A calcium silicate-based inorganic coating and preparation method thereof

By combining calcium silicate materials with low hydration activity and high carbonization activity with long-chain alkyl alkoxysilane, and adding inorganic dispersants and polymer emulsions, an efficient inorganic coating is formed, which solves the problem of weak adhesion properties of inorganic coatings. , the problem of poor corrosion resistance, significantly improves its bonding performance and corrosion resistance.

CN116891647BActive Publication Date: 2024-10-18WUHAN UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310948272.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-27
Publication Date
2024-10-18
Estimated Expiration
2043-07-27

AI Technical Summary

Technical Problem

The existing inorganic coatings have weak bonding properties and poor corrosion resistance, which limits their wide application on the surface of building materials.

Method used

Calcium silicate materials with low hydration activity and high carbonization activity are combined with long-chain alkyl alkoxysilane, and an efficient inorganic coating is formed by adding inorganic dispersant, polycarboxylic acid high-efficiency water-reducing agent and polymer emulsion. Improve bonding performance and corrosion resistance.

Benefits of technology

It significantly improves the bonding performance and corrosion resistance of the inorganic coating, enhances the bonding degree with the matrix and weather resistance, and solves the problems of weak bonding performance and poor corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116891647B_ABST
    Figure CN116891647B_ABST
Patent Text Reader

Abstract

The present invention discloses an inorganic coating based on calcium silicate and a preparation method thereof. The raw materials of the inorganic coating based on calcium silicate include: a calcium silicate material and a long-chain alkyl alkoxy silane; wherein the calcium silicate material is at least one of a calcium silicate mineral with low hydration activity and high carbonization activity or an industrial waste residue containing at least 60wt% of a calcium silicate mineral with low hydration activity and high carbonization activity; and the long-chain alkyl alkoxy silane is a long-chain alkyl alkoxy silane with a carbon chain containing 8 to 20 carbons. Based on the advantages of the existing common inorganic coatings such as high mechanical properties and strong weather resistance, the present invention further effectively improves the bonding performance and corrosion resistance of the inorganic coating, and solves the problems of weak bonding performance and poor corrosion resistance of the existing inorganic coatings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic coating materials, and in particular to an inorganic coating based on calcium silicate and a preparation method thereof. Background Art

[0002] Coating materials are mostly used to protect the surface of cement concrete, steel products, and wood, to prevent scratches, decay, rust, cracks, and other defects on the surface of products, and to prevent corrosive substances such as salt ions from penetrating into the interior and causing functional failure. Among the many coating categories, they can be divided into two categories: organic and inorganic according to the raw materials.

[0003] Organic coatings can achieve excellent corrosion resistance and bonding properties, and are more widely used in society. However, most of them release pungent gases during the construction process, and a large amount of organic matter in the coating is not easily degraded by the natural environment, causing an environmental burden, and it is easy to develop peeling and bulging damage, indicating that the stability and weather resistance of organic coatings are poor. Inorganic coatings are mostly made of sodium silicate, calcium silicate, etc. as raw materials. Although they do not have excellent corrosion resistance and bonding properties, they have higher stability, generally have stronger weather resistance, and have strong mechanical properties and are not easy to be damaged. It can be seen that compared with organic coatings, inorganic coatings generally have better mechanical properties and weather resistance than general organic coatings. However, weak bonding properties and poor corrosion resistance make inorganic coatings unable to be widely used.

[0004] Therefore, in order to improve important functions such as the bonding performance between inorganic coatings and substrates, it is necessary to explore effective functional admixtures or improve preparation methods. Summary of the invention

[0005] The purpose of the present invention is to overcome the above technical deficiencies, propose an inorganic coating based on calcium silicate and a preparation method thereof, and solve the technical problems of weak bonding performance and poor corrosion resistance of inorganic coatings in the prior art.

