A bias-resistant iron-poor manganese-zinc ferrite material and a preparation method thereof

By adjusting the proportion of the main component and the auxiliary component of the iron-poor manganese-zinc ferrite material, combined with the sintering process, the problem of inductance drop after the material is DC biased is solved, and the inductor bias drop is reduced and the application frequency is increased.

CN116891376BActive Publication Date: 2024-10-25GUANGDONG ZHAOQING MAGSOURCE ELECTRONIC CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310984434.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-07
Publication Date
2024-10-25
Estimated Expiration
2043-08-07

AI Technical Summary

Technical Problem

The inductance of existing iron-poor manganese-zinc ferrite materials drops by more than 50% after DC bias and cannot recover on its own, which limits its application and promotion.

Method used

By adjusting the proportion of the main component and auxiliary component of the material, including the combination of Fe2O3, Mn3O4, ZnO and cobalt oxide, doping SiO2, CaCO3, V2O5, Nb2O5, Bi2O3, MoO3 and other oxides, and using a specific preparation method for sintering, Improve the material's anti-offset shedding properties.

Benefits of technology

It achieves an inductor bias reduction of ≤15%, increases the application frequency of the material, and has a higher Bs than nickel-zinc materials with the same magnetic permeability, overcoming the problem of inductance drop.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004380562850000111
    Figure BDA0004380562850000111
Patent Text Reader

Abstract

The present invention relates to an anti-bias drop iron-poor manganese-zinc ferrite material and a preparation method thereof. The ferrite material comprises a main component and an auxiliary component, wherein the main component is 48-49 mol% of Fe2O3, 39-45 mol% of Mn3O4 and 7-12 mol% of ZnO in terms of MnO; and the auxiliary component is 100 mol% of Co based on the total weight of the main component. x wt% cobalt oxide and at least three selected from SiO2, CaCO3, V2O5, Nb2O5, Bi2O3, MoO3, wherein x The value range is the mol% value of MnO in the main component divided by (35±4); the iron-poor manganese-zinc ferrite material with resistance to bias drop of the present invention can effectively reduce the inductance drop of the anti-EMI magnetic core caused by bias.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of soft magnetic ferrite materials, and in particular to an anti-bias drop iron-poor manganese-zinc ferrite material and a preparation method thereof. Background Art

[0002] Today's society is developing from the Internet era to the Internet of Things era. If the Internet takes people as the objects of connection and service, then the Internet of Things expands the objects of information network connection and service from people to objects to realize "Internet of Everything". The ubiquitous information network connection makes the space we live in more and more electromagnetic interference. The effective way to solve or reduce electromagnetic pollution and improve the anti-electromagnetic interference ability of electronic equipment is to adopt electromagnetic compatibility design, which requires a large number of anti-EMI materials.

[0003] Commonly used anti-EMI materials include iron-rich manganese-zinc ferrites for use below 10MHz and nickel-zinc ferrites for use above 10MHz. In recent years, based on production compatibility and cost reduction considerations, iron-poor manganese-zinc ferrite materials that can be used above 10MHz have achieved certain development. Chinese patents (Jiangfen Magnetic Material CN101857426A, Jiangmen Anci CN111138179A, CN111138180A, CN111138181A, Dongci CN110156451A, Chunguang CN112142457A, Baosteel CN110824395A, Tianyuan CN110845228A, Tianming CN101805173A) have successively disclosed iron-poor manganese-zinc ferrite materials with a magnetic permeability of 650 to 4000, which greatly expanded the operating frequency range of manganese-zinc ferrite materials and partially replaced the application field of nickel-zinc ferrite. However, a problem was also found in the application. After the poor iron manganese zinc ferrite core was subjected to DC bias or equivalent operation, the inductance dropped by more than 50% and could not recover by itself. It must be treated with magnetic neutralization before it can be used again. However, it is impractical to add a magnetic neutralization device in the actual application scenario, which greatly limits the application and promotion of poor iron manganese zinc ferrite materials.

[0004] Therefore, it is urgent to find a new type of bias-resistant iron-poor manganese-zinc ferrite material and a preparation method thereof to overcome the problems existing in the prior art. Summary of the invention

[0005] In order to overcome the problem that the inductance of the existing poor iron manganese zinc ferrite cannot recover by itself due to the inductance drop after DC bias, the present invention provides a bias drop-resistant poor iron manganese zinc ferrite material and a preparation method thereof.

[0006] One object of the present invention is to provide a bias-resistant low-iron manganese-zinc ferrite material characterized in that: the ferrite material comprises a main component and an auxiliary component, the main component is 48-49 mol% of Fe 2 O 3 , 39-45 mol% Mn based on MnO 3 O 4 and 7 to 12 mol% ZnO; and the auxiliary component is xwt% cobalt oxide based on the total weight of the main component as Co, wherein the value range of x is the mol% value of MnO in the main component divided by (35±4).

[0007] The ferrite material is also doped with SiO 2 、CaCO 3 、V 2 O 5 , Nb 2 O 5 、Bi 2 O 3 、MoO 3 At least three of the above, based on the total weight of the main components, SiO 2 40~100ppm, CaCO 3 200~800ppm, V 2 O 5 0~300ppm, Nb 2 O 5 50~400ppm, Bi 2 O 3 0~500ppm, MoO 3 0~500ppm.

[0008] Furthermore, the cobalt oxide may be Co 3 O 4 、Co 2 O 3 Or CoO or any one of them or a mixture thereof. If it is a mixture, the Co content thereof needs to be tested in advance.

[0009] Furthermore, the cobalt oxide is Co 3 O 4 The effect is best. Because Co 3 O 4 It has a cubic spinel structure and is easier to undergo solid solution diffusion reaction with spinel-structured manganese-zinc ferrite.

