Lithium manganese iron phosphate coated lithium manganate positive electrode material and preparation method thereof

Through the nano- nano-coated lithium manganese iron phosphate, the problem of poor circulation performance of lithium manganese oxide materials at high temperatures is solved, the energy density and cycle stability are improved, and the energy density and cycle stability are met. High capacity demand.

CN118908285APending Publication Date: 2024-11-08QINGDAO QIANYUN HIGH TECH NEW MATERIAL

Patent Information

Application Number
CN202410972227.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The main reason for the poor circulation performance of lithium manganese material at high temperatures is that manganese elements react with electrolyte to cause manganese dissolution. The existing coating technology uses expensive and active LiCoO2 materials, resulting in insufficient stability of the coating layer, and lithium manganese oxide materials The capacity of the gram is low and cannot meet the high capacity requirements.

Method used

Lithium manganese phosphate nano- nano- nano- coating LiMnxFe(1-x)PO4 was coated on the LiMn2O4 surface by supercritical method, and high conductivity and chemically stable PEDOT:DSS were used as an additive to enhance the conductivity of the material. and stability, reduce process steps and are suitable for industrial production.

Benefits of technology

It significantly improves the energy density and cycle stability of lithium manganese oxide materials, reduces manganese dissolution phenomenon, improves discharge capacity and cycle performance, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908285A_ABST
    Figure CN118908285A_ABST
Patent Text Reader

Abstract

The invention relates to the field of preparation of lithium ion battery positive electrode materials, in particular to a lithium manganese iron phosphate coated lithium manganate positive electrode material and a preparation method thereof. The preparation method comprises the following steps: (1) uniformly mixing a manganese source and a lithium source in an efficient mixer, heating to a sintering temperature from room temperature, and sintering the mixed material to obtain a LiMn2O4 material; (2) dissolving a manganese source, an iron source, a phosphorus source, a carbon source, a lithium source and an additive in water, adding the LiMn2O4 material, and uniformly stirring to obtain composite slurry; (3) introducing nitrogen into the reaction kettle, heating and pressurizing to a certain temperature and pressure in a stirring state so as to change the slurry into a supercritical state, and cooling and decompressing after reaction in the state so as to obtain reacted slurry; and (4) filtering and drying the slurry after the reaction to obtain the lithium iron manganese phosphate coated lithium manganate positive electrode material. The method has the advantages that the lithium manganese iron phosphate nanocrystallization uniform coating is realized, the energy density is improved, the manganese dissolution in the circulation process is reduced, and meanwhile, the preparation efficiency is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of lithium ion battery positive electrode materials, in particular to a lithium manganese iron phosphate coated lithium manganate positive electrode material and a preparation method thereof. Background Art

[0002] With the continuous development of electronic devices such as spacecraft, electric vehicles, medical equipment and communication equipment, lithium-ion batteries have become an indispensable part of them. Lithium manganese oxide with a quartz structure has become one of the most actively studied, most developed and most promising cathode materials due to its excellent electrochemical properties, rich raw material sources, good safety performance, environmental protection and non-toxicity, and is favored by scientific research institutions and commercial companies. It is generally believed that the main reason for the poor high-temperature cycle performance of lithium manganese oxide materials is that the reaction between manganese elements and electrolytes in lithium manganese oxide materials intensifies under high temperature environments, causing a large amount of manganese elements to dissolve. In order to solve the problem of manganese dissolution, Chinese invention patent publication number CN1282113A uses a liquid phase coating technology to coat a layer of LiCoO2 particles on the surface of LiMn2O4 particles to prevent the dissolution of manganese during the cycle. However, first of all, LiCO2 is expensive, and secondly, LiCoO is more active and less stable. The side reactions of contact with the electrolyte during the cycle increase, resulting in the destruction of the coating layer, thereby affecting the cycle. Moreover, the current gram capacity of LiMn2O4 positive electrode material is less than 120mAh / g, which is too low to meet the demand for higher capacity usage.

[0003] Lithium iron manganese phosphate (LiMn x Fe 1-x PO4) cathode materials are currently being widely studied due to their higher voltage platform (3.8V-4.1V), high gram capacity (>140mAh / g) and material stability comparable to that of lithium iron phosphate LiFePO4.