[0006] In a first aspect, the present invention provides an inorganic coating based on calcium silicate, wherein the raw materials of the inorganic coating based on calcium silicate include: a calcium silicate material and a long-chain alkyl alkoxy silane; wherein:

[0007] The calcium silicate material is at least one of a calcium silicate mineral with low hydration activity and high carbonization activity or an industrial waste residue containing at least 60 wt% of a calcium silicate mineral with low hydration activity and high carbonization activity;

[0008] The long-chain alkylalkoxysilane is a long-chain alkylalkoxysilane having a carbon chain of 8 to 20 carbon atoms.

[0009] In a second aspect, the present invention provides a method for preparing an inorganic coating based on calcium silicate, comprising the following steps:

[0010] The calcium silicate material, the inorganic dispersant, the polycarboxylic acid high-efficiency water reducing agent, the polymer emulsion, the long-chain alkyl alkoxy silane and water are uniformly mixed to obtain the inorganic coating based on calcium silicate;

[0011] The calcium silicate-based inorganic coating is applied to the surface of a substrate and carbonized and cured to form a calcium silicate-based inorganic coating.

[0012] Compared with the prior art, the beneficial effects of the present invention include:

[0013] Based on the advantages of existing common inorganic coatings such as high mechanical properties and strong weather resistance, the present invention further effectively improves the bonding performance and corrosion resistance of the inorganic coating, solving the problems of weak bonding performance and poor corrosion resistance of the existing inorganic coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 1 is a graph showing the flowability test results of the inorganic coatings obtained in Example 1 of the present invention and Comparative Examples 1, 3, 4, and 6;

[0015] Figure 2 is a microscopic morphology of the coating formed in Comparative Example 1 of the present invention;

[0016] Figure 3 is a microscopic morphology of the coating formed in Example 1 of the present invention;

[0017] Figure 4 1 is a graph showing the test results of the chloride ion diffusion coefficient (NEL) of the coatings formed in Example 1 of the present invention and Comparative Examples 1, 4 and 7;

[0018] Figure 5 1 is a graph showing the bonding strength test results of the coatings formed by Example 1 of the present invention and Comparative Examples 1, 4 and 7. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0020] In a first aspect, the present invention provides an inorganic coating based on calcium silicate. The raw materials of the inorganic coating based on calcium silicate include: a calcium silicate material and a long-chain alkyl alkoxy silane.

[0021] The present invention adds long-chain alkyl alkoxy silane to the inorganic coating based on calcium silicate, thereby enhancing the bonding degree between the inorganic coating and the substrate, and further improving the bonding performance and anti-corrosion performance of the coating.

[0022] In this embodiment, the long-chain alkyl alkoxysilane is a long-chain alkyl alkoxysilane having a carbon chain of 8 to 20 carbon atoms, for example, it may be one or more of octyltriethoxysilane, octyltrimethoxysilane, dodecyltrimethoxysilane, and the like.

[0023] In this embodiment, the calcium silicate material is at least one of calcium silicate minerals with low hydration activity and high carbonization activity or industrial waste slag containing at least 60wt% of calcium silicate minerals with low hydration activity and high carbonization activity; the calcium silicate mineral with low hydration activity and high carbonization activity is at least one of γ-type dicalcium silicate, monocalcium silicate, and tricalcium disilicate; the industrial waste slag can be a material with low hydration activity and high carbonization activity such as steel slag or magnesium slag.

[0024] In this embodiment, the calcium silicate-based inorganic coating is formed by uniformly mixing raw materials of the calcium silicate-based inorganic coating, coating the raw materials on the surface of the substrate, and then carbonizing and curing the mixture.

[0025] The present invention does not limit the coating method, and those skilled in the art can choose according to actual conditions. For example, spray coating, dip coating, scraper coating, etc. can be used. The inventors found during the experiment that the addition of long-chain alkyl alkoxy silane will increase the viscosity of the slurry. Although it can improve the bonding performance, excessive addition is not conducive to smooth spraying. Therefore, if the spraying method is selected, the amount of long-chain alkyl alkoxy silane added needs to be controlled.

