbonization is carried out under the protection of an inert gas, which is nitrogen or argon, and the gas flow rate is controlled at 10-50L / min.
[0058] In step A of the preparation method of this invention, the carbonized material is etched using a strongly acidic solution containing metal ions. The strongly acidic solution is at least one of sulfuric acid, nitric acid, hydrofluoric acid, and hydrochloric acid, with a hydrogen ion concentration of 1–10 mol / L. The metal ions in the strongly acidic solution are Ag. + Mg 2+ Al 3+ At least one of the following (the metal ion is added via a metal ion salt, wherein the anion in the metal ion salt matches the anion in the strong acid), the concentration of the metal ion in the strongly acidic solution containing the metal ion is 0.1–0.5 mol / L, Si@SiO x The mass ratio of the @C material to the volume ratio of the strongly acidic solution containing metal ions is 1g: 2.5~6mL.
[0059] Strong acid solution etches away SiO x During passivation, hollow interlayers are formed, which simultaneously chemically activates the hard carbon coating, increasing its channel count. After etching, Ag... + Mg 2+ Al 3+ Metal ions increase the electrical contact between the core and shell, improving conductivity and lithium ion insertion / extraction rate. The metal element produced by the reduction of metal ions with Si-H bonds on the silicon surface or water molecules in strong acid solution remains in the pores and hollow interlayers of the porous hard carbon coating.
[0060] In step B of the preparation method of the present invention, the graphite is artificial graphite or natural graphite, the mass ratio of the graphite to the silicon-carbon matrix is 1 to 1.5:1, and the median particle size of the graphite is 3 to 20 μm.
[0061] In step B of the preparation method of the present invention, solid-phase mixing is generally carried out in a fusion machine. The rotation speed of solid-phase mixing is 2000-3000 rpm, and the solid-phase mixing time is 10-60 min.
[0062] In step B of the preparation method of this invention, carbonization is carried out under the protection of an inert gas, which is nitrogen or argon. Before the carbonization reaction, the inert gas is first purged for 30-60 minutes, then the inert gas inlet rate is reduced, and a carbon precursor gas is introduced. The inert gas is nitrogen or argon, and the carbon precursor gas is at least one of methane, ethane, propane, ethylene, propylene, and acetylene. The flow rate of the carbon precursor gas is 2-10 L / min, and the inlet flow rate ratio of the inert gas to the carbon precursor gas is 1-10:99-90.
[0063] In step B of the preparation method of the present invention, the vapor deposition carbonization temperature is 700-1300℃, the heating rate is 2-15℃ / min, and after carbonization, the material is sieved through a 325-mesh sieve and the material passing through the sieve is taken to obtain the product.
[0064] Based on the aforementioned silicon-carbon anode material, the present invention also provides a lithium-ion battery anode, which is prepared from the aforementioned silicon-carbon anode material or the silicon-carbon anode material prepared by the aforementioned method; and the present invention also provides a lithium-ion battery, which uses the aforementioned anode as the anode.
[0065] The present invention will be further described in detail below through embodiments, but the scope of protection of the present invention is not limited to the embodiments described herein.
[0066] In this invention, the nano-silicon was purchased commercially, and its surface SiO₂ was used. x The thickness is about 2-3 nm; the inner walls of the reaction vessel and fusion machine used in the experiment were coated with tungsten carbide.
[0067] Example 1
[0068] Step A: Add 100g of sucrose and 2kg of anhydrous ethanol to a reaction vessel. Disperse 500g of nano-silicon with a median particle size of 80nm in the mixture. Set the temperature to 85℃, stir, mix, and dry. The stirring speed of the reaction vessel is 200rpm. Collect the solvent using a solvent recovery device. Dry the obtained material in an 80℃ constant temperature oven for 12h, then transfer it to an argon-protected box-type carbonization furnace for calcination. The gas flow rate is 15L / min, the heating rate is 5℃ / min, the carbonization temperature is 800℃, and the holding time is 1h. After completion, allow it to cool naturally to obtain Si@SiO. x @C material. Take 400g Si@SiO x @C material was placed in a mixed solution of 1L 0.1mol / L AgNO3 and 5mol / L HNO3, sonicated at 40℃ for 2h, washed 3-5 times with deionized water, and then dried in an oven at 80℃ for 12h to obtain a silicon-carbon matrix.
[0069] Step B: Take 400g of silicon-carbon matrix and 400g of artificial graphite with a median particle size of 8um obtained in Step A and put them into a fusion machine for solid-phase mixing at a speed of 2500rpm for 10min. Then, transfer the produced material into a CVD deposition furnace, purge with argon gas (15L / min) for 40min, reduce the argon gas inlet rate to 55mL / min, the acetylene gas inlet rate to 5L / min, the heating rate to 5℃ / min, the carbonization coating temperature to 1200℃, and the holding time to 1h. After the process, allow it to cool naturally and sieve it through a 325-mesh sieve to obtain the final Si@void@C / Gr@C anode active material.
