A carbon dot / dye@metal organic framework composite material and its preparation method and application

By embedding carbon quantum dots and dyes into metal-organic frameworks to form composite materials with dual emission fluorescence peaks, the problems of single fluorescence emission and insufficient stability are solved, and high-sensitivity fluorescent probe detection and multiple applications are achieved.

CN116948639BActive Publication Date: 2024-10-01ANHUI POLYTECHNIC UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310863635.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-14
Publication Date
2024-10-01
Estimated Expiration
2043-07-14

AI Technical Summary

Technical Problem

Existing carbon quantum dot materials mainly have a single blue fluorescence emission, which is easily disturbed by environmental factors, and there are few studies on dual-emission fluorescent materials, resulting in insufficient fluorescence performance and stability.

Method used

Carbon quantum dots with blue fluorescence and high quantum yield dyes are embedded into metal organic frameworks, and the fluorescence emission is adjusted through dye modification to form carbon dots/dyes@metal organic framework composites with dual emission fluorescence peaks and used for ratiometric fluorescence The probe detects heavy metal ions.

Benefits of technology

It achieves the stability and photochemical activity of carbon quantum dots and dyes, avoids aggregation-induced fluorescence quenching, exhibits excellent water solubility and dual-emission fluorescence peaks, improves sensitivity to target analytes, and is suitable for fluorescent probes, Photocatalysis, anti-counterfeiting materials and LED luminescent materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116948639B_ABST
    Figure CN116948639B_ABST
Patent Text Reader

Abstract

The present invention provides a carbon dot / dye@metal organic framework composite material and its preparation method and application. By adding the prepared CDs and dyes in the synthesis process of the metal organic framework, a CDs / dye@metal organic framework composite material is prepared. The composite material has a wide absorption spectrum and emission spectrum. The types of CDs and dyes can be changed according to needs to change the position of the dual (multi) fluorescence emission peak. The synthesis method is simple and convenient. This fluorescent composite material has both the high stability of the metal organic framework and the tunable excitation wavelength of CDs. It has been successfully used to establish a ratio fluorescence probe to detect mercury ions, and is expected to be applied to photocatalysis, anti-counterfeiting materials, biological imaging, pollutant degradation and LED luminescent materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of material preparation, and in particular to a carbon dot / dye@metal organic framework composite material and a preparation method and application thereof. Background Art

[0002] Carbon quantum dots have many advantages, such as excellent optical properties, good water solubility, low toxicity, environmental friendliness, wide raw material sources, low cost, good biocompatibility, etc. Since carbon quantum dots were first discovered, many synthesis methods have been developed, including arc discharge method, laser ablation method, electrochemical synthesis method, chemical oxidation method, combustion method, hydrothermal synthesis method, microwave synthesis method, template method, etc.

[0003] Carbon dots (CDs) are promising nanomaterials in the fields of fluorescent probes, chemical and biological sensing, drug detection, drug delivery, and photocatalysis due to their excellent properties such as high photothermal stability, easy surface modification, adjustable composition and fluorescence emission, good biocompatibility, and low cytotoxicity. Most of the CDs reported so far have a single fluorescence peak of blue light emission, which is easily interfered by other substances and uncontrollable factors such as instrument voltage and concentration changes.

[0004] Metal-organic frameworks, as a new type of porous material composed of organic ligands and metal ions, have many excellent properties such as adjustable skeleton structure, large specific surface area, adjustable pore size and shape. The highly porous structure of metal-organic frameworks can be used to develop nanocluster / metal-organic framework composites to enhance the fluorescence properties of nanoclusters.

[0005] However, there is little research on dual (multi) emission fluorescent materials. Summary of the invention

[0006] The purpose of the present invention is to provide a carbon dot / dye@metal organic framework composite material and a preparation method thereof, CDs with blue fluorescence and a dye with high quantum yield are embedded in a metal organic framework, and a new metal organic framework with dual emission fluorescence peaks is developed, which exhibits excellent water solubility and dual emission fluorescence peaks, and not only avoids fluorescence quenching caused by aggregation-induced CDs and dye molecules, but also maintains the stability and photochemical activity of CDs and dyes.