[0004] At present, lithium iron manganese phosphate positive electrode materials are often mixed and coated with lithium manganese oxide positive electrode materials to improve the capacity and cycle performance of lithium manganese oxide; the commonly used mixing method is to mix lithium iron manganese phosphate and lithium manganese oxide in a certain proportion. The material prepared by this method has the problem of uneven lithium iron manganese phosphate coating on lithium manganese oxide. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a lithium manganese iron phosphate coated lithium manganate positive electrode material, which realizes the advantages of lithium manganese iron phosphate nano-sized and uniformly coated, improves energy density and reduces manganese dissolution during the cycle, and has high preparation efficiency. The present invention also provides a preparation method thereof.

[0006] The method for preparing the lithium manganese iron phosphate coated lithium manganate positive electrode material of the present invention comprises the following steps:

[0007] (1) uniformly mixing a manganese source and a lithium source in a high-efficiency mixer, heating the mixture from room temperature to a sintering temperature, and sintering the mixed material to obtain a LiMn2O4 material;

[0008] (2) According to the chemical formula of lithium manganese iron phosphate, LiMn x Fe (1-x) PO4, x is 0.5-0.7, a manganese source, an iron source, a phosphorus source, a carbon source, a lithium source and an additive are dissolved in water, and then the LiMn2O4 material obtained in step (1) is added and stirred evenly to obtain a composite slurry, wherein the additive is poly (3,4-ethylenedioxythiophene): dextran sulfate (ie, PEDOT:DSS).

[0009] (3) introducing nitrogen into a high-temperature and high-pressure reactor containing the composite slurry, heating and pressurizing to a certain temperature and pressure under stirring to make the slurry become a supercritical state, and cooling and releasing the pressure after the reaction in this state to obtain a post-reaction slurry;

[0010] (4) After the reaction, the slurry is filtered and dried to obtain the lithium manganese iron phosphate-coated lithium manganate positive electrode material.

[0011] Preferably, in step (1), the manganese source is at least one of manganese dioxide and manganese tetroxide, and the lithium source is at least one of lithium carbonate and lithium hydroxide.

[0012] Preferably, in step (2), the manganese source is at least one of manganese sulfate, manganese nitrate, and manganese acetate, the iron source is at least one of ferric nitrate and ferric sulfate, the lithium source is at least one of lithium carbonate and lithium hydroxide, the phosphorus source is at least one of phosphoric acid and diammonium phosphate, and the carbon source is at least one of glucose and sucrose.

[0013] Preferably, in step (2), the molar amount of the additive is 1%-5% of the total molar amount of Mn and Fe in the manganese source and the iron source.

[0014] Preferably, in step (2), LiMn x Fe (1-x) PO4 mass accounts for the LiMn2O4 material and LiMn x Fe (1-x) 5-20% of the total mass of PO4.

[0015] Preferably, in step (1), the heating rate is 4-6°C / min, the sintering temperature is 750-800°C, and the sintering time is 10-16h.

[0016] Preferably, in step (3), the temperature of the reactor is 350-400° C., the pressure is 25-30 MPa, and the time is 20-30 min.

[0017] The lithium manganese iron phosphate coated lithium manganate positive electrode material of the present invention is prepared by the above-mentioned preparation method.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. The additive PEDOT:DSS of the present invention is a composite conductive polymer material, which has the characteristics of high conductivity, chemical stability, thermal stability, etc. The additive can exert its good electrochemical activity when coated on the surface of the material, and can reduce the interface resistance between the positive electrode and the electrolyte, thereby improving the conductivity and stability of the material;

[0020] 2. The present invention uses a supercritical method to convert nano-LiMn into x Fe (1-x) PO4 is evenly coated on the surface of LiMn2O4, which is more fine and uniform than the traditional mechanical ball milling mixing and hydrothermal coating. x Fe (1-x) PO4 is coated on the surface of LiMn2O4 in one step, which reduces the conventional preparation of LiMn x Fe (1-x) The high-temperature sintering and other process steps required for PO4 have a simple process flow and a fast reaction rate, making it suitable for large-scale industrial production. For the synthesized materials, it improves the structural stability, effectively inhibits the dissolution of manganese metal from the material, improves the cycle stability of the battery, and at the same time improves the discharge capacity of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a comparison chart of the discharge capacity of Examples 1-4 and Comparative Example 1 at 0.2C. DETAILED DESCRIPTION

[0022] The technical solution of the present invention will be clearly and completely described below in conjunction with embodiments.

