Silver-coated copper powder with compact coating and preparation method of silver-coated copper powder
Through the combination of dilute nitric acid rinsing and electroless plating, the problem of immature domestic silver-clad copper powder technology has been solved, and the preparation of silver-clad copper powder with low silver content and high conductivity has been achieved. It is suitable for large-scale industrial production and breaks the import monopoly.
Patent Information
- Application Number
- CN202411245581.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
AI Technical Summary
The domestic silver-clad copper powder technology is immature, and it is difficult to maintain good conductivity under low silver content, resulting in the domestic market relying on imported products, high production costs, high equipment requirements, and insufficient coverage density and electrical performance.
The copper powder is quickly rinsed with dilute nitric acid, combined with the electroless plating method, through the pH adjustment, the action of dispersant and complexing agent, a dense silver-clad layer is formed, and the reaction conditions are controlled to prepare silver-clad copper powder with low silver content, which is suitable for large Large-scale industrial production.
It has achieved good density, low silver content and excellent electrical performance of silver, and can coat micron-level copper powder. It is suitable for copper powder of different particle sizes, reducing production costs and equipment requirements, and is suitable for large-scale industrial production.
Smart Images

Figure CN119057065A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal powder processing, in particular to a densely coated silver-coated copper powder and a preparation method thereof. Background Art
[0002] With the rapid development of the electronic information industry, precious metal electronic paste has become one of the key materials for the production of various electronic components. Currently, the most widely used and largest amount of metal is silver powder. However, silver is relatively expensive and prone to electron migration. Copper powder has excellent conductivity similar to silver (the volume resistivity of silver is 1.59×10 -6 Ω·cm, the volume resistivity of copper is 1.72×10 -6 Ω·cm), but poor oxidation resistance, conductivity drops sharply after oxidation. Silver-coated copper powder is a composite material with a silver surface and copper core evenly plated on the copper surface, which maintains the excellent conductivity of copper powder and silver powder, while overcoming the problems of electron migration of silver powder and easy oxidation of copper powder during use. It has low cost and has the prospect of large-scale application.
[0003] There are two methods for preparing silver-coated copper powder: physical method and chemical method. Physical method includes mixed ball milling method, spray pyrolysis method, etc., which have high requirements on equipment, high production cost, and poor coating effect on small-particle copper powder; chemical method includes electron beam radiation method, chemical plating method, etc. Among them, although electron beam radiation method is chemical reduction, the electron irradiation accelerator is expensive and the production cost is high. Compared with other methods, chemical plating method has simple process and low preparation cost. Therefore, the preparation method of silver-coated copper powder is mainly chemical plating.
[0004] Foreign manufacturers have been deeply involved in this industry for many years, and the silver-coated copper powder they prepare has good coating density and low silver content. However, the technology of domestic silver-coated copper powder is still immature, and it is difficult to ensure that the silver-coated copper powder produced can maintain good conductivity while having a low silver content. It is rare to produce qualified silver-coated copper powder that can be used on a large scale. The silver-coated copper powder used in the domestic market is still mainly imported.
[0005] Patent application CN201210389912.3 discloses a method for preparing silver-coated copper powder, wherein copper and a complexing agent are mixed, and copper is used as a reducing agent to replace silver ions in silver sulfate to obtain silver-coated copper powder. However, the invention requires ultrasonic stirring, has certain requirements for equipment, and is limited to laboratory preparation. Patent application CN 201510198208.3 discloses a method for preparing silver-coated copper powder by replacement reduction method, wherein other reducing agents are added while dripping silver solution, and silver particles are slowly immersed on the replaced silver crystal nuclei to obtain coated silver-coated copper powder. However, the invention has complicated reaction steps, rough coating surface, more reagents, high reaction temperature, high cost, and poor electrical properties, making it difficult to apply.
[0006] The patent application CN202110176568.9 discloses a preparation method of multi-step reduction deposition coating, which adopts chemical plating method, and after multiple reductions of silver ions to silver particles and deposition on the surface of copper powder, the deposition and coating of silver element is controlled by different complexing agents and dispersants to obtain silver-coated copper powder. However, the invention has cumbersome steps, and the coating surface is relatively rough. A high silver coating amount is required for good electrical properties. It is still in the experimental stage and difficult to realize production. The patent application CN202210836431.6 discloses a method for obtaining silver-coated copper powder by chemical plating. In a solution in which copper powder is evenly dispersed, a silver ammonia solution is gradually added dropwise for replacement reaction, thereby preparing silver-coated copper powder. However, the invention has high requirements for equipment and is not suitable for large-scale industrial production.
