A P-type ZrCoSb-based semi-Hassler single-crystal alloy and its preparation method
By doping Sn into ZrCoSb-based alloys and employing magnetic levitation melting and vertical Bridgman directional crystallization techniques, a P-type ZrCoSb1-xSnx semi-Hassler single-crystal alloy was prepared, which solved the problem of low carrier mobility and optimized electrical transport performance.
Patent Information
- Application Number
- CN202310636461.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-05-31
AI Technical Summary
The low carrier mobility of existing P-type ZrCoSb-based alloys limits further optimization of their thermoelectric properties. Grain boundaries are the main scattering centers of carriers in polycrystalline alloys, and existing research is mostly based on polycrystalline alloys.
By doping Sn into ZrCoSb-based alloys, P-type ZrCoSb1-xSnx semi-Hassler single crystal alloys were prepared. Magnetic levitation melting and vertical Bridgman directional crystallization techniques were used to eliminate the negative impact of grain boundaries on charge carriers, forming a MgAgAs-type crystal structure.
By increasing carrier concentration and mobility and optimizing electrical transport parameters such as conductivity, Seebeck coefficient and power factor, the electrical transport performance of P-type ZrCoSb-based single crystal alloys was improved.
Smart Images

Figure CN116905091B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field, and more particularly to a P-type ZrCoSb-based semi-Hassler single-crystal alloy and its preparation method. Background Technology
[0002] ZrCoSb semi-Hassler alloys are excellent medium- and high-temperature thermoelectric alloys, and their thermoelectric properties have been greatly developed and optimized. However, compared with N-type ZrCoSb-based alloys, the lower carrier mobility hinders further optimization of the thermoelectric properties of P-type ZrCoSb-based alloys. For polycrystalline thermoelectric alloys, grain boundaries are one of the main carrier scattering centers. Although researchers have optimized their carrier mobility through a series of modulation strategies, most of these studies have been based on polycrystalline alloys. Summary of the Invention
[0003] In view of this, the present invention provides a P-type semi-Hassler single crystal alloy and its preparation method, and the P-type semi-Hassler single crystal alloy provided by the present invention has excellent electrical transport properties.
[0004] To achieve the above-mentioned objective, the present invention provides a P-type ZrCoSb-based semi-Hassler single crystal alloy, wherein the chemical composition of the P-type ZrCoSb-based semi-Hassler single crystal alloy is ZrCoSb1-xSnx. In the ZrCoSb1-xSnx, the value range of x is 0.1≤x≤0.3; The P-type ZrCoSb-based semi-Hassler single-crystal alloy has a MgAgAs-type crystal structure.
[0005] Preferably, the value of x is 0.16, 0.20 or 0.24.
[0006] This invention also provides a method for preparing the aforementioned P-type ZrCoSb-based semi-Hassler single-crystal alloy, comprising the following steps: Corresponding to the chemical element composition of the ZrCoSb-based semi-Hassler single crystal alloy, the alloy raw materials were melted under a protective atmosphere to obtain a semi-Hassler polycrystalline alloy ingot. The semi-Hassler polycrystalline alloy ingot was subjected to vertical Bridgman orientation crystallization under a protective atmosphere to obtain the P-type ZrCoSb-based semi-Hassler single-crystal alloy.
[0007] Preferably, the melting is magnetic levitation melting; the melting process involves heating the raw material to a molten state and holding it at that temperature for 30-45 seconds; the melting process is repeated 3-5 times.
[0008] Preferably, the vertical Bridgeman oriented crystallization includes the following steps: The semi-Hasler polycrystalline alloy ingot is placed in a crucible and heated to the melting temperature under a protective atmosphere. The alloy molten material is obtained in the crucible by chemical treatment. Using the crucible as a reference, the crystallization furnace chamber is raised along the crucible to allow the alloy to melt and undergo directional crystallization; The rising rate of the crystallization furnace is 0.3~2 mm / h.
[0009] Preferably, the process of heating to the material melting temperature is as follows: The material is heated to a first temperature at a first heating rate, and then heated to a melting temperature at a second heating rate. The first heating rate is 10~15℃ / min, and the first temperature is 1000℃; The second heating rate is 2~5℃ / min, and the material temperature is 1560~1600℃.
