A preparation method of powder control scraper

By adding functional coatings to the metal powder control squeegee, the problem of difficulty in adjusting the developer thickness, uniformity and charge amount of the existing squeegee is solved, achieving higher product qualification rate and functionality, and adapting to laser High performance requirements for imaging office equipment.

CN116891676BActive Publication Date: 2024-10-25ZHU HAI YOU TAI HUA GONG YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310859454.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-13
Publication Date
2024-10-25
Estimated Expiration
2043-07-13

AI Technical Summary

Technical Problem

The existing metal powder control scraper has performance limitations in controlling the thickness, uniformity and charge of the developer. It is especially difficult to adjust developers with small particle sizes, resulting in poor product versatility and inability to meet the needs of miniaturization and high-speed laser imaging office equipment. The development trend of chemicalization and long service life.

Method used

Add a uniform layer of functional coating on the stainless steel sheet of the metal powder control scraper. The coating is composed of polyurethane resin, fluorine-modified polyester resin, isocyanate curing agent, etc., and is applied by spraying, dipping or brushing, and Pre-dried at 60-80℃ and then solidified to enhance the frictional electrification, wear resistance and lubricity of the scraper.

Benefits of technology

It improves the qualification rate and functionality of the product, enhances the wear resistance, lubrication and stain resistance of the scraper, meets the customer's multi-functional requirements, improves printing blackness and uniformity, and adapts to laser imaging office equipment high performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004337131720000051
    Figure BDA0004337131720000051
Patent Text Reader

Abstract

The present invention belongs to the field of forming technology of laser imaging office equipment parts, and specifically relates to a method for preparing a powder control scraper. The method for preparing a powder control scraper provided by the present invention comprises the following steps: S1 scraper processing; S2 cleaning the scraper obtained in step S1; S3 preparing the coating according to the formula requirements; S4 uniformly coating the coating prepared in step S3 on the working position of the scraper cleaned in step S2 to obtain a coated product; S5 first pre-drying the coated product obtained in step S4 in an oven at 60-80°C, the pre-drying time is 10-25 minutes, and then curing at 80-130°C, and the curing time is 15-30 minutes. Through the method for preparing a powder control scraper provided by the present invention, the qualified rate of the prepared product is high, and the functionality of the product is increased, so that it has good triboelectric charging, wear resistance, lubricity, anti-fouling and other functions, does not stick toner, and improves the printing blackness and uniformity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of forming parts of laser imaging office equipment, and in particular relates to a method for preparing a powder control scraper. Background Art

[0002] The function of the powder control scraper of laser imaging office equipment is to control the thickness and uniformity of the developer layer on the developer and the friction charge. Powder control scrapers are generally divided into two types: metal powder control scrapers acting on elastic developer components and non-metal powder control scrapers acting on rigid developer components. Metal powder control scrapers are mainly made of metal brackets and stainless steel sheets welded or riveted.

[0003] Ordinary metal powder control scrapers can only determine their ability to control the thickness, uniformity and charge of the developer through the properties of their own materials. Due to the constraints of the raw materials themselves and the processing technology, the surface properties of stainless steel sheets are difficult to adjust, especially for the thickness and charge of small-particle developers. At present, various toner cartridges on the market have different requirements for scrapers, resulting in poor product versatility and difficulties for manufacturers to develop supporting products. Especially now that laser imaging office equipment is showing a trend of miniaturization, high speed and long service life, the adaptability requirements for scrapers are getting higher and higher. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a powder control scraper. After the metal powder control scraper is processed, a uniform functional coating is added on the stainless steel sheet, so that the qualified rate of the prepared product is high, and the functionality of the product is increased, so that it has good triboelectric charging, wear resistance, lubricity and other functions.

[0005] The technical solution adopted by the present invention to solve the above technical problems is:

[0006] A method for preparing a powder control scraper comprises the following steps:

[0007] S1 Scraper processing: Weld or rivet the steel sheets punched out according to size onto the metal bracket to obtain the scraper;

[0008] S2: cleaning the scraper obtained in step S1 to remove impurities and oil stains on the scraper surface;

[0009] S3 prepares the coating according to the formula requirements;

[0010] S4 uniformly coating the coating prepared in step S3 on the working position of the scraper cleaned in step S2 to obtain a coated product;

[0011] S5: firstly put the coated product obtained in step S4 into an oven at 60-80°C for pre-drying for 10-25 minutes, and then cure it at 80-130°C for 15-30 minutes.

[0012] Furthermore, the coating method in step S4 is spraying, dipping or brushing.