[0026] In some specific embodiments of the present invention, spraying is adopted, and the mass ratio of calcium silicate material to long-chain alkyl alkoxysilane is 1:(0.002-0.04), preferably 1:(0.005-0.02). Within this usage ratio range, a flowing slurry can be formed to ensure smooth spraying process.

[0027] In this embodiment, the raw materials of the above-mentioned calcium silicate-based inorganic coating also include: inorganic dispersant. The present invention can improve the fluidity of the slurry by adding an appropriate amount of inorganic dispersant, making the spraying operation smoother and more fluent, while filling the pores in the coating to make the coating more dense; but excessive addition will lead to reduced fluidity of the coating slurry. Furthermore, the inorganic dispersant is silicon powder. Furthermore, the specific surface area of ​​the microsilica powder is 20,000 to 25,000 m 2 / kg; the dosage ratio of calcium silicate material to inorganic dispersant is 1:(0.01-0.15), further 1:(0.05-0.1).

[0028] In this embodiment, the raw materials of the above-mentioned calcium silicate-based inorganic coating also include: polycarboxylic acid high-efficiency water-reducing agent. The present invention adds polycarboxylic acid high-efficiency water-reducing agent to make the polycarboxylic acid molecules adsorbed together with the calcium silicate particles through electrostatic adsorption. The water film formed by the hydrophilic side chains of the polycarboxylic acid molecules plays a lubricating role, and the long-chain structure of the side chains can provide a steric hindrance effect, improve the agglomeration of powder particles, and improve the fluidity of the slurry. Furthermore, the solid content of the polycarboxylic acid high-efficiency water-reducing agent is 10% to 60%, and further 40% to 50%; the mass ratio of calcium silicate material to polycarboxylic acid high-efficiency water-reducing agent is 1: (0.01 to 0.05).

[0029] In this embodiment, the raw materials of the above-mentioned calcium silicate-based inorganic coating also include: polymer emulsion. The present invention improves the sedimentation and stratification phenomenon in the slurry by adding polymer emulsion. Further, the polymer emulsion is at least one of acrylic emulsion, pure acrylic emulsion, and styrene-butadiene emulsion. Furthermore, the solid content of the polymer emulsion is 40% to 50%; the amount ratio of calcium silicate material to polymer emulsion is 1: (0.005 to 0.025).

[0030] In some preferred embodiments of the present invention, the above-mentioned calcium silicate-based inorganic coating, calculated by weight, comprises raw materials including: 50-70 parts of calcium silicate material, 3-5 parts of inorganic dispersant, 1.5-3 parts of polycarboxylic acid high-efficiency water reducer, 1.0-2.0 parts of polymer emulsion, 0.2-2.0 parts of long-chain alkyl alkoxy silane and 22-28 parts of water.

[0031] In a second aspect, the present invention provides a method for preparing an inorganic coating based on calcium silicate, comprising the following steps:

[0032] S1, mixing calcium silicate material, inorganic dispersant, polycarboxylic acid high-efficiency water reducing agent, polymer emulsion, long-chain alkyl alkoxy silane and water to obtain an inorganic coating based on calcium silicate;

[0033] S2. Applying the above-mentioned calcium silicate-based inorganic coating to the surface of the substrate and carbonizing and curing it to form a calcium silicate-based inorganic coating.

[0034] In this embodiment, the step of uniformly mixing the calcium silicate material, the inorganic dispersant, the polycarboxylic acid high-efficiency water reducer, the polymer emulsion, the long-chain alkyl alkoxy silane and water specifically includes:

[0035] S11, mixing the calcium silicate material and the inorganic dispersant uniformly to obtain a first mixture;

[0036] S12, mixing the polycarboxylate high-efficiency water reducer and water uniformly to obtain a second mixture;

[0037] S13, mixing the first mixture and the second mixture evenly to obtain a third mixture;

[0038] S14, adding the polymer emulsion to the third mixture in batches and mixing evenly to obtain a fourth mixture;

[0039] S15. Add long-chain alkyl alkoxysilane to the fourth mixture and mix evenly to obtain an inorganic coating based on calcium silicate.