[0010] Preferably, the heat preservation time of the chemical is 3 to 6 hours.
[0011] Preferably, during the vertical Bridgman orientation crystallization, the temperature change inside the crucible is as follows: the temperature of the reactant decreases at a rate of 2~5℃ / min to 1510~1550℃.
[0012] Preferably, the pressure of the vertical Bridgman oriented crystallization is 112,000 to 130,000 Pa.
[0013] Preferably, after the vertical Bridgeman orientation crystallization, the product after orientation crystallization is further cooled. The cooling process is as follows: the temperature is reduced to a first cooling temperature at a first cooling rate, and then increased to room temperature at a second cooling rate; The first cooling rate is 2~5℃ / min, and the first cooling temperature is 1000~1200℃; the second cooling rate is 10~25℃ / min.
[0014] This invention provides a P-type semi-Hassler single-crystal alloy, wherein the chemical composition of the P-type ZrCoSb-based semi-Hassler single-crystal alloy is ZrCoSb1-xSnx; the value of x in ZrCoSb1-xSnx ranges from 0.1 to x ≤ 0.3; and the P-type ZrCoSb-based semi-Hassler single-crystal alloy has a MgAgAs type crystal structure. This invention introduces additional holes by doping Sn at Sb sites, thereby increasing the carrier concentration. Furthermore, the P-type ZrCoSb1-xSnx single-crystal alloy obtained by this invention eliminates the negative impact of grain boundaries on carrier transport. Based on the optimization of carrier mobility and carrier concentration, the electrical transport parameters conductivity, Seebeck coefficient, and power factor are optimized. Attached Figure Description
[0015] Figure 1 shows the XRD patterns of the ZrCoSb-based semi-Hassler single-crystal alloys prepared in Examples 1-3; Figure 2 is a SEM image of the ZrCoSb-based semi-Hassler single-crystal alloy prepared in Example 2; Figure 3 shows the electrical conductivity of the ZrCoSb-based semi-Hassler single-crystal alloys prepared in Examples 1-3; Figure 4 shows the Seebeck coefficient of the ZrCoSb-based semi-Hassler single-crystal alloys prepared in Examples 1-3; Figure 5 shows the power factor diagrams of the ZrCoSb-based semi-Hassler single-crystal alloys in Examples 1-3. Detailed Implementation
[0016] This invention provides a P-type ZrCoSb-based semi-Hassler single crystal alloy, wherein the chemical composition of the P-type ZrCoSb-based semi-Hassler single crystal alloy is ZrCoSb1-xSnx; In the ZrCoSb1-xSnx, the value range of x is 0.1≤x≤0.3; The P-type ZrCoSb-based semi-Hassler single-crystal alloy has a MgAgAs-type crystal structure.
[0017] In this invention, the value range of x in ZrCoSb1-xSnx is 0≤x≤0.25, preferably 0.15≤x≤0.25, and more preferably 0.16, 0.20 or 0.24.
[0018] In this invention, the preferred crystal structure of the P-type ZrCoSb-based semi-Hassler single-crystal alloy is a MgAgAs type crystal structure with space group [missing information]. F -43m.
[0019] This invention also provides a method for preparing the above-described P-type ZrCoSb-based semi-Hassler single-crystal alloy, comprising the following steps: Corresponding to the chemical element composition of the ZrCoSb-based semi-Hassler single crystal alloy, the alloy raw materials were melted under a protective atmosphere to obtain a semi-Hassler polycrystalline alloy ingot. The semi-Hassler polycrystalline alloy ingot was subjected to vertical Bridgman orientation crystallization under a protective atmosphere to obtain the P-type ZrCoSb-based semi-Hassler single-crystal alloy.
[0020] In this invention, the alloy raw material includes Zr particles, Co particles, Sb particles, and Sn particles, and the particle sizes of the Zr particles, Co particles, Sb particles, and Sn particles are preferably independently determined. 2*3mm 3*3mm, 2-6mm (quasi-spherical) 2*5mm. In this invention, the purity of the Zr particles, Co particles, Sb particles and Sn particles is preferably 99.5%, 99.95%, 99.99%, and 99.95%, respectively.