[0010] Another object of the present invention is to provide a method for preparing the above-mentioned ferrite material, characterized in that it comprises the following steps:

[0011] 1) Ingredients: weigh the main ingredients according to the designed components;

[0012] 2) Mixing: put the main ingredients into a sand mill or a ball mill and mix them thoroughly to obtain a powder;

[0013] 3) Pre-burning: pre-burn the obtained powder at a temperature of 850-950°C for 1-3 hours, and then cool down naturally to obtain the pre-burned material;

[0014] 4) Second grinding: adding auxiliary components to the above-mentioned pre-sintered material, and performing a second grinding to obtain a slurry with an average particle size of about 1 μm;

[0015] 5) Granulation: Based on the total weight of the powder of the slurry obtained in step 4), 8 to 10 wt% of an aqueous solution of polyvinyl alcohol with a concentration of 8 to 10 wt% is added thereto, and the mixture is uniformly mixed and granulated to obtain a granular material for molding;

[0016] 6) Molding: adding a polyvinyl alcohol aqueous solution with a concentration of 0.1-0.5 wt% to the granules obtained in step 5) to make the moisture content of the powder reach 0.15-0.45 wt%, and adding 0.1-0.5 wt% of zinc stearate based on the total weight of the obtained water-containing powder to mix the materials, and pressing and molding into a green product;

[0017] 7) Sintering: the sintering temperature is 1260-1340°C, the heat preservation time is 4-8 hours, and the manganese-zinc ferrite material is obtained after cooling out of the furnace.

[0018] Furthermore, in step 6), the density of the pressed green body is 3.0±0.2 g / cm 3 .

[0019] Furthermore, in step 7), air sintering is used from room temperature to high temperature, and a small amount of nitrogen is used to protect the cooling in the cooling stage. The equilibrium oxygen partial pressure in the cooling stage is calculated according to the formula lg(P(O 2 ))=ab / T, where a is 5-8, b is 11000-15000, and T is the absolute temperature.

[0020] The beneficial effects of the present invention are:

[0021] The inductance of the existing poor iron manganese zinc ferrite cores on the market drops by more than 50% after being subjected to DC bias, and cannot recover on their own. Based on theoretical guidance and combined with a large number of experimental studies, the present invention finds that the anti-bias drop characteristics of the poor iron manganese zinc ferrite material have a certain correlation with the Br / Bs ratio (i.e., the residual magnetism ratio), and the residual magnetism ratio has a certain correlation with the relative proportion of the MnO content and the Co doping amount in the main components of the poor iron manganese zinc ferrite material. Due to the inertial operation of the high-permeability manganese zinc ferrite material, the value of Br was not paid special attention to in the early development process of the poor iron manganese zinc ferrite material, and the important parameter of the residual magnetism ratio was ignored, resulting in the problem that the poor iron manganese zinc ferrite material had a bias drop of more than 50% and could not recover on its own after it was put on the market. The poor iron manganese zinc ferrite material obtained under the composition and preparation method of the present invention can overcome this problem, and the material has Tc ≥ 160°C, Bs ≥ 470mT, μ i =1000~2000, Br / Bs≤0.2, and the bias drop of inductance ≤15%. The application frequency of this iron-poor 1.5K material can be higher than that of 3K material, and higher than the Bs of nickel-zinc material with the same magnetic permeability. DETAILED DESCRIPTION

[0022] In order to better understand the present invention, the present invention is further described below in conjunction with the examples. However, the scope of protection claimed by the present invention is not limited to the scope involved in the examples of the present invention. Unless otherwise mentioned, the ingredients and test methods mentioned in the examples disclosed in this patent are conventional methods known to those skilled in the art.

[0023] In order to better understand the present invention, the present invention is further described below in conjunction with the examples. However, the scope of protection claimed by the present invention is not limited to the scope involved in the examples of the present invention. Unless otherwise mentioned, the ingredients and test methods mentioned in the examples disclosed in this patent are conventional methods known to those skilled in the art.

[0024] Example 1

[0025] 1) Ingredients: According to the design composition: 48.0 mol% Fe 2 O 3 , 45.0 mol% Mn based on MnO 3 O 4 and 7.0 mol% ZnO, weighing the main components;

[0026] 2) Mixing: put the main ingredients into a sand mill or a ball mill and mix for 30 minutes to obtain a powder;

[0027] 3) Pre-burning: pre-burn the obtained powder at a temperature of 850°C for 3 hours, and then cool naturally to obtain the pre-burned material;

[0028] 4) Second grinding: Add auxiliary components to the above pre-sintered material: 1.40wt% Co 2 O 3 , 40ppm SiO 2 , 200ppm CaCO 3 , 50ppm Nb 2 O 5 、300ppm Bi 2 O 3 , 400ppm MoO 3 , grinding for the second time to an average particle size of 0.9 μm to obtain a slurry;

[0029] 5) Granulation: Based on the total weight of the powder of the slurry obtained in step 4), 8 wt% of a 10 wt% aqueous solution of polyvinyl alcohol is added thereto, and the mixture is uniformly mixed and granulated to obtain granules for molding;

[0030] 6) Molding: Add a 0.1 wt% polyvinyl alcohol aqueous solution to the granules obtained in step 5) to make the moisture content of the powder reach 0.35 wt%, and add 0.5 wt% zinc stearate based on the total weight of the obtained water-containing powder to mix the materials, and press to form a green compact with a density of 2.8 g / cm 3 Green products;

[0031] 7) Sintering: The sintering temperature is 1340℃, the holding time is 4 hours, and air sintering is used from room temperature to high temperature. A small amount of nitrogen is used to protect the cooling in the cooling stage. The equilibrium oxygen partial pressure in the cooling stage is calculated according to the formula lg(P(O 2 ))=ab / T, where a is 7.8, b is 14540, and T is absolute temperature. The material is cooled and taken out of the furnace to obtain manganese-zinc ferrite material.