[0007] Another object of the present invention is to provide an application of the carbon dot / dye@metal organic framework composite material for detecting mercury ions using a ratiometric fluorescent probe.

[0008] The specific technical solutions of the present invention are as follows:

[0009] A method for preparing a carbon dot / dye@metal organic framework composite material, specifically comprising:

[0010] During the preparation of the metal organic framework, CDs and dyes are added, stirred and mixed, and reacted to obtain the product.

[0011] The metal organic framework is selected from ZIF-8, UiO-66 or ZIF-67;

[0012] The dye includes but is not limited to rhodamine 6G (Rh6G), rhodamine B, Nile blue, neutral red, fluorescent yellow or quinaldine red;

[0013] The CDs (carbon dots) are CDs with an emission wavelength of 350-700 nm; the CDs are synthesized by hydrothermal or microwave method;

[0014] After the reaction, the CDs / dye@metal organic framework composite material powder is obtained by washing, centrifugal drying.

[0015] The CDs include but are not limited to carbon dots prepared by using citric acid and urea or citric acid and ethylenediamine as raw materials;

[0016] Preferably, the preparation method of the CDs is:

[0017] Dissolve citric acid and urea in ultrapure water, transfer them into Teflon liner after dissolving by ultrasonic stirring, place the assembled reactor in an oven with set temperature for heating, take out the reaction solution after the reaction is finished, filter and centrifuge and dialyze to obtain CDs.

[0018] The carbon dots / dye@metal organic framework composite materials are CDs / Rh6G@ZIF-8 and CDs / Rh6G@UiO-66.

[0019] Preferably, the carbon dot / dye@metal organic framework composite material is CDs / Rh6G@ZIF-8, and the preparation method is: 2-methylimidazole and zinc nitrate are respectively dissolved in methanol, and the obtained zinc nitrate solution is dripped into the 2-methylimidazole solution. After the dropwise addition is completed, CDs and rhodamine 6G are immediately added, and then stirring and mixing are continued, and then standing for 12 to 36 hours. After the reaction is completed, the obtained solid is washed and centrifuged 3 to 5 times, and finally dried to obtain CDs / Rh6G@ZIF-8 orange-red powder.

[0020] The mass ratio of 2-methylimidazole to zinc nitrate is 1:1-10:1, preferably 2:1;

[0021] The concentration of the 2-methylimidazole in methanol is 0.01-0.05 g / mL;

[0022] The mass ratio of 2-methylimidazole to CDs is 100:1-10, preferably 100:1;

[0023] The mass ratio of CDs to rhodamine 6G is 1:0.48-0.51, preferably 1:0.5;

[0024] The growth of ZIF-8 is a surface-restricted process, and the formation of ZIF-8 is affected by the amount of ligands or ions in the solvent. 2+ As the ratio increases, the ZIF-8 particles formed are larger, and the large ZIF-8 particles are formed by the aggregation of smaller ZIF-8 nanocrystals. 2+ ions can form ZIF-8 nuclei in a very short time. 2+ The ratio and solvent volume have a great influence on the morphology of ZIF-8, and the product morphology obtained with different addition amounts is different.

[0025] Preferably, the carbon dot / dye@metal organic framework composite material is CDs / Rh6G@UiO-66, and the preparation method is: dissolving terephthalic acid and sodium acetate in N,N-dimethylformamide DMF respectively, ultrasonically mixing the two solutions obtained, adding zirconium tetrachloride, and continuing to ultrasonicate until the zirconium tetrachloride is completely dissolved, then adding CDs and Rh6G thereto, and then transferring the mixed liquid into a Teflon-lined reactor, heating the reaction, and after the reaction is completed, taking out the reaction liquid, and after multiple centrifugal drying, obtaining CDs / Rh6G@UiO-66 orange-red powder.