[0021] In this invention, the melting process is preferably magnetic levitation melting. The melting process is preferably performed by heating the raw material to a molten state and holding it at that temperature for 30-45 seconds, more preferably 40 seconds. The protective atmosphere is preferably high-purity argon, with a purity preferably ≥99.99%. The melting process is preferably performed ≥3-5 times, more preferably 3-4 times. The melting process is preferably carried out in a magnetic levitation induction furnace.
[0022] In this invention, after obtaining the semi-Hasler polycrystalline alloy ingot and before performing vertical Bridgeman oriented crystallization, it is preferable to further crush the semi-Hasler polycrystalline alloy ingot.
[0023] In this invention, the crushing is preferably performed to a thickness of approximately 1 mm. This invention does not impose any special limitations on the specific implementation of the crushing process; operations familiar to those skilled in the art can be used.
[0024] After obtaining the semi-Hasler polycrystalline alloy ingot, the present invention performs vertical Bridgman oriented crystallization on the semi-Hasler polycrystalline alloy ingot under a protective atmosphere to obtain the P-type ZrCoSb-based semi-Hasler single crystal alloy.
[0025] In this invention, the vertical Bridgman orientation crystallization includes the following steps: The semi-Hasler polycrystalline alloy ingot is placed in a crucible and heated to the melting temperature under a protective atmosphere to obtain the alloy molten material. Using the crucible as a reference, the crystallization furnace chamber is raised along the crucible to allow the alloy to melt and undergo directional crystallization.
[0026] This invention involves placing a semi-Hasler polycrystalline alloy ingot in a crucible and, under a protective atmosphere, heating it to the melting temperature to obtain a molten alloy.
[0027] In this invention, the process of heating to the material melting temperature is preferably as follows: The material is heated to a first temperature at a first heating rate, and then heated to a melting temperature at a second heating rate. In this invention, the first heating rate is preferably 10~15℃ / min, more preferably 12℃ / min, and the first temperature is preferably 1000℃; In this invention, the second heating rate is preferably 2~5℃ / min, more preferably 3~4℃ / min, and the material processing temperature is preferably 1560~1600℃. In this invention, the material processing holding time is preferably 3~6h, more preferably 4h.
[0028] After obtaining the alloy molten material, the present invention uses the crucible as a reference and raises the crystallization furnace chamber along the crucible to allow the alloy to melt and undergo directional crystallization.
[0029] In this invention, the crucible is preferably a graphite crucible, the bottom of the crucible is conical, and the cone angle of the bottom of the crucible is 25~35°, more preferably 30°.
[0030] In this invention, the pressure of the vertical Bridgman oriented crystallization is preferably 120,000~130,000 Pa, more preferably 125,000 Pa. In this invention, the rising rate of the crystallization furnace is preferably 0.3~2 mm / h, more preferably 0.5 mm / h.
[0031] In this invention, during vertical Bridgman orientation crystallization, the temperature change inside the crucible is as follows: the temperature of the reactant decreases at a rate of 2~5℃ / min to 1510~1550℃, preferably: the temperature of the reactant decreases at a rate of 3℃ / min to 1550℃.
[0032] In this invention, vertical Bridgman orientation crystallization is used to drive nucleation and development through supercooling under the premise of seedless crystal-induced growth. Then, through crystal competition and elimination, single crystals are gradually grown. The small-angle design of the crucible accelerates the crystal elimination process.
[0033] In this invention, after the vertical Bridgman orientation crystallization, the product after orientation crystallization is further cooled.
[0034] In this invention, the cooling process is as follows: cooling to a first cooling temperature at a first cooling rate, and then heating to room temperature at a second cooling rate.
[0035] In this invention, the first cooling rate is 2~5℃ / min, preferably 3℃ / min, and the first cooling temperature is preferably 1000~1200℃, more preferably 1100℃; the second cooling rate is preferably 10~25℃ / min, more preferably 15℃ / min.