[0070] Example 2
[0071] Step A: Add 100g of polyaniline and 2kg of acetone to a reactor. Disperse 500g of nano-silicon with a median particle size of 80nm in the reactor. Set the temperature to 85℃, stir, mix, and dry. The stirring speed of the reactor is 200rpm. Collect the solvent using a solvent recovery device. Dry the obtained material in an 80℃ constant temperature oven for 12 hours, then transfer it to an argon-protected box-type carbonization furnace for calcination. The gas flow rate is 15L / min, the heating rate is 5℃ / min, the carbonization temperature is 800℃, and the holding time is 1 hour. After completion, allow it to cool naturally to obtain Si@SiO. x @C material. Take 400g Si@SiO x @C material was placed in a mixed solution of 1L 0.1mol / L AgF and 5mol / L HF, sonicated at 40℃ for 2h, washed 3-5 times with deionized water, and then dried in an oven at 80℃ for 12h to obtain a silicon-carbon matrix.
[0072] Step B: Take 400g of silicon-carbon matrix and 400g of artificial graphite with a median particle size of 12um obtained in Step A, put them into a fusion machine for solid-phase mixing at 2500rpm for 10min. Then, transfer the produced material into a CVD deposition furnace, purge with argon gas (15L / min) for 40min, reduce the argon gas inlet rate to 50mL / min, the methane gas inlet rate to 4L / min, the heating rate to 5℃ / min, the carbonization coating temperature to 1200℃, and the holding time to 1h. After the process, allow it to cool naturally and sieve it through a 325-mesh screen to obtain the final Si@void@C / Gr@C anode active material.
[0073] Example 3
[0074] Step A: Add 50g of polystyrene and 2kg of acetone to a reactor. Disperse 500g of nano-silicon with a median particle size of 80nm in the reactor. Set the temperature to 85℃, stir, mix, and dry. The stirring speed of the reactor's agitator is 200rpm. Collect the solvent using a solvent recovery device. Dry the obtained material in an 80℃ constant temperature oven for 12 hours, then transfer it to an argon-protected box-type carbonization furnace for calcination. The gas flow rate is 15L / min, the heating rate is 5℃ / min, the carbonization temperature is 800℃, and the holding time is 1 hour. After completion, allow it to cool naturally to obtain Si@SiO. x @C material. Take 400g Si@SiO x The material was placed in a 1L mixed solution of 0.5mol / L MgCl3 and 3mol / L HCl, sonicated at 40℃ for 2 hours, washed 3-5 times with deionized water, and then dried in an 80℃ oven for 12 hours to obtain a silicon-carbon matrix.
[0075] Step B: Take 400g of silicon-carbon matrix and 500g of artificial graphite with a median particle size of 12um obtained in Step A, put them into a fusion machine for solid-phase mixing at 2500rpm for 10min. Then transfer the produced material into a CVD deposition furnace, purge with nitrogen gas (15L / min) for 40min, reduce the nitrogen gas inlet rate to 55mL / min, the ethane gas inlet rate to 5L / min, the heating rate to 5℃ / min, the carbonization temperature to 1000℃, and the holding time to 3h. After completion, allow it to cool naturally and sieve it through a 325-mesh sieve to obtain the final Si@void@C / Gr@C anode active material.
[0076] Example 4
[0077] Step A: Add 50g of polystyrene and 2kg of n-butanol to a reactor. Disperse 500g of nano-silicon with a median particle size of 100nm in the reactor. Set the temperature to 120℃, stir, mix, and dry. The stirring speed of the reactor is 200rpm. Collect the solvent using a solvent recovery device. Dry the obtained material in a 110℃ constant temperature oven for 12 hours, then transfer it to an argon-protected box-type carbonization furnace for calcination. The gas flow rate is 15L / min, the heating rate is 5℃ / min, the carbonization temperature is 700℃, and the holding time is 2 hours. After completion, allow it to cool naturally to obtain Si@SiO. x @C material. Take 400g Si@SiO x @C material was placed in a mixed solution of 1L 0.5mol / L AgCl3 and 3mol / L HCl, sonicated at 40℃ for 2h, washed 3-5 times with deionized water, and then dried in an oven at 80℃ for 12h to obtain a silicon-carbon matrix.
[0078] Step B: Take 400g of silicon-carbon matrix and 600g of artificial graphite with a median particle size of 18um obtained in Step A, put them into a fusion machine for solid-phase mixing at a speed of 2800rpm for 15min. Then, transfer the produced material into a CVD deposition furnace, purge with argon gas (15L / min) for 40min, reduce the argon gas inlet rate to 55mL / min, the acetylene gas inlet rate to 5L / min, the heating rate to 5℃ / min, the carbonization temperature to 1000℃, and the holding time to 3h. After completion, allow it to cool naturally and sieve it through a 325-mesh sieve to obtain the final Si@void@C / Gr@C anode active material.