[0026] The mass ratio of terephthalic acid to sodium acetate is 1:1-5:1, preferably 3:1;

[0027] The concentration of terephthalic acid in DMF is 0.01-0.05 g / mL;

[0028] The mass ratio of terephthalic acid to zirconium tetrachloride is 5-7:1, preferably 6:1;

[0029] The mass ratio of zirconium tetrachloride, CDs and Rh6G is 1:0.04-0.06:0.025-0.035, preferably 1:0.05:0.025;

[0030] The heating reaction refers to the reaction at 120±10°C for 4±0.5h;

[0031] In the composite material prepared above, the dye is modified on the surface of the carbon quantum dots, and the color of the product can be adjusted by adjusting the dosage. Then, the carbon quantum dots modified with the dye are wrapped into the MOF crystal cavity during the MOF crystal formation process.

[0032] The present invention provides a carbon dot / dye@metal organic framework composite material, which is prepared by the above method.

[0033] The invention provides an application of a carbon dot / dye@metal organic framework composite material for detecting heavy metal ions as a ratiometric fluorescent probe, preferably for detecting mercury ions.

[0034] The present invention develops a novel metal organic framework with dual emission fluorescence peaks by embedding CDs with blue fluorescence and dyes with high quantum yield into a metal organic framework. The fluorescence emission and color of carbon quantum dots are modified and adjusted with dyes, and then they are encapsulated in MOF, so that the effect achieved is to have the advantages of both. Experiments show that CDs / dye@metal organic framework exhibits excellent water solubility and dual emission fluorescence peaks, which not only avoids fluorescence quenching caused by aggregation induction of CDs and dye molecules, but also maintains the stability and photochemical activity of CDs and dyes. The synthesized CDs / dye@metal organic framework is expected to be applied to the dual emission peaks of ratio fluorescence probes and ratio fluorescence sensors. The two-peak reference can establish a self-calibration system, thereby eliminating environmental influences and improving the sensitivity to target analytes. It can also be used for photocatalysis, anti-counterfeiting materials, biological imaging, pollutant degradation and LED luminescent materials. The degraded pollutants include various antibiotics, organic dyes and cosmetics that may be contained in natural water bodies.

[0035] Compared with the prior art, the present invention prepares a CDs / dye@metal organic framework composite material by adding the prepared CDs and dyes during the synthesis of the metal organic framework. The composite material has a wide absorption spectrum and emission spectrum, and the types of CDs and dyes can be changed according to needs to change the position of the dual (multi) fluorescence emission peaks. The synthesis method is simple and convenient. This fluorescent composite material has both the high stability of the metal organic framework and the tunable excitation wavelength of CDs. It has been successfully used to establish a ratio fluorescence probe and is expected to be applied to photocatalysis, anti-counterfeiting materials, biological imaging, pollutant degradation, and LED luminescent materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 is a high-resolution transmission electron microscope image of the CDs prepared in Example 1;

[0037] Figure 2 is the UV-fluorescence spectrum of the CDs prepared in Example 1;

[0038] Figure 3 is a scanning electron microscope image of ZIF-8 prepared in Example 2;

[0039] Figure 4 This is a scanning electron microscope image of UiO-66 prepared in Example 3;

[0040] Figure 5 This is a scanning electron microscope image of CDs / Rh6G@ZIF-8 prepared in Example 4;

[0041] Figure 6 This is the infrared spectrum of CDs / Rh6G@ZIF-8 prepared in Example 4;

[0042] Figure 7 The XRD spectrum of CDs / Rh6G@ZIF-8 prepared in Example 4;

[0043] Figure 8 The UV-fluorescence spectrum of CDs / Rh6G@ZIF-8 prepared in Example 4;

[0044] Fig. 9 CDs / Rh6G@ZIF-8 prepared in Example 4 and different concentrations of Hg 2+ Fluorescence emission spectra of the mixture;

[0045] Fig.10 CDs / Rh6G@ZIF-8 prepared in Example 4 and different concentrations of Hg 2+ Mixed linear relationships;

[0046] Fig.11 is a scanning electron microscope image of ZIF-8 prepared in Example 6;

[0047] Fig.12 This is a scanning electron microscope image of CDs / Rh6G@ZIF-8 prepared in Example 7;

[0048] Fig.13 This is a scanning electron microscope image of CDs / Rh6G@ZIF-8 prepared in Example 8;

[0049] Fig.14 Schematic diagram of the synthesis of CDs / Rh6G@ZIF-8 in Example 4. DETAILED DESCRIPTION

[0050] Various exemplary embodiments of the present invention are described below. This detailed description should not be considered as limiting the present invention. It is only used to describe specific embodiments, not to limit the present invention. Instead, it should be understood to include but not be limited to the following examples, which are a more detailed description of the present invention.