[0040] In step S11, the calcium silicate material and the inorganic dispersant are mixed uniformly by stirring; this step is to achieve the purpose of pre-dispersion and make the solid powder more evenly distributed. In some specific embodiments of the present invention, a stirring rod is used to manually stir at a uniform speed for 30 to 60 seconds.

[0041] In step S12, the polycarboxylate superplasticizer and water are mixed uniformly by stirring; this step is to make the polycarboxylate superplasticizer disperse uniformly in the water. In some specific embodiments of the present invention, a stirring rod is used to manually stir at a uniform speed for 5 to 10 seconds.

[0042] In step S13, the first mixture and the second mixture are mixed evenly by stirring; the stirring process is to make the solid particles fully dispersed and fully mixed with the liquid.

[0043] In step S14, the polymer emulsion is added to the third mixture in batches and mixed evenly by stirring. This step is to destroy the emulsion network structure and improve fluidity by long-term high-speed whipping to prevent the slurry from losing fluidity after adding long-chain alkyl alkoxysilane. In some specific embodiments of the present invention, a hand-held stirrer is used with a stirring speed of 100 to 150 r / min, no more than 1.0 g of emulsion is added each time, and the stirring time after each addition is not less than 30 s.

[0044] In step S15, long-chain alkyl alkoxy silane is added to the fourth mixture and mixed evenly by stirring. This step is to fully mix the fourth mixture with the long-chain alkyl alkoxy silane. In some specific embodiments of the present invention, a hand-held stirrer is used, the stirring speed is 100 to 150 r / min, and the stirring time is not less than 30 s.

[0045] The present invention does not limit the type of substrate, and those skilled in the art can select according to actual conditions. For example, the inorganic coating of the present invention can act on the surface of most building materials such as cement concrete substrate, steel substrate, wood substrate, etc.

[0046] In this embodiment, the carbonization curing conditions are: carbonization temperature of 0-50° C., relative humidity of 10-70%, carbon dioxide volume concentration of 60%-99.8%, relative partial pressure of 0-0.3 MPa, and curing time ≥12 h.

[0047] In some specific embodiments of the present invention, the carbonization curing conditions are: carbonization temperature of 10-50° C., relative humidity of 50-70%, carbon dioxide volume concentration of 60%-99.8%, relative partial pressure of 0.1-0.3 MPa, and curing time of 18-36 h.

[0048] Example 1

[0049] This embodiment provides a method for preparing an inorganic coating based on calcium silicate, comprising the following steps:

[0050] (1) Mix 65g of dicalcium silicate and 5g of microsilica powder into a uniform powder;

[0051] (2) 1.8 g of polycarboxylic acid high-efficiency water reducer (solid content 40%) and 28 g of water were prepared into a uniform solution and poured into the powder, and stirred at a speed of 100 r / min for 30 s;

[0052] (3) Add 1.5 g acrylic emulsion (solid content 45%) twice and stir evenly;

[0053] (4) adding 1.0 g of octyltriethoxysilane and continuing to stir at a speed of 120 r / min for 60 s to obtain a coating;

[0054] (5) Use a pneumatic spray gun to evenly spray the coating onto the surface of the cement concrete substrate, and place it in a carbonation curing container for carbonation curing in a carbon dioxide atmosphere with a carbon dioxide concentration of 95%, a carbonation relative partial pressure of 0.1 MPa, a temperature of 25°C, and a relative humidity of 60% for 24 hours.