[0079] Comparative Example 1
[0080] Step A: Add 100g of sucrose and 2kg of anhydrous ethanol to a reaction vessel. Disperse 500g of nano-silicon with a median particle size of 80nm in the mixture. Set the temperature to 85℃, stir, mix, and dry. The stirring speed of the reaction vessel is 200rpm. Collect the solvent using a solvent recovery device. Dry the obtained material in an 80℃ constant temperature oven for 12h, then transfer it to an argon-protected box-type carbonization furnace for calcination. The gas flow rate is 15L / min, the heating rate is 5℃ / min, the carbonization temperature is 800℃, and the holding time is 1h. After completion, allow it to cool naturally to obtain Si@SiO. x @C material.
[0081] Step B: Take the Si@SiO obtained in Step A x 400g of Si@SiO3 material and 400g of artificial graphite with a median particle size of 8µm were placed in a fusion machine for solid-phase mixing at 2500 rpm for 10 minutes. The resulting material was then transferred to a CVD deposition furnace, where argon gas was introduced for venting at a flow rate of 15 L / min, a heating rate of 5℃ / min, a carbonization temperature of 1200℃, and a holding time of 1 hour. After the carbonization process, the material was allowed to cool naturally and then sieved through a 325-mesh sieve to obtain the final Si@SiO3. x @C / Gr@C negative electrode active material.
[0082] Comparative Example 2
[0083] Step A: Add 2 kg of acetone to a reactor, disperse 500 g of nano-silicon with a median particle size of 80 nm in it, set the temperature to 85 °C, stir and dry, and maintain the stirring speed of the reactor at 200 rpm. Collect the solvent using a solvent recovery device. Dry the obtained material in an 80 °C constant temperature oven for 12 hours, then transfer it to an argon-protected box-type carbonization furnace for calcination. The gas flow rate is 15 L / min, the heating rate is 5 °C / min, the carbonization temperature is 800 °C, and the holding time is 1 hour. After completion, allow it to cool naturally to obtain Si@SiO. x Materials. Take 400g of Si@SiO xThe material was placed in a mixed solution of 1L 0.1mol / L AgF and 5mol / L HF, sonicated at 40℃ for 2 hours, washed 3-5 times with deionized water, and then dried in an 80℃ oven for 12 hours for later use.
[0084] Step B: Take 400g of the material obtained in Step A and 400g of artificial graphite with a median particle size of 12um, put them into a fusion machine for solid-phase mixing at a speed of 2500rpm for 10min. Then, transfer the produced material into a CVD deposition furnace, purge with argon gas (15L / min) for 40min, reduce the argon gas inlet rate to 50mL / min, the methane gas inlet rate to 4L / min, the heating rate to 5℃ / min, the carbonization coating temperature to 1200℃, and the holding time to 1h. After the process, allow it to cool naturally and sieve it through a 325-mesh screen to obtain the final Si@void / Gr@C anode active material.
[0085] Electrochemical performance testing: The multilayer core-shell structure silicon-carbon anode active material prepared through the above implementation case was used to make anode sheets with an active material: carbon black: binder ratio of 8:1:1. The anode sheets were then assembled into half-cells to test their electrochemical performance.
[0086] Table 1. Electrochemical and material physical properties of the examples and comparative products.
[0087]
[0088] As can be seen from the above cases, after etching and creating pores in the silicon-carbon matrix and introducing a multilayer coating process, the specific surface area and median particle size of the finished particles are slightly increased, but the first charge-discharge efficiency and capacity retention are greatly improved. This indicates that the material structure design of this application suppresses the volume expansion of the lithium intercalation of nano-silicon particles and hinders the direct contact between the electrolyte and silicon, effectively improving the first coulombic efficiency and cycle capacity retention of the finished product.