[0007] At present, the silver-coated copper powder used by domestic manufacturers is still mainly imported; compared with foreign countries, the domestic silver-coated copper technology is immature, and there are very few domestic silver-coated copper powder manufacturers. From the electron microscope images of the samples obtained by the inventors, the prepared silver-coated copper powder has poor coating properties and a rough surface. At the same time, the silver content is high, the economic benefits are low, and the application is greatly limited. Summary of the invention
[0008] In view of the above problems existing in the prior art, the present invention provides a silver-coated copper powder with compact coating and a preparation method thereof. The present invention adopts a chemical plating method, and the obtained silver-coated copper powder has good compactness, low silver content, excellent electrical properties, can effectively coat various micron-level copper powders, and can prepare silver-coated copper powder with a smaller particle size than the currently used one, which has a strong technical advantage.
[0009] The technical solution of the present invention is as follows:
[0010] A densely coated silver-coated copper powder, the preparation method of the silver-coated copper powder comprising the following steps:
[0011] (1) quickly washing the copper powder with dilute nitric acid, adding a dispersant, adjusting the pH value with a pH adjuster, and finally adding water to prepare a copper system;
[0012] (2) weighing a reducing agent and dissolving it in water, then adding a pH adjuster to adjust the pH value, and finally adding water to prepare a reducing system;
[0013] (3) weighing silver nitrate and dissolving it in water, adding a complexing agent for complexation, and finally adding water to prepare a silver ammonia plating solution system;
[0014] (4) mixing the reduction system obtained in step (2) and the copper system obtained in step (1) and stirring them evenly, then adding the silver ammonia plating solution system obtained in step (3) to react, and obtaining primary silver-coated copper powder after the reaction is complete;
[0015] (5) The primary silver-coated copper powder is cleaned with water, a coating agent is added for dispersion and coating, and the powder is dried to obtain a silver-coated copper powder with good compactness.
[0016] Preferably, the concentration of the dilute nitric acid in step (1) is 3-5wt%, and the flushing time of the dilute nitric acid is 3-60s; the mass volume ratio of the copper powder before flushing to the copper system prepared by adding water is 1:8-12kg / L.
[0017] Preferably, the dispersant in step (1) is at least one of gum arabic, gum guar, sodium pyrophosphate and gelatin; the amount of the dispersant is 1-10wt% of the copper powder before washing; and the dispersant is dispersed in water to form an emulsion before use.
[0018] Preferably, the reducing agent in step (2) is at least one of ascorbic acid, glucose, hydroxylammonium sulfate, sodium hypophosphite, and sodium borohydride; the amount of the reducing agent is 1.0-1.1 times the theoretical value required for reducing silver; the mass volume ratio of the reducing agent to the reducing system prepared by adding water is 1.5:18-22kg / L.
[0019] Preferably, the pH adjusting agent in steps (1) and (2) is at least one of ammonia water, sodium hydroxide, potassium hydroxide, acetic acid, and sodium acetate; and the pH value adjusted in steps (1) and (2) is in the range of 8-14, respectively.
[0020] Preferably, the amount of silver nitrate used in step (3) is 23-35% of the mass of the copper powder before rinsing; the mass volume ratio of the silver nitrate to the silver ammonia plating solution system prepared by adding water at last is 2.65:48-52 kg / L.
[0021] Preferably, the complexing agent in step (3) is at least one of ammonia water, ethylenediaminetetraacetic acid, salicylic acid, sodium thiosulfate, and sodium cyanide; and the amount of the complexing agent used is 1.1-3.0 times the theoretical value of the amount required for complexing silver nitrate.
[0022] Preferably, the volume ratio of the copper system, the reduction system and the silver ammonia plating solution system in step (4) is 8-10:1-2:3-5; and the reaction time is 30min-60min.
[0023] Preferably, the coating agent in step (5) is at least one of stearic acid, erucic acid, oleic acid, hexadecanoic acid and tetradecanoic acid; and the amount of the coating agent used is 0.1-1.0% of the mass of the copper powder before washing.
[0024] Preferably, the temperature during the preparation of the silver-coated copper powder is controlled at 15-45°C.
[0025] Furthermore, step (1) of washing the copper powder with dilute nitric acid can remove the oxide layer on its surface and some crystals with weak bonding force, making the copper powder smooth and compact, and at the same time activating the copper powder so that the silver particles are more easily deposited on the surface to form a dense coating layer.