[0032] 8) Test: HP4284A LCR tester is used to measure the room temperature inductance L of the sample magnetic ring under the conditions of 10kHz and 0.25V. 0 , calculate the initial magnetic permeability μ of the material i ; Use SY-8258 BH tester to test Bs and Br of sample magnetic ring at 50Hz, 1200A / m, 25℃, and calculate the remanence ratio Br / Bs; Use HP4284A and HP42841A DC bias source to test the sample magnetic ring at 30A / m DC bias, without magnetic neutralization treatment, and then measure the room temperature inductance L of the sample magnetic ring at 10kHz and 0.25mT. 1 , calculate the bias reduction ratio D L =(L 0 -L 1 ) / L 0 .

[0033] Measured results: μi =1017,Br / Bs=0.19,D L =14%, bias reduction ratio D L Significantly less than 50%.

[0034] Example 2

[0035] 1) Ingredients: According to the design composition: 48.1 mol% Fe 2 O 3 , 44.4 mol% Mn based on MnO 3 O 4 and 7.5 mol% ZnO, weighing the main components;

[0036] 2) Mixing: put the main ingredients into a sand mill or a ball mill and mix for 35 minutes to obtain a powder;

[0037] 3) Pre-burning: pre-burn the obtained powder at a temperature of 950°C for 1 hour, and then cool naturally to obtain the pre-burned material;

[0038] 4) Second grinding: Add auxiliary components to the above pre-sintered material: 1.37wt% Co 2 O 3 +Co 3 O 4 Mixture, 40ppm SiO 2 , 200ppm CaCO 3 , 50ppm Nb 2 O 5 , 400ppm MoO 3 , grinding for the second time to an average particle size of 0.92 μm to obtain a slurry;

[0039] 5) Granulation: Based on the total weight of the powder of the slurry obtained in step 4), add 9 wt % of a 10 wt % polyvinyl alcohol aqueous solution thereto, mix evenly and granulate to obtain granules for molding;

[0040] 6) Molding: Add a 0.2 wt% polyvinyl alcohol aqueous solution to the granules obtained in step 5) to make the moisture content of the powder reach 0.42 wt%, and add 0.3 wt% zinc stearate based on the total weight of the obtained water-containing powder to mix the materials, and press to form a green compact with a density of 2.9 g / cm 3 Green products;

[0041] 7) Sintering: The sintering temperature is 1330℃, the holding time is 5 hours, and air sintering is used from room temperature to high temperature. A small amount of nitrogen is used to protect the cooling in the cooling stage. The equilibrium oxygen partial pressure in the cooling stage is calculated according to the formula lg(P(O 2))=ab / T, where a is 6.75, b is 13000, and T is absolute temperature. The material is cooled and taken out of the furnace to obtain manganese-zinc ferrite material.

[0042] 8) Test: HP4284A LCR tester is used to measure the room temperature inductance L of the sample magnetic ring under the conditions of 10kHz and 0.25V. 0 , calculate the initial magnetic permeability μ of the material i ; Use SY-8258 BH tester to test Bs and Br of sample magnetic ring at 50Hz, 1200A / m, 25℃, and calculate the remanence ratio Br / Bs; Use HP4284A and HP42841A DC bias source to test the sample magnetic ring at 30A / m DC bias, without magnetic neutralization treatment, and then measure the room temperature inductance L of the sample magnetic ring at 10kHz and 0.25mT. 1 , calculate the bias reduction ratio D L =(L 0 -L 1 ) / L 0 .

[0043] Measured results: μ i =1190, Br / Bs=0.19, D L =10%, bias reduction ratio D L Significantly less than 50%.

[0044] Example 3

[0045] 1) Ingredients: According to the design composition: 48.2 mol% Fe 2 O 3 , 43.8 mol% Mn based on MnO 3 O 4 and 8.0 mol% ZnO, weighing the main components;

[0046] 2) Mixing: put the main ingredients into a sand mill or a ball mill and mix for 40 minutes to obtain a powder;

[0047] 3) Pre-burning: pre-burn the obtained powder at a temperature of 880°C for 2.5 hours, and then cool naturally to obtain the pre-burned material;

[0048] 4) Second grinding: Add auxiliary components to the above pre-sintered material: 1.34wt% CoO, 40ppm SiO 2 , 200ppm CaCO 3 , 50ppm Nb 2 O 5 、300ppm Bi 2 O 3, grinding for the second time to an average particle size of 0.93 μm to obtain a slurry;

[0049] 5) Granulation: Based on the total weight of the powder of the slurry obtained in step 4), 10 wt% of a 9 wt% aqueous solution of polyvinyl alcohol is added thereto, and the mixture is mixed and granulated to obtain granules for molding;

[0050] 6) Molding: Add 0.5 wt% polyvinyl alcohol aqueous solution to the granules obtained in step 5) to make the moisture content of the powder reach 0.37 wt%, and add 0.3 wt% zinc stearate based on the total weight of the obtained water-containing powder to mix the materials, and press to form a green compact with a density of 3.0 g / cm 3 Green products;

[0051] 7) Sintering: The sintering temperature is 1310℃, the holding time is 6 hours, and air sintering is used from room temperature to high temperature. A small amount of nitrogen is used to protect the cooling in the cooling stage. The equilibrium oxygen partial pressure in the cooling stage is calculated according to the formula lg(P(O 2 ))=ab / T, where a is 6.05, b is 12000, and T is absolute temperature. The material is cooled and taken out of the furnace to obtain manganese-zinc ferrite material.