[0013] Furthermore, the pre-drying time in step S5 is 15-20 minutes.

[0014] Furthermore, the curing time in step S5 is 20-25 minutes.

[0015] Furthermore, the coating in step S3 includes the following components and their weight percentages:

[0016] Polyurethane resin 10-30%, fluorine-modified polyester resin 10-20%, isocyanate curing agent 5-10%, ester / ketone solvent 50-80%, conductive carbon black or graphite 3-8%, dispersant 0.5-1.5% and silicone leveling agent 0.2-1.5%.

[0017] Furthermore, the dispersant is an ethylene oxide / propylene oxide copolymer.

[0018] In the present invention, the coating is prepared from polyurethane resin, fluorine-modified polyester resin and isocyanate curing agent, etc. The present invention adds a uniform functional coating layer on the stainless steel sheet after the metal powder control scraper is processed, so that the product has a high qualified rate and the functionality of the product is increased, so that it has good triboelectric charging, wear resistance and lubricity.

[0019] Compared with the prior art, the preparation method of the powder control scraper provided by the present invention has the following advantages:

[0020] (1) The preparation method of the powder control scraper provided by the present invention is simple and easy to industrialize.

[0021] (2) The product prepared by the preparation method of the powder control scraper provided by the present invention has strong functionality. The functionality of the original powder control scraper does not meet customer requirements due to the limitation of its own materials. In particular, for some small-particle developer products, ordinary metal powder control scrapers will have powder bleaching phenomenon. The method provided by the present invention can maintain the physical properties of the stainless steel sheet itself, while giving the stainless steel sheet a new functional surface, such as improving friction charging, wear resistance, lubricity, anti-fouling, etc., and improving printing blackness and uniformity, which can meet or even exceed a series of functional requirements of customers.

[0022] (3) The qualified rate of the products prepared by the method for preparing the powder control scraper provided by the present invention is high. The original stainless steel sheet will have more or less surface defects during the processing, and these defects will cause abnormalities on the photocopy surface. However, the method provided by the present invention can compensate for the defective positions of the stainless steel sheet through coating, providing better quality assurance for the product. DETAILED DESCRIPTION

[0023] The present invention is further illustrated below through the description of specific implementation modes, but this is not a limitation of the present invention. Those skilled in the art can make various modifications or improvements based on the basic idea of ​​the present invention, but as long as they do not deviate from the basic idea of ​​the present invention, they are all within the scope of the present invention.

[0024] Unless otherwise specified, the materials and reagents used in the examples of the present invention are commercially available.

[0025] Example 1: A method for preparing a powder control scraper

[0026] The preparation method of the powder control scraper comprises the following steps:

[0027] S1 Scraper processing: Weld or rivet the steel sheets punched out according to size onto the metal bracket to obtain the scraper;

[0028] S2: cleaning the scraper obtained in step S1 to remove impurities and oil stains on the scraper surface;

[0029] S3 prepares the coating according to the formula requirements;

[0030] S4: uniformly coating the coating prepared in step S3 on the working position of the scraper cleaned in step S2, by spraying, to obtain a coated product;

[0031] S5: firstly put the coated product obtained in step S4 into an oven at 60°C for pre-drying for 10 minutes, and then cure it at 80°C for 15 minutes.

[0032] The coating in step S3 is composed of the following components and their weight percentages:

[0033] 10% polyurethane resin, 10% fluorine-modified polyester resin, 5% isocyanate curing agent, 71.3% 1,2-propylene glycol diacetate, 3% conductive carbon black, 0.5% dispersant and 0.2% organosilicon leveling agent; the dispersant is ethylene oxide / propylene oxide copolymer.

[0034] Example 2: A method for preparing a powder control scraper

[0035] The preparation method of the powder control scraper comprises the following steps:

[0036] S1 Scraper processing: Weld or rivet the steel sheets punched out according to size onto the metal bracket to obtain the scraper;

[0037] S2: cleaning the scraper obtained in step S1 to remove impurities and oil stains on the scraper surface;

[0038] S3 prepares the coating according to the formula requirements;

[0039] S4: uniformly coating the coating prepared in step S3 on the working position of the scraper cleaned in step S2, by dipping, to obtain a coated product;

[0040] S5: firstly put the coated product obtained in step S4 into an oven at 80°C for pre-drying for 25 minutes, and then cure it at 130°C for 30 minutes.

[0041] The coating in step S3 is composed of the following components and their weight percentages:

[0042] 15% of polyurethane resin, 14% of fluorine-modified polyester resin, 10% of isocyanate curing agent, 50% of acetone, 8% of graphite, 1.5% of dispersant and 1.5% of organic silicon leveling agent; the dispersant is ethylene oxide / propylene oxide copolymer.