[0051] Although the present invention describes preferred methods and materials, any methods and materials similar or equivalent to the methods and materials described herein can also be used in the practice or testing of the present invention. Various modifications and changes can be made to the specific embodiments of the present invention without departing from the scope, essence and spirit of the present invention, which is easy for those skilled in the art.

[0052] Example 1

[0053] Preparation of CDs:

[0054] Accurately weigh 0.5000g of citric acid and 0.3000g of urea in a 50mL beaker, add 20mL of ultrapure water to dissolve by ultrasonication, and then transfer to a Teflon liner. Place the assembled reactor in an oven preheated to 160°C for 10 hours. After the reaction is completed, take out the reactor, cool it to room temperature, filter the resulting solution to remove large particle impurities, then transfer the filtrate to a centrifuge tube, centrifuge to remove small particle impurities, transfer the upper layer solution obtained by centrifugation to a dialysis bag for 48 hours, and freeze-dry the dialyzed CDs to obtain a dark brown CDs powder.

[0055] Example 2

[0056] Preparation of ZIF-8:

[0057] 0.6000 g of 2-methylimidazole and 0.3000 g of zinc nitrate were dissolved in 20 mL of methanol respectively. The obtained zinc nitrate solution was added dropwise into the 2-methylimidazole solution under stirring. After the addition was completed, the mixture was allowed to stand for 24 h to allow the reaction to complete. After the reaction was completed, the obtained solid was washed with methanol and centrifuged at 8000 r / min for 5 times. It was then dried in vacuum at 60°C to obtain ZIF-8 white powder.

[0058] Example 3

[0059] Preparation of UiO-66:

[0060] 0.4000g of terephthalic acid and 0.5000g of sodium acetate were dissolved in 20mL of DMF respectively. After the obtained mixture was uniformly mixed by ultrasonication, 0.1000g of zirconium tetrachloride was added, and ultrasonication was continued until the zirconium tetrachloride was completely dissolved. The mixed liquid was then transferred to a Teflon liner, and the assembled reactor was placed in an oven set at 120°C for heating and reaction for 4h. After the reaction was completed, the obtained solid was washed with methanol and centrifuged at 8000r / min for 5 times, and vacuum dried at 60°C to obtain UiO-66 white powder.

[0061] Example 4

[0062] A method for preparing a carbon dot / dye@metal organic framework composite material, specifically comprising:

[0063] 0.6000 g of 2-methylimidazole and 0.3000 g of zinc nitrate were respectively dissolved in 20 mL of methanol. The zinc nitrate solution was added dropwise into the 2-methylimidazole solution under stirring. After the addition was completed, 0.0060 g of CDs prepared in Example 1 and 0.0030 g of Rh6G were immediately added. Methanol was added to adjust the total volume to 50 mL. After standing for 24 hours, the mixture was washed with methanol and centrifuged at 8000 r / min for 5 times. The mixture was vacuum dried at 60°C to obtain a light reddish brown solid powder CDs / Rh6G@ZIF-8.

[0064] Figure 5 This is a scanning electron microscope image of CDs / Rh6G@ZIF-8 prepared in Example 4; Figure 6 This is the infrared spectrum of CDs / Rh6G@ZIF-8 prepared in Example 4; Figure 7 The XRD spectrum of CDs / Rh6G@ZIF-8 prepared in Example 4; Figure 8 This is the UV-fluorescence spectrum of CDs / Rh6G@ZIF-8 prepared in Example 4; it can be seen that the obtained product has fluorescence emission peaks of both carbon dots and dyes, and XRD also shows that the composite has both MOF peaks and CDs peaks.