[0052] 8) Test: HP4284A LCR tester is used to measure the room temperature inductance L of the sample magnetic ring under the conditions of 10kHz and 0.25V. 0 , calculate the initial magnetic permeability μ of the material i ; Use SY-8258 BH tester to test Bs and Br of sample magnetic ring at 50Hz, 1200A / m, 25℃, and calculate the remanence ratio Br / Bs; Use HP4284A and HP42841A DC bias source to test the sample magnetic ring at 30A / m DC bias, without magnetic neutralization treatment, and then measure the room temperature inductance L of the sample magnetic ring at 10kHz and 0.25mT. 1 , calculate the bias reduction ratio D L =(L 0 -L 1 ) / L 0 .

[0053] Measured results: μ i =1312, Br / Bs=0.19, D L =6%, bias reduction ratio D L Significantly less than 50%.

[0054] Example 4

[0055] 1) Ingredients: According to the design composition: 48.3 mol% Fe 2 O 3 , 43.2 mol% Mn based on MnO 3O 4 and 8.5 mol% ZnO, weighing the main components;

[0056] 2) Mixing: put the main ingredients into a sand mill or a ball mill and mix for 30 minutes to obtain a powder;

[0057] 3) Pre-burning: pre-burn the obtained powder at a temperature of 860°C for 2.5 hours, and then cool down naturally to obtain the pre-burned material;

[0058] 4) Second grinding: Add auxiliary components to the above pre-sintered material: 1.29wt% Co 3 O 4 , 40ppm SiO 2 , 200ppm CaCO 3 , 200ppm V 2 O 5 , 100ppm Nb 2 O 5 , grinding for the second time to an average particle size of 0.97 μm to obtain a slurry;

[0059] 5) Granulation: Based on the total weight of the powder of the slurry obtained in step 4), 10 wt% of a 10 wt% aqueous solution of polyvinyl alcohol is added thereto, and the mixture is uniformly mixed and granulated to obtain granules for molding;

[0060] 6) Molding: Add a 0.5 wt% polyvinyl alcohol aqueous solution to the granules obtained in step 5) to make the moisture content of the powder reach 0.15 wt%, and add 0.5 wt% zinc stearate based on the total weight of the obtained water-containing powder to mix the materials, and press to form a green compact with a density of 3.1 g / cm 3 Green products;

[0061] 7) Sintering: The sintering temperature is 1300℃, the holding time is 6 hours, and air sintering is used from room temperature to high temperature. A small amount of nitrogen is used to protect the cooling in the cooling stage. The equilibrium oxygen partial pressure in the cooling stage is calculated according to the formula lg(P(O 2 ))=ab / T, where a is 6.75, b is 13000, and T is absolute temperature. The material is cooled and taken out of the furnace to obtain manganese-zinc ferrite material.

[0062] 8) Test: HP4284A LCR tester is used to measure the room temperature inductance L of the sample magnetic ring under the conditions of 10kHz and 0.25V. 0 , calculate the initial magnetic permeability μ of the material i; Use SY-8258 BH tester to test Bs and Br of sample magnetic ring at 50Hz, 1200A / m, 25℃, and calculate the remanence ratio Br / Bs; Use HP4284A and HP42841A DC bias source to test the sample magnetic ring at 30A / m DC bias, without magnetic neutralization treatment, and then measure the room temperature inductance L of the sample magnetic ring at 10kHz and 0.25mT. 1 , calculate the bias reduction ratio D L =(L 0 -L 1 ) / L 0 .

[0063] Measured results: μ i =1448,Br / Bs=0.19,D L =2%, bias reduction ratio D L Significantly less than 50%.

[0064] Example 5

[0065] 1) Ingredients: According to the design composition: 48.4 mol% Fe 2 O 3 , 42.6 mol% Mn based on MnO 3 O 4 and 9.0 mol% ZnO, weighing the main components;

[0066] 2) Mixing: put the main ingredients into a sand mill or a ball mill and mix for 30 minutes to obtain a powder;

[0067] 3) Pre-burning: pre-burn the obtained powder at a temperature of 920°C for 2 hours, and then cool down naturally to obtain the pre-burned material;

[0068] 4) Second grinding: Add auxiliary components to the above pre-sintered material: 1.25wt% Co 3 O 4 , 40ppm SiO 2 , 200ppm CaCO 3 , 50ppm Nb 2 O 5 , grinding for the second time to an average particle size of 0.89 μm to obtain a slurry;

[0069] 5) Granulation: Based on the total weight of the powder of the slurry obtained in step 4), 10 wt% of a 9 wt% aqueous solution of polyvinyl alcohol is added thereto, and the mixture is uniformly mixed and granulated to obtain a granular material for molding;

[0070] 6) Molding: Add a 0.3 wt% polyvinyl alcohol aqueous solution to the granules obtained in step 5) to make the moisture content of the powder reach 0.35 wt%, and add 0.4 wt% zinc stearate based on the total weight of the obtained water-containing powder to mix the materials, and press to form a green compact with a density of 3.0 g / cm 3 Green products;

[0071] 7) Sintering: The sintering temperature is 1280℃, the holding time is 7 hours, and air sintering is used from room temperature to high temperature. A small amount of nitrogen is used to protect the cooling in the cooling stage. The equilibrium oxygen partial pressure in the cooling stage is calculated according to the formula lg(P(O 2 ))=ab / T, where a is 6.75, b is 13000, and T is absolute temperature. The material is cooled and taken out of the furnace to obtain manganese-zinc ferrite material.