[0055] Example 2

[0056] This embodiment provides a method for preparing an inorganic coating based on calcium silicate, comprising the following steps:

[0057] (1) Mix 50g of dicalcium silicate and 3g of microsilica powder into a uniform powder;

[0058] (2) 1.5 g of polycarboxylic acid high-efficiency water reducer (solid content 40%) and 22 g of water were prepared into a uniform solution and poured into the powder, and stirred at a speed of 100 r / min for 30 s;

[0059] (3) Add 1 g of acrylic emulsion (solid content 45%) twice and stir evenly;

[0060] (4) adding 0.3 g of octyltrimethoxysilane and continuing to stir at a speed of 120 r / min for 60 s to obtain a coating;

[0061] (5) Use a pneumatic spray gun to evenly spray the coating onto the surface of the wood substrate, and place the wood substrate in a carbonization curing container for carbonization curing in a carbon dioxide atmosphere with a carbon dioxide concentration of 60%, a carbonization relative partial pressure of 0.3 MPa, a temperature of 50°C, and a relative humidity of 50% for 18 hours.

[0062] Example 3

[0063] This embodiment provides a method for preparing an inorganic coating based on calcium silicate, comprising the following steps:

[0064] (1) Mix 70 g of steel slag and 4 g of microsilica powder into a uniform powder;

[0065] (2) Prepare a uniform solution of 3 g polycarboxylic acid high-efficiency water reducer (solid content 40%) and 25 g water, pour it into the powder, and stir at a speed of 100 r / min for 30 s;

[0066] (3) Add 1.6 g of acrylic emulsion (solid content 45%) in two portions and stir evenly;

[0067] (4) adding 1.5 g of dodecyltrimethoxysilane and continuing to stir at a speed of 120 r / min for 60 s to obtain a coating;

[0068] (5) Use a pneumatic spray gun to evenly spray the coating onto the surface of the wood substrate, and place the wood substrate in a carbonization curing container for carbonization curing in a carbon dioxide atmosphere with a carbon dioxide concentration of 80%, a carbonization relative partial pressure of 0.2 MPa, a temperature of 30°C, and a relative humidity of 70% for 36 hours.

[0069] Comparative Example 1

[0070] The only difference between Comparative Example 1 and Example 1 is that, during the preparation of the inorganic coating of Comparative Example 1, no octyltriethoxysilane was added.

[0071] Comparative Example 2

[0072] The only difference between Comparative Example 2 and Example 1 is that, during the preparation of the inorganic coating of Comparative Example 2, the dosage of octyltriethoxysilane is 3.0 g.

[0073] Comparative Example 3

[0074] The only difference between Comparative Example 3 and Example 1 is that during the preparation of the inorganic coating of Comparative Example 3, no silicon micropowder was added.

[0075] Comparative Example 4

[0076] The only difference between Comparative Example 4 and Example 1 is that no acrylic emulsion is added during the preparation of the inorganic coating of Comparative Example 4.

[0077] Comparative Example 5

[0078] The only difference between Comparative Example 5 and Example 1 is that during the preparation of the inorganic coating of Comparative Example 5, the amount of acrylic emulsion added is 2.0 g.

[0079] Comparative Example 6

[0080] The difference between Comparative Example 6 and Example 1 is that the preparation process of the inorganic coating is different; the details are as follows:

[0081] (1) Mix 65g of dicalcium silicate and 5g of microsilica powder into a uniform powder;

[0082] (2) 1.8 g of polycarboxylic acid high-efficiency water reducer (solid content 40%) and 28 g of water were prepared into a uniform solution and poured into the powder, and stirred at a speed of 100 r / min for 30 s;

[0083] (3) Add 1.5 g of acrylic emulsion (solid content 45%) and 1.0 g of octyltriethoxysilane, and continue stirring at a speed of 120 r / min for about 120 s until a uniformly dispersed coating is obtained.

[0084] Comparative Example 7

[0085] The only difference between Comparative Example 7 and Example 1 is that the carbonization time of Comparative Example 7 is 6 hours under a carbonization curing environment with a carbon dioxide concentration of 95%, a carbonization relative partial pressure of 0.1 MPa, a temperature of 25° C., and a relative humidity of 60%.