[0026] Furthermore, the encapsulating agent in step (5) is preferably stearic acid or oleic acid.
[0027] The beneficial technical effects of the present invention are:
[0028] 1. The present invention uses a dilute nitric acid solution to quickly rinse the copper powder, removes the oxide layer on the surface of the copper powder, and corrodes the weakly bonded crystals on the surface of the copper powder, making the copper powder smoother and more compact, and making the silver particles more easily and evenly deposited on the surface of the copper powder under molecular forces. This is a major technical breakthrough, because nitric acid solution can dissolve metallic copper, so nitric acid solution is usually not used in the art to clean copper powder, but dilute sulfuric acid, acetone, sodium hydroxide solution, ammonium sulfate solution and other less corrosive acids or bases are used.
[0029] The inventors have found through a large number of comparative experiments that nitric acid solution can reduce the protrusions and grooves on the surface of copper powder, making the copper powder more spherical, increasing the centripetal force during particle deposition, reducing the shedding phenomenon caused by the uneven surface during silver particle deposition, and making the silver particles deposited more evenly and tightly. Under the condition of controlling the concentration and rinsing time of the nitric acid solution, the dissolving effect of nitric acid on the copper powder can be minimized.
[0030] 2. The present invention uses copper powder that has been rapidly washed with dilute nitric acid, and in a uniformly dispersed copper system, through the combined action of a complexing agent and a dispersant, reduces silver ions to simple silver in a solution and adsorbs it on the surface of the copper powder to obtain densely coated silver-coated copper powder; after washing, filtering, wrapping, and drying, the silver-coated copper powder with good density is prepared, and the entire reaction process can be completed in one reactor, with low requirements on equipment. The present invention has a simple process, is easy to mass produce, and is suitable for large-scale industrial production.
[0031] 3. The present invention can be used to coat copper powders of different particle sizes. Generally, different particle sizes of copper powders and different silver coating amounts require different coating conditions, which can be adjusted by controlling the reaction speed and particle size of the silver particles. Generally speaking, the smaller the particle size of the coated copper powder and the less the coating amount, the smaller the silver particles required for better deposition and accumulation. This requires changing the reaction conditions to make the generated silver particles smaller and the coating smoother. The present invention controls the formation and growth of silver particles by adjusting the reaction temperature, concentration, dispersant and other conditions, and can well control the silver-coated copper powder with different silver coating amounts, prepare silver-coated copper powders of different particle sizes and excellent electrical properties, and ensure the stability of copper powder coating.
[0032] 4. Compared with foreign countries, there are only a few domestic manufacturers that can use the chemical reduction deposition method to prepare silver-coated copper powder with good conductivity. At present, the silver-coated copper powder used in China is still mainly imported. The present invention can prepare silver-coated copper powder with an average particle size of 1 μm, and the silver coating amount can be as low as 15%. It is expected to break the foreign monopoly on silver-coated copper powder and carry out domestic substitution. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a SEM image of the silver-coated copper powder prepared in Example 1;
[0034] Figure 2 This is a SEM image of the silver-coated copper powder prepared in Example 2;
[0035] Figure 3 This is a SEM image of the silver-coated copper powder prepared in Example 3;
[0036] Figure 4 This is a SEM image of the silver-coated copper powder prepared in Comparative Example 1;
[0037] Figure 5 This is the SEM image of imported silver-coated copper powder;
[0038] Figure 6 This is the SEM image of domestic silver-coated copper powder. DETAILED DESCRIPTION
[0039] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Embodiment 1:
[0041] (1) Weigh 10 kg of copper powder, rinse it with 3 wt % dilute nitric acid for 20 seconds, and put it into a No. 1 batching barrel after cleaning. Add an emulsion containing 300 g of gelatin that has been dispersed in water in advance, add sodium hydroxide to adjust the pH to 12, and finally add water to prepare a 100 L copper system, and adjust the temperature to 40°C.
[0042] (2) Weigh 1.5 kg of ascorbic acid into the No. 2 mixing barrel, add 10 L of water to dissolve it, add sodium hydroxide to adjust the pH to 12, and finally add water to prepare a 20 L reduction system, and adjust the temperature to 40°C.
[0043] (3) Weigh 2.65 kg of silver nitrate into the No. 3 mixing barrel, add 20 L of water to dissolve it, add 10 kg of ammonia water, and finally add water to prepare a 50 L silver ammonia plating solution system, and adjust the temperature to 40°C.