[0072] 8) Test: HP4284A LCR tester is used to measure the room temperature inductance L of the sample magnetic ring under the conditions of 10kHz and 0.25V. 0 , calculate the initial magnetic permeability μ of the material i ; Use SY-8258 BH tester to test Bs and Br of sample magnetic ring at 50Hz, 1200A / m, 25℃, and calculate the remanence ratio Br / Bs; Use HP4284A and HP42841A DC bias source to test the sample magnetic ring at 30A / m DC bias, without magnetic neutralization treatment, and then measure the room temperature inductance L of the sample magnetic ring at 10kHz and 0.25mT. 1 , calculate the bias reduction ratio D L =(L 0 -L 1 ) / L 0 .

[0073] Measured results: μ i =1504,Br / Bs=0.18,D L =1%, bias reduction ratio D L Significantly less than 50%.

[0074] Example 6

[0075] 1) Ingredients: According to the design composition: 48.5 mol% Fe 2 O 3 , 42.0 mol% Mn based on MnO 3 O 4 and 9.5 mol% ZnO, weighing the main components;

[0076] 2) Mixing: put the main ingredients into a sand mill or a ball mill and mix for 30 minutes to obtain a powder;

[0077] 3) Pre-burning: pre-burn the obtained powder at a temperature of 870°C for 2 hours, and then cool down naturally to obtain the pre-burned material;

[0078] 4) Second grinding: Add auxiliary components to the above pre-sintered material: 1.20wt% Co 3 O 4 , 50ppm SiO 2 , 200ppm CaCO 3 , 50ppm Nb 2 O 5 , grinding for the second time to an average particle size of 0.96 μm to obtain a slurry;

[0079] 5) Granulation: Based on the total weight of the powder of the slurry obtained in step 4), 10 wt% of a 10 wt% aqueous solution of polyvinyl alcohol is added thereto, and the mixture is uniformly mixed and granulated to obtain granules for molding;

[0080] 6) Molding: Add a 0.1 wt% polyvinyl alcohol aqueous solution to the granules obtained in step 5) to make the moisture content of the powder reach 0.45 wt%, and add 0.5 wt% zinc stearate based on the total weight of the obtained water-containing powder to mix the materials, and press to form a green compact with a density of 3.1 g / cm 3 Green products;

[0081] 7) Sintering: The sintering temperature is 1290℃, the holding time is 7 hours, and air sintering is used from room temperature to high temperature. A small amount of nitrogen is used to protect the cooling in the cooling stage. The equilibrium oxygen partial pressure in the cooling stage is calculated according to the formula lg(P(O 2 ))=ab / T, where a is 6.55, b is 13000, and T is absolute temperature. The material is cooled and taken out of the furnace to obtain manganese-zinc ferrite material.

[0082] 8) Test: HP4284A LCR tester is used to measure the room temperature inductance L of the sample magnetic ring under the conditions of 10kHz and 0.25V. 0 , calculate the initial magnetic permeability μ of the material i ; Use SY-8258 BH tester to test Bs and Br of sample magnetic ring at 50Hz, 1200A / m, 25℃, and calculate the remanence ratio Br / Bs; Use HP4284A and HP42841A DC bias source to test the sample magnetic ring at 30A / m DC bias, without magnetic neutralization treatment, and then measure the room temperature inductance L of the sample magnetic ring at 10kHz and 0.25mT. 1 , calculate the bias reduction ratio D L =(L 0 -L 1 ) / L 0 .

[0083] Measured results: μ i =1575,Br / Bs=0.18,D L <1%, bias reduction ratio D L Significantly less than 50%.

[0084] Example 7

[0085] 1) Ingredients: According to the design composition: 48.6 mol% Fe 2 O 3 , 41.4 mol% Mn based on MnO 3 O 4 and 10.0 mol% ZnO, weighing the main components;

[0086] 2) Mixing: put the main ingredients into a sand mill or a ball mill and mix for 30 minutes to obtain a powder;

[0087] 3) Pre-burning: pre-burn the obtained powder at a temperature of 900°C for 2 hours, and then cool down naturally to obtain the pre-burned material;

[0088] 4) Second grinding: Add auxiliary components to the above pre-sintered material: 1.16wt% Co 3 O 4 , 80ppm SiO 2 , 300ppm CaCO 3 , 50ppm Nb 2 O 5 , grinding for the second time to an average particle size of 0.9 μm to obtain a slurry;

[0089] 5) Granulation: Based on the total weight of the powder of the slurry obtained in step 4), 10 wt% of a 10 wt% aqueous solution of polyvinyl alcohol is added thereto, and the mixture is uniformly mixed and granulated to obtain granules for molding;

[0090] 6) Molding: Add a 0.5 wt% polyvinyl alcohol aqueous solution to the granules obtained in step 5) to make the moisture content of the powder reach 0.35 wt%, and add 0.2 wt% zinc stearate based on the total weight of the obtained water-containing powder to mix the materials, and press to form a green compact with a density of 3.0 g / cm 3 Green products;

[0091] 7) Sintering: The sintering temperature is 1320℃, the holding time is 6 hours, and air sintering is used from room temperature to high temperature. A small amount of nitrogen is used to protect the cooling in the cooling stage. The equilibrium oxygen partial pressure in the cooling stage is calculated according to the formula lg(P(O 2 ))=ab / T, where a is 6.65, b is 13000, and T is absolute temperature. The material is cooled and taken out of the furnace to obtain the manganese-zinc ferrite material.

[0092] 8) Test: HP4284A LCR tester is used to measure the room temperature inductance L of the sample magnetic ring under the conditions of 10kHz and 0.25V. 0 , calculate the initial magnetic permeability μ of the material i ; Use SY-8258 BH tester to test Bs and Br of sample magnetic ring at 50Hz, 1200A / m, 25℃, and calculate the remanence ratio Br / Bs; Use HP4284A and HP42841A DC bias source to test the sample magnetic ring at 30A / m DC bias, without magnetic neutralization treatment, and then measure the room temperature inductance L of the sample magnetic ring at 10kHz and 0.25mT. 1 , calculate the bias reduction ratio D L =(L 0 -L 1 ) / L 0 .