[0086] Experimental Group 1

[0087] The inorganic coatings obtained in Example 1 and Comparative Examples 1 to 6 were tested for their fluidity properties ( Figure 1 ) and sedimentation phenomenon observation (Table 1). Among them, the viscosity of the slurry was tested by rheometer to determine its excellent fluidity; the slurry state of the coating was observed after 48 hours to determine its storage stability at room temperature.

[0088] Among them, Comparative Examples 2 and 5 could not form a flowing slurry, so no performance test was conducted; Comparative Examples 3 and 6 could not form a slurry with good fluidity and were not suitable for spraying operations, so subsequent durability and bonding strength related tests were not conducted.

[0089] Table 1

[0090] Group Slurry state after sealing and standing for 48 hours at room temperature Example 1 No solid-liquid separation Comparative Example 1 No solid-liquid separation Comparative Example 2 \ Comparative Example 3 No solid-liquid separation Comparative Example 4 Solid-liquid separation occurs Comparative Example 5 \ Comparative Example 6 No solid-liquid separation

[0091] pass Figure 1 It can be seen from Table 1 that the coating formed in Example 1 of the present invention has good comprehensive properties, and has both good fluidity and storage stability at room temperature.

[0092] Experimental Group 2

[0093] The coatings obtained in Example 1 and Comparative Example 1 were subjected to microstructural observation.

[0094] During the carbonization curing process, the calcium silicate material precipitates calcium ions in the solution environment, and the carbonate ions provided by the dissolved carbon dioxide react with the calcium ions to form calcium carbonate, which provides the main mechanical properties for the inorganic coating of the present invention. Figure 2 and Figure 3 The calcium carbonate morphology of the coating was found to be that the addition of long-chain alkyl alkoxysilane would guide the calcium carbonate to develop into a typical calcite crystal morphology. The long-chain alkyl alkoxysilane in the present invention can be catalyzed under alkaline conditions formed by the hydrolysis of calcium silicate. The alkoxy group at one end automatically hydrolyzes to generate active silanol groups, which condense with the hydroxyl groups on the surface of calcium carbonate and calcium silicate to form chemical bonds, while the long-chain alkyl group at the other end of the molecular chain is oriented on the surface of the material to form a hydrophobic layer. It is speculated that this phenomenon will cause the calcium ion dissolution process of calcium silicate to be slowed down, the supersaturation value in the solution to be reduced, and the calcite crystal form to be formed. And because the alkoxy group will also form a chemical bond on the surface of calcium carbonate, the surface of the generated calcium carbonate is hydrophobic, which makes the coating have better corrosion resistance.

[0095] Experimental Group 3

[0096] The coatings obtained in the above-mentioned Example 1, Comparative Example 1, Comparative Example 4 and Comparative Example 7 were subjected to durability tests, and the standards are as follows:

[0097] Chloride ion corrosion resistance test: JCT 1086-2008.

[0098] pass Figure 4 It can be seen that compared with Comparative Examples 1, 4 and 7, Example 1 has stronger resistance to chloride ion corrosion, which means that this method is beneficial to the durability of the enhanced coating and can significantly improve the coating's resistance to chloride ion corrosion, but requires a certain carbonization curing time to obtain a coating structure with complete performance.

[0099] Experimental Group 4

[0100] The coatings obtained in the above-mentioned Example 1, Comparative Example 1, Comparative Example 4 and Comparative Example 7 were tested for bonding strength.

[0101] pass Figure 5 It can be seen that compared with Comparative Example 1, Example 1 can significantly improve the bonding degree between the inorganic coating and the substrate, and the bonding strength is increased by 50%. The reason may be that calcite calcium carbonate has a high hardness (H M =3), which can enhance the mechanical properties of the coating; at the same time, the chemical bonding between the long-chain alkyl alkoxy silane and the substrate surface helps to improve the bonding performance.