[0036] The technical solutions of this invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0037] Example 1 Preparation of ZrCoSb0.84Sn0.16: Corresponding to the chemical elemental composition of ZrCoSb0.84Sn0.16, Zr, Co, Sb and Sn particles were weighed and mixed as raw materials, with an additional 2% Sb element added.
[0038] The above raw materials were placed in a magnetic levitation induction furnace for suspension melting. After melting, the molten state was maintained for 35 seconds, and the melting process was repeated three times to obtain a P-type ZrCoSb0.84Sn0.16 semi-Hassler polycrystalline alloy. The semi-Hassler polycrystalline alloy was then crushed and placed in a graphite crucible with a conical bottom and a 25° cone angle. The temperature was increased to 1000°C at a rate of 15°C / min, then increased to 1600°C at a rate of 5°C / min, and held at this temperature for 6 hours. The temperature was then lowered to 1550°C, and the crystallization furnace chamber was raised along the crucible at a rate of 0.5 mm / h. At this point, the single crystal grew at a rate of 0.5 mm / h. After growth, the temperature was lowered to 1200°C at a rate of 3°C / min, and then lowered to room temperature at a rate of 15°C / min. Throughout the single crystal growth process, high-purity argon gas was introduced to maintain the furnace pressure at 120,000 Pa.
[0039] Example 2 The only difference from Example 1 is that ZrCoSb0.84Sn0.16 is replaced with ZrCoSb0.80Sn0.20.
[0040] Example 3 The only difference from Example 1 is that ZrCoSb0.84Sn0.16 is replaced with ZrCoSb0.76Sn0.24.
[0041] Figure 1 shows the XRD patterns of the ZrCoSb-based semi-Hassler single-crystal alloys prepared in Examples 1-3. Figure 1 It can be seen that, except for the CoSb3 impurity phase caused by the added Sb site element, the other peaks of the ZrCoSb1-xSnx single crystal alloy correspond to the ZrCoSb alloy standard PDF card. Furthermore, except for ZrCoSb0.76Sn0.24 along the a-axis, which is a highly oriented semi-Hassler polycrystalline alloy, the other alloys along the a or b axis are (…). l 20) Oriented single-crystal alloys.
[0042] Figure 2 is an SEM image of the ZrCoSb-based semi-Hassler single crystal alloy prepared in Example 2. As can be seen from Figure 2, the ZrCoSb-based semi-Hassler single crystal alloy has no grain boundaries, and the surface of the ZrCoSb-based semi-Hassler single crystal alloy prepared in Example 2 is clean and has no obvious pores.
[0043] The electrical properties of the ZrCoSb-based semi-Hassler single-crystal alloys prepared in Examples 1-3 were tested in this invention. Figure 3 shows the conductivity data of the ZrCoSb-based semi-Hassler single-crystal alloys prepared in Examples 1-3. Figure 3 As can be seen, the conductivity gradually increases with the increase of Sn doping content. For the ZrCoSb0.76Sn0.24 alloy, the conductivity along the b-axis is higher than that along the a-axis. Given a fixed Sn doping content, the increase in conductivity along the b-axis is mainly due to the stronger orientation of the b-axis.
[0044] Figure 4 shows the Seebeck coefficient data of the ZrCoSb-based semi-Hassler single-crystal alloys prepared in Examples 1-3; from Figure 4 As can be seen, the Seebeck coefficient decreases with increasing Sn doping content due to the coupling effect with carrier concentration. For the ZrCoSb0.76Sn0.24 alloy, although the b-axis direction has higher conductivity, the Seebeck coefficient in the b-axis direction is generally lower than that in the a-axis direction.
[0045] Figure 5 shows the calculated power factor data for ZrCoSb-based semi-Hassler single-crystal alloys in Examples 1-3; from Figure 5As can be seen, based on the synergistic regulation of conductivity and Seebeck coefficient, the P-type ZrCoSb0.76Sn0.24 single crystal alloy has a high power factor in the a-axis direction.