[0023] Unless otherwise specified, all raw materials used in the examples are commercially available.

[0024] Among them, PEDOT:DSS uses PEDOT:DSS aqueous dispersion produced by Mingyang Technology (Tianjin) Co., Ltd.

[0025] Example 1

[0026] (1) weighing 1 mol of electrolytic manganese dioxide and lithium carbonate at a Li:Mn molar ratio of 1.02:2, dispersing the mixture in a high-efficiency mixer for 30 min, sintering the mixed materials, heating the temperature from room temperature to 760° C. at a rate of 5° C. / min, sintering for 12 h, and grinding and sieving after cooling to obtain LiMn2O4 material;

[0027] (2) The chemical formula of lithium iron manganese phosphate is LiMn 0.6 Fe 0.4 PO4, weigh manganese sulfate and ferric sulfate according to the molar ratio of Mn to Fe of 6:4, prepare a solution with a total molar concentration of manganese sulfate and ferric sulfate of 0.1 mol / L, weigh lithium hydroxide according to the molar number of Li: the total molar number of Mn and Fe of 1.02:1, weigh diammonium phosphate according to the molar number of P: the total molar number of Mn and Fe of 1:1, and according to the theoretically generated LiMn 0.6 Fe 0.4 Glucose was weighed at 5% of the mass of PO4, and PEDOT:DSS was weighed at 2% of the total molar number of Mn and Fe. The above raw materials were added into a high-temperature and high-pressure reactor and stirred evenly; the theoretically prepared LiMn 0.6 Fe 0.4 PO4 mass Weigh the LiMn2O4 material (make LiMn 0.6 Fe 0.4 PO4 accounts for LiMn2O4 material and LiMn 0.6 Fe 0.4 PO4 mass) was added into a high temperature and high pressure reactor and stirred evenly to obtain a composite slurry;

[0028] (3) The high temperature and high pressure reactor was continuously stirred and nitrogen was introduced. The temperature was controlled at 400° C. and the pressure was 25 MPa to make the slurry become supercritical. The reaction was carried out for 20 minutes. After the pressure was released and cooled, the slurry was filtered and dried to obtain a nano-scale lithium manganese iron phosphate coated lithium manganese oxide positive electrode material with a coating amount of 5%.

[0029] Example 2

[0030] The difference between Example 2 and Example 1 is that in step (2), the theoretically prepared LiMn 0.6 Fe 0.4 PO4 accounts for LiMn2O4 material and LiMn 0.6 Fe 0.4 10% of the total mass of PO4.

[0031] Example 3

[0032] The difference between Example 3 and Example 1 is that in step (2), the theoretically prepared LiMn 0.6 Fe 0.4 PO4 accounts for LiMn2O4 material and LiMn 0.6 Fe 0.4 15% of the total mass of PO4.

[0033] Example 4

[0034] The difference between Example 4 and Example 1 is that in step (2), the theoretically prepared LiMn0.6 Fe 0.4 PO4 accounts for LiMn2O4 material and LiMn 0.6 Fe 0.4 20% of the total mass of PO4.

[0035] Comparative Example 1

[0036] This comparative example 1 uses the LiMn2O4 material obtained according to step (1) in Example 1.

[0037] Comparative Example 2

[0038] (1) weighing 1 mol of electrolytic manganese dioxide and lithium carbonate at a Li:Mn molar ratio of 1.02:2, dispersing the mixture in a high-efficiency mixer for 30 min, sintering the mixed materials, heating the temperature from room temperature to 760° C. at a rate of 5° C. / min, sintering for 12 h, and grinding and sieving after cooling to obtain LiMn2O4 material;

[0039] (2) The chemical formula of lithium iron manganese phosphate is LiMn 0.6 Fe 0.4 PO4, weigh manganese sulfate and ferric sulfate according to the molar ratio of Mn to Fe of 6:4, prepare a solution with a total molar concentration of manganese sulfate and ferric sulfate of 0.1 mol / L, weigh lithium hydroxide according to the molar number of Li: the total molar number of Mn and Fe of 1.02:1, weigh diammonium phosphate according to the molar number of P: the total molar number of Mn and Fe of 1:1, and according to the theoretically generated LiMn 0.6 Fe 0.4 Weigh glucose at 5% of the mass of PO4 and weigh PEDOT:DSS at 2% of the total molar number of Mn and Fe, add the above raw materials into a high-temperature and high-pressure reactor and stir evenly;