[0093] Measured results: μ i =1653,Br / Bs=0.18,D L <1%, bias reduction ratio D L Significantly less than 50%.

[0094] Example 8

[0095] 1) Ingredients: According to the design composition: 48.7 mol% Fe 2 O 3 , 40.8 mol% Mn based on MnO 3 O 4 and 10.5 mol% ZnO, weighing the main components;

[0096] 2) Mixing: put the main ingredients into a sand mill or a ball mill and mix for 30 minutes to obtain a powder;

[0097] 3) Pre-burning: pre-burn the obtained powder at a temperature of 910°C for 2 hours, and then cool naturally to obtain the pre-burned material;

[0098] 4) Second grinding: Add auxiliary components to the above pre-sintered material: 1.13wt% Co 3 O 4 , 40ppm SiO 2 , 300ppm CaCO 3 , 100ppm Nb 2 O 5 , grinding for the second time to an average particle size of 0.91 μm to obtain a slurry;

[0099] 5) Granulation: Based on the total weight of the powder of the slurry obtained in step 4), 10 wt% of a 10 wt% aqueous solution of polyvinyl alcohol is added thereto, and the mixture is uniformly mixed and granulated to obtain granules for molding;

[0100] 6) Molding: Add a 0.3 wt% polyvinyl alcohol aqueous solution to the granules obtained in step 5) to make the moisture content of the powder reach 0.35 wt%, and add 0.3 wt% zinc stearate based on the total weight of the obtained water-containing powder to mix the materials, and press to form a green compact with a density of 3.1 g / cm 3 Green products;

[0101] 7) Sintering: The sintering temperature is 1310℃, the holding time is 7 hours, and air sintering is used from room temperature to high temperature. A small amount of nitrogen is used to protect the cooling in the cooling stage. The equilibrium oxygen partial pressure in the cooling stage is calculated according to the formula lg(P(O 2 ))=ab / T, where a is 6.55, b is 13000, and T is absolute temperature. The material is cooled and taken out of the furnace to obtain manganese-zinc ferrite material.

[0102] 8) Test: HP4284A LCR tester is used to measure the room temperature inductance L of the sample magnetic ring under the conditions of 10kHz and 0.25V. 0 , calculate the initial magnetic permeability μ of the material i ; Use SY-8258 BH tester to test Bs and Br of sample magnetic ring at 50Hz, 1200A / m, 25℃, and calculate the remanence ratio Br / Bs; Use HP4284A and HP42841A DC bias source to test the sample magnetic ring at 30A / m DC bias, without magnetic neutralization treatment, and then measure the room temperature inductance L of the sample magnetic ring at 10kHz and 0.25mT. 1 , calculate the bias reduction ratio D L =(L 0 -L 1 ) / L 0 .

[0103] Measured results: μ i =1700, Br / Bs=0.19, D L =1%, bias reduction ratio D L Significantly less than 50%.

[0104] Example 9

[0105] 1) Ingredients: According to the design composition: 48.8 mol% Fe 2 O 3 , 40.2 mol% Mn based on MnO 3 O 4 and 11.0 mol% ZnO, weighing the main components;

[0106] 2) Mixing: put the main ingredients into a sand mill or a ball mill and mix for 30 minutes to obtain a powder;

[0107] 3) Pre-burning: pre-burn the obtained powder at a temperature of 930°C for 2 hours, and then cool naturally to obtain the pre-burned material;

[0108] 4) Second grinding: Add auxiliary components to the above pre-sintered material: 1.09wt% CoO, 40ppm SiO 2 , 300ppm CaCO 3 , 200ppm Nb 2 O 5 , grinding for the second time to an average particle size of 0.9 μm to obtain a slurry;

[0109] 5) Granulation: Based on the total weight of the powder of the slurry obtained in step 4), add 9 wt % of a 10 wt % polyvinyl alcohol aqueous solution thereto, mix evenly and granulate to obtain granules for molding;

[0110] 6) Molding: Add a 0.5 wt% polyvinyl alcohol aqueous solution to the granules obtained in step 5) to make the moisture content of the powder reach 0.35 wt%, and add 0.5 wt% zinc stearate based on the total weight of the obtained water-containing powder to mix the materials, and press to form a green compact with a density of 3.0 g / cm 3 Green products;

[0111] 7) Sintering: The sintering temperature is 1320℃, the holding time is 6 hours, and air sintering is used from room temperature to high temperature. A small amount of nitrogen is used to protect the cooling in the cooling stage. The equilibrium oxygen partial pressure in the cooling stage is calculated according to the formula lg(P(O 2 ))=ab / T, where a is 6.55, b is 13000, and T is absolute temperature. The material is cooled and taken out of the furnace to obtain manganese-zinc ferrite material.

[0112] 8) Test: HP4284A LCR tester is used to measure the room temperature inductance L of the sample magnetic ring under the conditions of 10kHz and 0.25V. 0 , calculate the initial magnetic permeability μ of the material i ; Use SY-8258 BH tester to test Bs and Br of sample magnetic ring at 50Hz, 1200A / m, 25℃, and calculate the remanence ratio Br / Bs; Use HP4284A and HP42841A DC bias source to test the sample magnetic ring at 30A / m DC bias, without magnetic neutralization treatment, and then measure the room temperature inductance L of the sample magnetic ring at 10kHz and 0.25mT. 1 , calculate the bias reduction ratio D L =(L 0 -L1 ) / L 0 .