[0046] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A p-type ZrCoSb-based semi-Hassler single-crystal alloy, characterized in that, The chemical composition of the P-type ZrCoSb-based semi-Hassler single crystal alloy is ZrCoSb1-xSnx; In ZrCoSb1-xSnx, the value of x is 0.16 or 0.20; The P-type ZrCoSb-based semi-Hassler single-crystal alloy has a MgAgAs-type crystal structure; The preparation method of the aforementioned P-type ZrCoSb-based semi-Hassler single crystal alloy includes the following steps: Corresponding to the chemical element composition of the ZrCoSb-based semi-Hassler single crystal alloy, the alloy raw materials were melted under a protective atmosphere to obtain a semi-Hassler polycrystalline alloy ingot. The semi-Hasler polycrystalline alloy ingot was subjected to vertical Bridgman orientation crystallization under a protective atmosphere to obtain the P-type ZrCoSb-based semi-Hasler single-crystal alloy. The vertical Bridgman oriented crystallization includes the following steps: The semi-Hasler polycrystalline alloy ingot is placed in a crucible and, under a protective atmosphere, is heated to the melting temperature to obtain molten alloy in the crucible. Using the crucible as a reference, the crystallization furnace chamber is raised along the crucible to allow the alloy to melt and undergo directional crystallization; The process of heating to the material melting temperature is as follows: heating to a first temperature at a first heating rate, and then heating to the material melting temperature at a second heating rate; the first heating rate is 10~15℃ / min, and the first temperature is 1000℃; the second heating rate is 2~5℃ / min, and the material melting temperature is 1560~1600℃; the rising rate of the crystallization furnace is 0.5mm / h. During the vertical Bridgman orientation crystallization, the temperature inside the crucible decreases from 2~5℃ / min to 1510~1550℃; the pressure during the vertical Bridgman orientation crystallization is 112000~130000Pa.
2. The method for preparing the P-type ZrCoSb-based semi-Hassler single-crystal alloy according to claim 1, characterized in that... Corresponding to the chemical element composition of the ZrCoSb-based semi-Hassler single crystal alloy, the alloy raw materials were melted under a protective atmosphere to obtain a semi-Hassler polycrystalline alloy ingot. The semi-Hasler polycrystalline alloy ingot was subjected to vertical Bridgman orientation crystallization under a protective atmosphere to obtain the P-type ZrCoSb-based semi-Hasler single-crystal alloy. The vertical Bridgman oriented crystallization includes the following steps: The semi-Hasler polycrystalline alloy ingot is placed in a crucible and, under a protective atmosphere, is heated to the melting temperature to obtain molten alloy in the crucible. Using the crucible as a reference, the crystallization furnace chamber is raised along the crucible to allow the alloy to melt and undergo directional crystallization; The process of heating to the material melting temperature is as follows: heating to a first temperature at a first heating rate, and then heating to the material melting temperature at a second heating rate; the first heating rate is 10~15℃ / min, and the first temperature is 1000℃; the second heating rate is 2~5℃ / min, and the material melting temperature is 1560~1600℃; the rising rate of the crystallization furnace is 0.5mm / h. During the vertical Bridgman orientation crystallization, the temperature inside the crucible decreases from 2~5℃ / min to 1510~1550℃; the pressure during the vertical Bridgman orientation crystallization is 112000~130000Pa.
3. The preparation method according to claim 2, characterized in that, The melting process is magnetic levitation melting; the melting process involves heating the raw material to a molten state and holding it at that temperature for 30-45 seconds; the melting process is repeated 3-5 times.
4. The preparation method according to claim 2, characterized in that, The heat preservation time of the chemical material is 3-6 hours.
5. The preparation method according to claim 2, characterized in that, The vertical Bridgman orientation crystallization process also includes cooling the crystallized product. The cooling process is as follows: cooling to a first cooling temperature at a first cooling rate, and then cooling to room temperature at a second cooling rate; the first cooling rate is 2~5℃ / min, the first cooling temperature is 1000~1200℃, and the second cooling rate is 10~25℃ / min.
Citation Information
Patent Citations
Method of growing zinc selenide single crystal
JP2002068898A
METHOD FOR PRODUCING FeGa ALLOY SINGLE CRYSTAL
JP2022020187A