[0044] (4) First, add the reducing system to the copper system, stir evenly, and then add the silver ammonia plating solution system to react. The feeding time during the control process is 2 minutes. After the feeding is completed, the reaction takes 30 minutes. The temperature during the reaction is controlled at 40°C.
[0045] (5) After the reaction is complete, the silver-coated copper powder is washed with water, 30 g of oleic acid is added for dispersion coating, and then dried to obtain densely coated silver-coated copper powder.
[0046] The surface morphology of the silver-coated copper powder prepared in Example 1 is as follows Figure 1 As shown in the figure, it can be seen that the silver layer coated on the surface of the silver-coated copper powder prepared by the present invention is smooth and dense, and the powder is evenly dispersed.
[0047] Embodiment 2:
[0048] Comparative Example 1, in step (1), a modification was made, the emulsion containing 300g of gelatin was changed to an emulsion containing 1kg of guar gum, and the remaining steps were the same. The surface morphology of the prepared silver-coated copper was as follows: Figure 2 As shown. Figure 2 It can be seen that replacing the type of dispersant and increasing the amount of dispersant can make the generated silver particles smaller, thereby coating copper powder with smaller particle size, and then controlling the product particle size of silver-coated copper powder.
[0049] Embodiment 3:
[0050] Comparative Example 1, the operation method of step (2) was modified as follows: 3.67 kg of silver nitrate was weighed into a mixing bucket, 20 L of water was added to dissolve, 15 kg of ammonia water was added, the temperature was adjusted to 40° C., and water was added to prepare a 50 L silver ammonia plating solution system. At the same time, the feeding time of step (4) was modified to 4 min.
[0051] The silver coating amount in this embodiment is 20%, and the surface morphology of the prepared silver-coated copper powder is as follows. Figure 3 As shown in the figure, it can be seen that the particle size prepared in this embodiment is larger.
[0052] Comparative Example 1:
[0053] Comparative Example 1, the dilute nitric acid in step (1) was changed to 3 wt % dilute sulfuric acid, and the surface morphology of the prepared silver-coated copper powder was as follows: Figure 4 As shown. Figure 4 It can be seen that the surface of the powder is relatively rough and there are many small particles. This is because dilute sulfuric acid can only remove the oxide layer but cannot remove the protrusions and grooves on the surface. The silver particles are hindered by these crystals during deposition, resulting in unstable adsorption and falling off.
[0054] Comparative Example 2:
[0055] The inventor purchased imported silver-coated copper powder and domestic silver-coated copper powder from the market, and their surface morphologies were as follows: Figure 5 and Figure 6 As shown. Figure 5 It can be seen that the coating surface of the imported powder is relatively smooth, with fewer small particles but larger average particles. Figure 6 It can be seen that the particle size of domestic powder is smaller than that of imported powder, but the coating surface is rough and the coating effect is average. The silver coating amount of imported powder is 20%, and the silver coating amount of domestic powder is 30%. In comparison, the silver content of the powder prepared by the present invention can be as low as 15%, the coating surface is smooth and flat, and the particle size is small, which has certain advantages in application.
[0056] Test example:
[0057] 1. The particle size and other aspects of Examples 1-3, Comparative Example 1 and Comparative Example 2 were tested. The test results are shown in Table 1.
[0058] Table 1
[0059]
[0060]
[0061] 2. Resistance tests were performed on Examples 1-3, Comparative Examples 1 and 2 at different temperatures. The test results are shown in Table 2, wherein the lower the resistance data, the better the conductive property of the silver-coated copper powder.
[0062] Table 2
[0063] Serial number Example 1 Example 2 Example 3 Comparative Example 1 Imported flour Domestic powder 140℃ / 30min 6.10E-04 9.00E-04 5.10E-04 2.40E-03 1.60E-03 1.70E-03 160℃ / 30min 5.90E-04 8.80E-04 4.30E-04 1.60E-03 1.20E-03 1.20E-03 180℃ / 30min 4.60E-04 6.00E-04 3.30E-04 1.60E-03 8.90E-04 8.80E-04 200℃ / 30min 3.40E-04 4.30E-04 2.50E-04 1.20E-03 7.00E-04 7.60E-04
[0064] Combining Table 1 and Table 2, it can be seen that the silver-coated copper powder prepared by the present invention has an overall smaller particle size than that of imported and domestic powders, which is more in line with the development trend of future slurries. At the same time, it has certain advantages in electrical properties when the silver content is lower, and has greater economic value.