[0113] Measured results: μ i =1776,Br / Bs=0.19,D L =5%, bias reduction ratio D L Significantly less than 50%.

[0114] Example 10

[0115] 1) Ingredients: According to the design composition: 48.9 mol% Fe 2 O 3 , 39.6 mol% Mn based on MnO 3 O 4 and 11.5 mol% ZnO, weighing the main components;

[0116] 2) Mixing: put the main ingredients into a sand mill or a ball mill and mix for 30 minutes to obtain a powder;

[0117] 3) Pre-burning: pre-burn the obtained powder at a temperature of 910°C for 2 hours, and then cool naturally to obtain the pre-burned material;

[0118] 4) Second grinding: Add auxiliary components to the above pre-sintered material: 1.05wt% CoO, 40ppm SiO 2 , 400ppm CaCO 3 , 300ppm Nb 2 O 5 , grinding for the second time to an average particle size of 0.92 μm to obtain a slurry;

[0119] 5) Granulation: Based on the total weight of the powder of the slurry obtained in step 4), 10 wt% of a 9 wt% aqueous solution of polyvinyl alcohol is added thereto, and the mixture is mixed and granulated to obtain granules for molding;

[0120] 6) Molding: Add a 0.3 wt% polyvinyl alcohol aqueous solution to the granules obtained in step 5) to make the moisture content of the powder reach 0.35 wt%, and add 0.5 wt% zinc stearate based on the total weight of the obtained water-containing powder to mix the materials, and press to form a green compact with a density of 3.1 g / cm 3 Green products;

[0121] 7) Sintering: The sintering temperature is 1300℃, the holding time is 7 hours, and air sintering is used from room temperature to high temperature. A small amount of nitrogen is used to protect the cooling in the cooling stage. The equilibrium oxygen partial pressure in the cooling stage is calculated according to the formula lg(P(O 2 ))=ab / T, where a is 6.65, b is 13000, and T is absolute temperature. The material is cooled and taken out of the furnace to obtain the manganese-zinc ferrite material.

[0122] 8) Test: HP4284A LCR tester is used to measure the room temperature inductance L of the sample magnetic ring under the conditions of 10kHz and 0.25V. 0 , calculate the initial magnetic permeability μ of the material i ; Use SY-8258 BH tester to test Bs and Br of sample magnetic ring at 50Hz, 1200A / m, 25℃, and calculate the remanence ratio Br / Bs; Use HP4284A and HP42841A DC bias source to test the sample magnetic ring at 30A / m DC bias, without magnetic neutralization treatment, and then measure the room temperature inductance L of the sample magnetic ring at 10kHz and 0.25mT. 1 , calculate the bias reduction ratio D L =(L 0 -L 1 ) / L 0 .

[0123] Measured results: μ i =1835,Br / Bs=0.19,D L =11%, bias reduction ratio D L Significantly less than 50%.

[0124] Embodiment 11

[0125] 1) Ingredients: According to the design composition: 49.0 mol% Fe 2 O 3 , 39.0 mol% Mn based on MnO 3 O 4 and 12.0 mol% ZnO, weighing the main components;

[0126] 2) Mixing: put the main ingredients into a sand mill or a ball mill and mix for 30 minutes to obtain a powder;

[0127] 3) Pre-burning: pre-burn the obtained powder at a temperature of 950°C for 1 hour, and then cool naturally to obtain the pre-burned material;

[0128] 4) Second grinding: Add auxiliary components to the above pre-sintered material: 1.00wt% Co 2 O 3 40ppm SiO 2 , 500ppm CaCO 3 , 300ppm Nb 2 O 5 , grinding for the second time to an average particle size of 0.92 μm to obtain a slurry;

[0129] 5) Granulation: Based on the total weight of the powder of the slurry obtained in step 4), 10 wt% of an 8 wt% aqueous solution of polyvinyl alcohol is added thereto, and the mixture is uniformly mixed and granulated to obtain granules for molding;

[0130] 6) Molding: Add a 0.2 wt% polyvinyl alcohol aqueous solution to the granules obtained in step 5) to make the moisture content of the powder reach 0.35 wt%, and add 0.5 wt% zinc stearate based on the total weight of the obtained water-containing powder to mix the materials, and press to form a green compact with a density of 3.2 g / cm 3 Green products;

[0131] 7) Sintering: The sintering temperature is 1260℃, the holding time is 8 hours, and air sintering is used from room temperature to high temperature. A small amount of nitrogen is used to protect the cooling in the cooling stage. The equilibrium oxygen partial pressure in the cooling stage is calculated according to the formula lg(P(O 2 ))=ab / T, where a is 5.35, b is 11000, and T is absolute temperature. The material is cooled and taken out of the furnace to obtain manganese-zinc ferrite material.

[0132] 8) Test: HP4284A LCR tester is used to measure the room temperature inductance L of the sample magnetic ring under the conditions of 10kHz and 0.25V. 0 , calculate the initial magnetic permeability μ of the material i ; Use SY-8258 BH tester to test Bs and Br of sample magnetic ring at 50Hz, 1200A / m, 25℃, and calculate the remanence ratio Br / Bs; Use HP4284A and HP42841A DC bias source to test the sample magnetic ring at 30A / m DC bias, without magnetic neutralization treatment, and then measure the room temperature inductance L of the sample magnetic ring at 10kHz and 0.25mT. 1 , calculate the bias reduction ratio D L =(L 0 -L 1 ) / L 0 .

[0133] Measured results: μ i =2000,Br / Bs=0.19,D L =15%, bias reduction ratio D L Significantly less than 50%.

[0134] Comparative Examples 1-4

[0135] The doping component ratios, preparation methods, and tests of Comparative Examples 1-4 are the same as those of Example 6. The only difference is that the main component ratios of Comparative Examples 1-4 are different, as shown in Table 1.