[0043] Embodiment 3, a method for preparing a powder control scraper

[0044] The preparation method of the powder control scraper comprises the following steps:

[0045] S1 Scraper processing: Weld or rivet the steel sheets punched out according to size onto the metal bracket to obtain the scraper;

[0046] S2: cleaning the scraper obtained in step S1 to remove impurities and oil stains on the scraper surface;

[0047] S3 prepares the coating according to the formula requirements;

[0048] S4: uniformly coating the coating prepared in step S3 on the working position of the scraper cleaned in step S2 by brushing to obtain a coated product;

[0049] S5: firstly put the coated product obtained in step S4 into an oven at 70°C for pre-drying for 15 minutes, and then cure it at 90°C for 20 minutes.

[0050] The coating in step S3 is composed of the following components and their weight percentages:

[0051] 30% of polyurethane resin, 10% of fluorine-modified polyester resin, 5% of isocyanate curing agent, 51.3% of 3-ethoxyethyl propionate, 3% of conductive carbon black, 0.5% of dispersant and 0.2% of organic silicon leveling agent; the dispersant is ethylene oxide / propylene oxide copolymer.

[0052] Embodiment 4: A method for preparing a powder control scraper

[0053] The preparation method of the powder control scraper comprises the following steps:

[0054] S1 Scraper processing: Weld or rivet the steel sheets punched out according to size onto the metal bracket to obtain the scraper;

[0055] S2: cleaning the scraper obtained in step S1 to remove impurities and oil stains on the scraper surface;

[0056] S3 prepares the coating according to the formula requirements;

[0057] S4: uniformly coating the coating prepared in step S3 on the working position of the scraper cleaned in step S2, wherein the coating method is spraying to obtain a coated product;

[0058] S5: firstly put the coated product obtained in step S4 into an oven at 70°C for pre-drying for 20 minutes, and then cure it at 120°C for 25 minutes.

[0059] The coating in step S3 is composed of the following components and their weight percentages:

[0060] 10% of polyurethane resin, 20% of fluorine-modified polyester resin, 5% of isocyanate curing agent, 58.5% of isophorone, 5% of graphite, 1% of dispersant and 0.5% of organic silicon leveling agent; the dispersant is ethylene oxide / propylene oxide copolymer.

[0061] Test Example 1: Scraper Wear Test

[0062] 1. Test materials: scrapers prepared in Example 1, Example 2, Example 3, and Example 4.

[0063] 2. Test method: Carry out abrasion test in accordance with the industry standard JB / T10934-2010 "Technical requirements for cleaning scrapers for photoconductive drums of digital copiers and laser printers".

[0064] 3. Test results

[0065] The test results are shown in Table 1.

[0066] Table 1: Scraper wear test results

[0067]

[0068] The wear value is measured by marking the Shore hardness. The standard wear value indicates the wear amount of the scraper without a coating layer under different hardness indicators. The percentage value indicates the percentage of the weight difference of the product before and after the test to the weight of the product before the test. It can be seen from Table 1 that the scrapers prepared in Example 1, Example 2, Example 3, and Example 4 of the present invention all meet the industry standards, and their wear values ​​are much lower than the standard values, which shows that the scraper prepared by the preparation method of the powder-controlled scraper provided by the present invention can play a good wear-resistant role. In addition, the scraper prepared by the preparation method of the powder-controlled scraper provided by the present invention has good friction charging and lubricity and other functions.

[0069] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and the specification only describe the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which shall fall within the scope of the invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a powder control scraper, characterized in that: The following steps are involved: S1 Scraper processing: Weld or rivet the steel sheets punched out according to size onto the metal bracket to obtain the scraper; S2: cleaning the scraper obtained in step S1 to remove impurities and oil stains on the scraper surface; S3 prepares the coating according to the formula requirements; S4: uniformly coating the coating prepared in step S3 on the working position of the scraper cleaned in step S2 by brushing to obtain a coated product; S5: pre-drying the coated product obtained in step S4 in an oven at 70°C for 15 minutes, and then curing at 90°C for 20 minutes; The coating in step S3 is composed of the following components and their weight percentages: 30% of polyurethane resin, 10% of fluorine-modified polyester resin, 5% of isocyanate curing agent, 51.3% of 3-ethoxyethyl propionate, 3% of conductive carbon black, 0.5% of dispersant and 0.2% of organic silicon leveling agent; the dispersant is ethylene oxide / propylene oxide copolymer.