[0040] (3) The high temperature and high pressure reactor was continuously stirred, nitrogen was introduced, the temperature was controlled at 400°C, the pressure was 25 MPa, the slurry became supercritical, the reaction was carried out for 20 minutes, the pressure was released and the slurry was filtered and dried after cooling to obtain LiMn 0.6 Fe 0.4 PO4 material.

[0041] (4) LiMn 0.6 Fe 0.4 PO4 material accounts for LiMn2O4 material and LiMn 0.6 Fe 0.4 Weigh LiMn2O4 material, which is 5% of the total mass of PO4, and then mix it with LiMn 0.6 Fe 0.4 The PO4 materials are mechanically mixed in a ball mill to obtain a blended material as a positive electrode material.

[0042] Comparative Example 3

[0043] (1) weighing 1 mol of electrolytic manganese dioxide and lithium carbonate at a Li:Mn molar ratio of 1.02:2, dispersing the mixture in a high-efficiency mixer for 30 min, sintering the mixed materials, heating the temperature from room temperature to 760° C. at a rate of 5° C. / min, sintering for 12 h, and grinding and sieving after cooling to obtain LiMn2O4 material;

[0044] (2) The chemical formula of lithium iron manganese phosphate is LiMn 0.6 Fe 0.4 PO4, weigh manganese sulfate and ferric sulfate according to the molar ratio of Mn to Fe of 6:4, prepare a solution with a total molar concentration of manganese sulfate and ferric sulfate of 0.1 mol / L, weigh lithium hydroxide according to the molar number of Li: the total molar number of Mn and Fe of 1.02:1, weigh diammonium phosphate according to the molar number of P: the total molar number of Mn and Fe of 1:1, and according to the theoretically generated LiMn 0.6 Fe 0.4 PO4 mass 5% glucose was weighed, and the above raw materials were added into a high temperature and high pressure reactor and stirred evenly; the theoretically prepared LiMn 0.6 Fe 0.4 PO4 mass Weigh the LiMn2O4 material (make LiMn 0.6 Fe 0.4 PO4 accounts for LiMn2O4 material and LiMn 0.6 Fe 0.4 PO4 mass) was added into a high temperature and high pressure reactor and stirred evenly to obtain a composite slurry;

[0045] (3) The high temperature and high pressure reactor was continuously stirred and nitrogen was introduced. The temperature was controlled at 400° C. and the pressure was 25 MPa to make the slurry become supercritical. The reaction was carried out for 20 minutes. After the pressure was released and cooled, the slurry was filtered and dried to obtain a nano-scale lithium manganese iron phosphate coated lithium manganese oxide positive electrode material with a coating amount of 5%.

[0046] Performance Testing

[0047] The positive electrode materials obtained in Examples 1-4 and Comparative Examples 1-3, acetylene black and polyvinylidene fluoride (PVDF) binder were uniformly mixed in a weight ratio of 94:3:3, dispersed in N-methylpyrrolidone (NMP) solution to obtain a paste-like mixture, coated on aluminum foil, and vacuum dried at 90°C overnight to obtain a battery positive electrode sheet.

[0048] Assembly of button cells (2016 model) was performed in a glove box filled with high-purity argon:

[0049] A lithium metal sheet was used as the negative electrode, a polypropylene film was used as the separator, 1 mol LiPF6 was dissolved in ethyl carbonate / dimethyl carbonate (EC / DMC volume ratio 1:1) as the electrolyte, and the above-mentioned positive electrode sheet was used as the positive electrode of the battery to obtain a lithium-ion battery.

[0050] The charging and discharging performance tests of lithium-ion batteries were carried out on a blue power test system at room temperature. The test voltage range was 3.0-4.3V. The test results are shown in Table 1.