[0089] The embodiments of the present invention have been described above. However, the present invention is not limited to the above embodiments. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing silicon-carbon anode material for lithium-ion batteries, characterized in that: Includes the following steps: A. Preparation of silicon-carbon matrix: nano-silicon, hard carbon precursor material and organic solvent are mixed, heated and stirred to remove the organic solvent, dried, and the powder is collected; the powder is carbonized under the protection of inert atmosphere to obtain Si@SiO x @C material; the Si@SiO x @C material is added to a strong acidic solution containing metal ions, ultrasonic treatment, washing and drying to obtain a silicon-carbon matrix; B. The silicon-carbon matrix obtained in step A is mixed with graphite in a solid phase. The resulting material is coated and carbonized under a mixed atmosphere of inert atmosphere and carbon precursor gas. After cooling, it is sieved to obtain Si@void@C / Gr@C composite material, which is the silicon-carbon anode material for lithium-ion batteries. In step A, the median particle size of the nanosilicon is 40-150 nm, and the surface has SiO x passivation layer, 1 < x < 2; In step A, the hard carbon precursor material is at least one of polyaniline, polypyrrole, polystyrene, polyacrylonitrile, polyimide, polyvinylidene chloride, sucrose, glucose, and phenolic resin. In step A, the mass ratio of the organic solvent to the hard carbon precursor material is 10~40:1; In step A, the mass ratio of the nano-silicon to the hard carbon precursor material is 5~10:1~2; In step A, the strongly acidic solution is hydrofluoric acid, and the hydrogen ion concentration in the solution is 1~10 mol / L; In step A, the metal ion in the strongly acidic solution containing metal ions is Ag. + ; In step A, the concentration of metal ions in the strongly acidic solution containing metal ions is 0.1~0.5 mol / L; In step A, the Si@SiO x The mass ratio of the C material to the volume of the strongly acidic solution containing metal ions is 1 g: 2.5~6 mL; The lithium-ion battery silicon-carbon anode material has a silicon-carbon matrix and graphite as the core, and a vapor-deposited carbon coating layer as the shell, forming an outer core-shell structure. The silicon-carbon matrix has nano-silicon as the core and a porous hard carbon coating layer as the shell, with channels in the porous hard carbon coating layer and hollow interlayers between the nano-silicon and the porous hard carbon coating layer, forming an inner core-double-shell structure. The channels and hollow interlayers of the porous hard carbon coating layer contain a metallic element, which is Ag.
2. The method for preparing silicon-carbon anode material for lithium-ion batteries according to claim 1, characterized in that: At least one of the following must be met: The thickness of the vapor-deposited carbon coating layer is 10~30 nm; The porous hard carbon coating layer has micropores as its main structure, with a pore size of less than 2 nm. The thickness of the hollow interlayer is 1~5nm.
3. The method for preparing the silicon-carbon anode material for lithium-ion batteries according to claim 1, characterized in that: In step A, at least one of the following conditions must be met: The organic solvent is at least one selected from methanol, ethanol, ethylene glycol, propanol, isopropanol, n-butanol, acetone, toluene, and xylene. The thickness of the passivation layer is 1~5nm.
4. The method for preparing the silicon-carbon anode material for lithium-ion batteries according to claim 1, characterized in that: In step A, at least one of the following conditions must be met: The temperature for heating and stirring to remove organic solvents is 50~200℃; The time for removing organic solvents by heating and stirring is 3~12 hours; The rotation speed for heating and stirring to remove organic solvents is 100~1000 rpm; The drying temperature is 50~200℃; The drying time is 3-12 hours; The carbonization temperature is 700~1300℃, and the heating rate is 2~15℃ / min; The carbonization holding time is 1~10h; The inert atmosphere is nitrogen or argon, and the gas flow rate is 10~50 L / min.
5. The method for preparing the silicon-carbon anode material for lithium-ion batteries according to claim 1, characterized in that: In step B, at least one of the following must be satisfied: The graphite is either artificial or natural graphite. The mass ratio of graphite to silicon-carbon matrix is 1~1.5:1; The median particle size of the graphite is 3~20μm; The inert atmosphere is nitrogen or argon; The carbon precursor gas is at least one of methane, ethane, propane, ethylene, propylene, and acetylene. The flow rate of the carbon precursor gas is 2~10 L / min; The inert atmosphere to carbon precursor gas inlet flow rate ratio is 1~10:99~90.
6. The method for preparing the silicon-carbon anode material for lithium-ion batteries according to claim 1, characterized in that: In step B, at least one of the following must be satisfied: The rotational speed for solid-phase mixing is 2000~3000 rpm; The solid-phase mixing time is 10~60 min; The vapor deposition carbonization temperature is 700~1300℃, and the heating rate is 2~15℃ / min; The sieving process involves passing the material through a 325-mesh sieve and collecting the material that passes through the sieve.
7. A negative electrode for a lithium-ion battery, characterized in that, The silicon-carbon anode material is prepared by the method for preparing the silicon-carbon anode material for lithium-ion batteries according to any one of claims 1 to 6.
8. A lithium-ion battery, characterized in that, The lithium-ion battery negative electrode as described in claim 7 is used as the negative electrode.
Citation Information
Patent Citations
Silicon-carbon composite material and preparation method thereof and application thereof in lithium ion battery
CN106159213A
Porous silicon composite powder embedded with metal nanoparticles
CN112952068A
Lithium ion battery silicon-carbon negative electrode material and preparation method thereof
CN113964307A