[0136] Comparative Examples 5-6

[0137] The ratio of main components and doping components, preparation and testing methods of Comparative Examples 5-6 and Example 6 are the same, and the only difference is that the ratio of auxiliary components in Comparative Examples 5-6 is different, as shown in Table 1.

[0138] Comparative Examples 7-12

[0139] The ratio of main components and auxiliary components, preparation and testing methods of Comparative Examples 7-12 are the same as those of Example 6. The only difference is that the ratio of doping components in Comparative Examples 7-12 is different, as shown in Table 1.

[0140] Table 1 Comparative Example Component Ratio

[0141]

[0142] The doping ratios of Comparative Examples 7-12 are beyond the scope of the present invention. All samples are abnormally crystalline, but the crystallization performances are different. For example, MoO 3 Excessive addition leads to crystal spots on the sample surface, while Bi 2 O 3 Excessive amount leads to crystallization inside the sample.

[0143] The main component ratio of Comparative Examples 1-4 exceeds the main component range of the present invention (Fe 2 O 3 :48~49mol%、Mn 3 O 4 (in terms of MnO): 29-35 mol%, ZnO: 17-22 mol%), wherein Fe 2 O 3 The ratio is too low, and the excess cation vacancies accelerate the grain growth, resulting in the crystallization of the sample; the Fe 2 O 3 When the ratio is near the positive range, a small amount of Fe will be generated during the atmosphere sintering process. 2+ ions, greatly reducing the resistivity of the sample and increasing the eddy current loss, resulting in the sample being unable to be used for high frequencies above 10 MHz; the ZnO ratio of comparative example 3 is too low, and the magnetic permeability is lower than the scope of the present invention; the ZnO ratio of comparative example 4 is too high, and the magnetic permeability is higher than the scope of the present invention, and the Curie temperature and Bs are lower than the scope of the present invention.

[0144] The proportion of auxiliary components in Comparative Examples 5-6 exceeds the scope of the present invention (xwt% of cobalt oxide based on the total weight of the main component as Co, where the value of x is the mol% value of MnO in the main component divided by (35±4), i.e., 1.08-1.35wt%). The proportion of Co added in Comparative Example 5 is too low, and Co 2+ The compensation is insufficient, the remanence ratio reaches 0.44, and the bias is reduced by 43%; the Co addition ratio of comparative example 6 is too high, and Co 2+Overcompensation, the residual magnetism ratio reaches 0.50 and the bias is reduced by 46%.

[0145] The present invention has been described above by preferred embodiments, but it should be understood that these preferred embodiments are not intended to limit the scope of protection of the present invention. On the contrary, any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention defined by the attached claims.

Claims

1. A bias-resistant iron-poor manganese-zinc ferrite material, characterized in that: The ferrite material comprises a main component and an auxiliary component, wherein the main component is 48-49 mol% of Fe2O3, 39-45 mol% of Mn3O4 and 7-12 mol% of ZnO in terms of MnO; and the auxiliary component is 10-20 mol% of Co based on the total weight of the main component. x wt% of cobalt oxide and at least three selected from SiO2, CaCO3, V2O5, Nb2O5, Bi2O3, MoO3, wherein x The value range is the mol% value of MnO in the main component divided by (35±4); based on the total weight of the main component, SiO2 is 40~100ppm, CaCO3 is 200~800ppm, V2O5 is 0~300ppm, Nb2O5 is 50~400ppm, Bi2O3 is 0~500ppm, MoO3 is 0~500ppm; Tc≥160℃, Bs≥470mT, μ i =1000~2000, Br / Bs≤0.2, and the bias reduction of inductance ≤15%.

2. The bias drop resistant iron-poor manganese-zinc ferrite material according to claim 1, characterized in that: The cobalt oxide is a mixture of one or more of Co3O4, Co2O3 and CoO.

3. The method for preparing the bias-resistant iron-poor manganese-zinc ferrite material according to any one of claims 1 to 2, characterized in that: The steps include: 1) Ingredients: weigh the main ingredients according to the designed components; 2) Mixing: Mix the main ingredients in a sand mill or ball mill and mix thoroughly to obtain powder; 3) Pre-burning: Pre-burn the obtained powder at a temperature of 850~950℃ for 1~3 hours, and then cool down naturally to obtain the pre-burned material; 4) Second grinding: Add auxiliary components to the above-mentioned pre-sintered material and grind it to an average particle size of about 1 μm to obtain a slurry; 5) Granulation: Based on the total weight of the powder of the slurry obtained in step 4), add 8-10 wt% of an aqueous solution of polyvinyl alcohol with a concentration of 8-10 wt%, mix evenly and granulate to obtain granules for molding; 6) Molding: adding a polyvinyl alcohol aqueous solution with a concentration of 0.1-0.5 wt% to the granular material obtained in step 5) to make the moisture content of the powder reach 0.15-0.45 wt%, and adding 0.1-0.5 wt% of zinc stearate based on the total weight of the obtained water-containing powder to mix the materials, and pressing and molding into a green product; 7) Sintering: The sintering temperature is 1260~1340℃, the holding time is 4~8 hours, and the manganese-zinc ferrite material is obtained after cooling out of the furnace.

4. The preparation method according to claim 3, characterized in that: In step 6), the green compact has a density of 3.0±0.2 g / cm 3 .

5. The preparation method according to claim 3, characterized in that: In the step 7), air sintering is used from room temperature to high temperature, and a small amount of nitrogen is used to protect the cooling in the cooling stage. The equilibrium oxygen partial pressure in the cooling stage is calculated according to the formula lg(P(O2))=ab / T, where a is 5-8, b is 11000-15000, and T is the absolute temperature.