[0102] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. An inorganic coating based on calcium silicate, characterized in that The raw materials include, by weight: 50-70 parts of calcium silicate material, 3-5 parts of inorganic dispersant, 1.5-3 parts of polycarboxylic acid high-efficiency water reducing agent, 1.0-2.0 parts of polymer emulsion, 0.2-2.0 parts of long-chain alkyl alkoxy silane and 22-28 parts of water; wherein, The calcium silicate material is at least one of a calcium silicate mineral with low hydration activity and high carbonization activity or an industrial waste residue containing at least 60wt% of a calcium silicate mineral with low hydration activity and high carbonization activity; the calcium silicate mineral with low hydration activity and high carbonization activity is at least one of γ-type dicalcium silicate, monocalcium silicate, and tricalcium disilicate; The long-chain alkyl alkoxy silane is a long-chain alkyl alkoxy silane having a carbon chain containing 8 to 20 carbons; The inorganic dispersant is silicon powder; The polymer emulsion is at least one of acrylic emulsion, pure acrylic emulsion and styrene-butadiene emulsion; The calcium silicate-based inorganic coating is formed by uniformly mixing the raw materials of the calcium silicate-based inorganic coating, coating the raw materials on the surface of the substrate, and performing carbonization curing.

2. The inorganic coating based on calcium silicate according to claim 1, characterized in that The long-chain alkyl alkoxysilane is one or more of octyltriethoxysilane, octyltrimethoxysilane and dodecyltrimethoxysilane.

3. The inorganic coating based on calcium silicate according to claim 1, characterized in that The solid content of the polycarboxylic acid high-efficiency water reducing agent is 10% to 60%, and the solid content of the polymer emulsion is 40% to 50%.

4. A method for preparing an inorganic coating based on calcium silicate as claimed in claim 1, characterized in that: The following steps are involved: The calcium silicate material, the inorganic dispersant, the polycarboxylic acid high-efficiency water reducing agent, the polymer emulsion, the long-chain alkyl alkoxy silane and water are uniformly mixed to obtain an inorganic coating based on calcium silicate; The calcium silicate-based inorganic coating is applied to the surface of a substrate and carbonized and cured to form a calcium silicate-based inorganic coating.

5. The method for preparing the inorganic coating based on calcium silicate according to claim 4, characterized in that: The step of uniformly mixing the calcium silicate material, the inorganic dispersant, the polycarboxylic acid high-efficiency water reducing agent, the polymer emulsion, the long-chain alkyl alkoxy silane and water specifically comprises: Mixing the calcium silicate material and the inorganic dispersant uniformly to obtain a first mixture; Mixing the polycarboxylate high-efficiency water reducer and water uniformly to obtain a second mixture; Mixing the first mixture and the second mixture evenly to obtain a third mixture; Adding polymer emulsion to the third mixture in batches and mixing evenly to obtain a fourth mixture; Add long-chain alkyl alkoxysilane to the fourth mixture and mix well to obtain a calcium silicate-based inorganic coating.

6. The method for preparing the inorganic coating based on calcium silicate according to claim 4, characterized in that: The coating method is one of spraying, dipping or scraping.

7. The method for preparing the inorganic coating based on calcium silicate according to claim 4, characterized in that: The carbonization curing conditions are as follows: carbonization temperature of 0-50° C., relative humidity of 10-70%, carbon dioxide volume concentration of 60%-99.8%, relative partial pressure of 0-0.3 MPa, and curing time of ≥12 h.

Citation Information

Patent Citations

  • Hydrophobic finish compositions with extended flow time retention and building products made thereof

    CN107406688A

  • Low-wettability high-durability composite Portland cement and preparation method thereof

    CN112624688A

  • Calcium carbonate-based inorganic coating and preparation method and use method thereof

    CN112897966A