[0051] Table 1 Battery performance test table of Examples 1-4 and Comparative Examples 1-3

[0052]

[0053] From Examples 1-4 and Comparative Example 1, Figure 1 , the coating of lithium iron manganese phosphate can improve the performance of lithium manganese oxide material. With the increase of the coating amount of lithium iron manganese phosphate, the discharge capacity, material energy density and cycle retention rate all increase; from Example 1 and Comparative Example 2, lithium iron manganese phosphate is coated on the surface of lithium manganese oxide by supercritical method, and the cycle performance and discharge capacity of the material are better than those of simple mechanical mixing of the two, indicating that the coating of the present invention is more uniform; from Example 1 and Comparative Example 3, the use of the additive PEDOT:DSS helps to improve the capacity and cycle performance of the coated material; in summary, the present invention significantly improves the capacity and cycle performance of lithium manganese oxide material.

Claims

1. A method for preparing a lithium manganese iron phosphate coated lithium manganate positive electrode material, characterized in that: The following steps are involved: (1) uniformly mixing a manganese source and a lithium source in a high-efficiency mixer, heating the mixture from room temperature to a sintering temperature, and sintering the mixed material to obtain a LiMn2O4 material; (2) According to the chemical formula of lithium manganese iron phosphate, LiMn x Fe (1-x) PO4, x is 0.5-0.7, a manganese source, an iron source, a phosphorus source, a carbon source, a lithium source and an additive are dissolved in water, and the LiMn2O4 material obtained in step (1) is added and stirred to obtain a composite slurry, wherein the additive is poly(3,4-ethylenedioxythiophene): dextran sulfate; (3) introducing nitrogen into a reaction kettle containing the composite slurry, heating and pressurizing the slurry under stirring to make the slurry become a supercritical state, and cooling and releasing the pressure after the reaction in this state to obtain a post-reaction slurry; (4) After the reaction, the slurry is filtered and dried to obtain the lithium manganese iron phosphate-coated lithium manganate positive electrode material.

2. The method for preparing the lithium manganese iron phosphate coated lithium manganate positive electrode material according to claim 1, characterized in that: In step (1), the manganese source is at least one of manganese dioxide and manganese tetroxide, and the lithium source is at least one of lithium carbonate and lithium hydroxide.

3. The method for preparing the lithium manganese iron phosphate coated lithium manganate positive electrode material according to claim 1, characterized in that: In step (2), the manganese source is at least one of manganese sulfate, manganese nitrate, and manganese acetate, the iron source is at least one of iron nitrate and iron sulfate, the lithium source is at least one of lithium carbonate and lithium hydroxide, the phosphorus source is at least one of phosphoric acid and diammonium phosphate, and the carbon source is at least one of glucose and sucrose.

4. The method for preparing the lithium manganese iron phosphate coated lithium manganate positive electrode material according to claim 1, characterized in that: In step (2), the molar number of the additive is 1%-5% of the total molar number of Mn and Fe in the manganese source and the iron source.

5. The method for preparing the lithium manganese iron phosphate coated lithium manganate positive electrode material according to claim 1, characterized in that: In step (2), LiMn x Fe (1-x) PO4 mass accounts for the LiMn2O4 material and LiMn x Fe (1-x) 5-20% of the total mass of PO4.

6. The method for preparing the lithium manganese iron phosphate coated lithium manganate positive electrode material according to claim 1, characterized in that: In step (1), the heating rate is 4-6°C / min, the sintering temperature is 750-800°C, and the sintering time is 10-16h.

7. The method for preparing the lithium manganese iron phosphate coated lithium manganate positive electrode material according to claim 1, characterized in that: In step (3), the temperature of the reactor is 350-400° C., the pressure is 25-30 MPa, and the time is 20-30 min.

8. A lithium manganese iron phosphate coated lithium manganate positive electrode material, characterized in that: The invention is prepared by the preparation method according to claims 1 to 7.

Citation Information

Patent Citations

  • Positive electrode material of lithium ion cell and its preparation method

    CN1282113A

Cited By

  • Lithium triborate coated lithium manganate positive electrode material and preparation method thereof

    CN119812292A

  • Lithium Manganate Cathode Material Coated with Lithium Triborate and Preparation Method Thereof

    CN119812292B

  • Method for preparing carbon and lithium manganese phosphate double-coated lithium manganate

    CN120271047A

  • A method for preparing carbon and lithium manganese phosphate double-coated lithium manganate

    CN120271047B

  • Lithium manganese iron phosphate positive electrode material and preparation method thereof

    CN120749165A