[0065] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and implementation modes, and can be fully applicable to various fields suitable for the present invention. For those familiar with the art, for those of ordinary skill in the art, various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principle and spirit of the present invention. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A densely coated silver-coated copper powder, characterized in that: The preparation method of the silver-coated copper powder comprises the following steps: (1) quickly washing the copper powder with dilute nitric acid, adding a dispersant, adjusting the pH value with a pH adjuster, and finally adding water to prepare a copper system; (2) weighing a reducing agent and dissolving it in water, then adding a pH adjuster to adjust the pH value, and finally adding water to prepare a reducing system; (3) weighing silver nitrate and dissolving it in water, adding a complexing agent for complexation, and finally adding water to prepare a silver ammonia plating solution system; (4) mixing the reduction system obtained in step (2) and the copper system obtained in step (1) and stirring them evenly, then adding the silver ammonia plating solution system obtained in step (3) to react, and obtaining primary silver-coated copper powder after the reaction is complete; (5) The primary silver-coated copper powder is cleaned with water, a coating agent is added for dispersion and coating, and the powder is dried to obtain a silver-coated copper powder with good compactness.
2. The silver-coated copper powder according to claim 1, characterized in that: The concentration of the dilute nitric acid in step (1) is 3-5wt%, and the flushing time of the dilute nitric acid is 3-60s; the mass volume ratio of the copper powder before flushing to the copper system prepared by adding water at last is 1:8-12kg / L.
3. The silver-coated copper powder according to claim 1, characterized in that: The dispersant in step (1) is at least one of gum arabic, gum guar, sodium pyrophosphate and gelatin; the amount of the dispersant is 1-10wt% of the copper powder before washing; the dispersant is dispersed in water to form an emulsion before use.
4. The silver-coated copper powder according to claim 1, characterized in that: The reducing agent in step (2) is at least one of ascorbic acid, glucose, hydroxylammonium sulfate, sodium hypophosphite, and sodium borohydride; the amount of the reducing agent is 1.0-1.1 times the theoretical value required for reducing silver; the mass volume ratio of the reducing agent to the reducing system prepared by adding water is 1.5:18-22kg / L.
5. The silver-coated copper powder according to claim 1, characterized in that: The pH regulators in steps (1) and (2) are ammonia water and sodium hydroxide respectively. 、 At least one of potassium hydroxide, acetic acid and sodium acetate; the pH value of steps (1) and (2) is adjusted to a range of 8-14 respectively.
6. The silver-coated copper powder according to claim 1, characterized in that: The amount of silver nitrate used in step (3) is 23-35% of the mass of the copper powder before washing; the mass volume ratio of the silver nitrate to the silver ammonia plating solution system prepared by adding water at last is 2.65:48-52kg / L.
7. The silver-coated copper powder according to claim 1, characterized in that: The complexing agent in step (3) is at least one of ammonia water, ethylenediaminetetraacetic acid, salicylic acid, sodium thiosulfate and sodium cyanide; the amount of the complexing agent is 1.1-3.0 times the theoretical value of the amount required for complexing silver nitrate.
8. The silver-coated copper powder according to claim 1, characterized in that: The volume ratio of the copper system, the reduction system and the silver ammonia plating solution system in step (4) is 8-10:1-2:3-5; and the reaction time is 30min-60min.
9. The silver-coated copper powder according to claim 1, characterized in that: The coating agent in step (5) is at least one of stearic acid, erucic acid, oleic acid, hexadecanoic acid and tetradecanoic acid; the amount of the coating agent is 0.1-1.0% of the mass of the copper powder before washing.
10. The silver-coated copper powder according to claim 1, characterized in that: The temperature during the preparation of the silver-coated copper powder is controlled at 15-45°C.
Citation Information
Patent Citations
Preparation method of silver-copper coating powder
CN102950282B
Silver-coated copper powder and preparation method thereof
CN106148926A
Preparation method of silver-coated copper powder
CN113020587A
Silver-coated copper powder and preparation method thereof
CN115156529B
Cited By
Preparation method of smooth and compact silver-coated copper powder
CN120115713A
Conductive slurry for BC battery and preparation method thereof
CN120708963A
Double-peak copper powder prepared through liquid phase reduction method and technology and application of double-peak copper powder
CN120885702A
Preparation method of silver-coated copper powder
CN121156262A
Silver-coated copper powder and preparation method and application thereof