[0065] Example 5

[0066] A method for preparing a carbon dot / dye@metal organic framework composite material, specifically comprising:

[0067] Accurately weigh 0.6000g of terephthalic acid and 0.2000g of sodium acetate and dissolve them in 20mL of DMF, ultrasonically dissolve them, then add 0.1000g of zirconium tetrachloride, continue ultrasonication for 10min until the zirconium tetrachloride is completely dissolved, add 0.0050g of CDs prepared in Example 1 and 0.0025g of Rh6G, transfer the reaction solution into a Teflon liner, and place the assembled reactor in an oven at 120°C for 4h. After the reaction is completed, wash the solid obtained by the reaction with methanol and centrifuge it at 8000r / min for 5 times. The solid obtained by centrifugation is dried in a vacuum drying oven to obtain a light red solid powder CDs / Rh6G@UiO-66.

[0068] Example 6

[0069] Preparation of ZIF-8:

[0070] 0.7000 g of 2-methylimidazole and 0.2500 g of zinc nitrate were dissolved in 20 mL of methanol respectively. The zinc nitrate solution was added dropwise into the 2-methylimidazole solution under stirring. After the addition was completed, the mixture was allowed to stand for 24 h, washed and centrifuged with methanol at 8000 r / min for 5 times, and dried in vacuo at 60°C to obtain a white solid powder ZIF-8.

[0071] Example 7 (for comparison)

[0072] A method for preparing a carbon dot / dye@metal organic framework composite material, specifically comprising:

[0073] 0.6000 g of 2-methylimidazole and 0.3000 g of zinc nitrate were dissolved in 20 mL of methanol respectively. The zinc nitrate solution was added dropwise to the 2-methylimidazole solution under stirring. After the addition was complete, 0.0060 g of CDs prepared in Example 1 was added. continue Stir for 10 minutes , then 0.0030 g of rhodamine 6G was added, and methanol was added to adjust the total volume to 50 mL. After standing for 24 h, the mixture was washed and centrifuged 5 times at 8000 r / min with methanol, and vacuum dried at 60 °C to obtain a light reddish brown solid powder CDs / Rh6G@ZIF-8.

[0074] Example 8 (for comparison)

[0075] A method for preparing a carbon dot / dye@metal organic framework composite material, specifically comprising:

[0076] Dissolve 0.6000 g of 2-methylimidazole and 0.3000 g of zinc nitrate in 20 mL of methanol respectively. Add the zinc nitrate solution drop by drop into the 2-methylimidazole solution under stirring until the addition is complete. Stir for 10 minutes. Then, 0.0060 g of CDs prepared in Example 1 was added. Continue stirring for 10 min. , then add 0.0030g of rhodamine 6G, add methanol to adjust the total volume to 50mL, let it stand for 24h, wash and centrifuge it with methanol at 8000r / min for 5 times, and dry it in vacuum at 60℃ to obtain a light reddish brown solid powder CDs / Rh6G@ZIF-8.

[0077] Comparing Example 4, Example 7 and Example 8, it can be seen that adding CDs and Rhodamine 6G at different times has a great influence on the morphology of CDs / Rh6G@ZIF-8. In Example 4, adding CDs and Rhodamine 6G at the early stage of ZIF-8 formation is more conducive to the formation of ZIF-8 coated with CDs and Rhodamine 6G. On the contrary, in Example 7 and Example 8, adding CDs or Rhodamine 6G after 10 minutes of ZIF-8 synthesis will form a huge and extremely irregular CDs / Rh6G@ZIF-8 ( Fig.12 , Fig.13 ). This may be because the functional groups in CDs or Rh6G are similar to anionic surfactants, which play a bridging role between the small ZIF-8 particles formed in the early stage of the reaction, which leads to cross-linking between the small ZIF-8 particles formed, and finally forms a huge and extremely irregular "cross-linked" product of CDs, Rh6G and ZIF-8. Therefore, when synthesizing metal organic framework materials, adding carbon dots and dyes at the early stage of crystal formation is conducive to the formation of regular morphology, otherwise irregular composites will be obtained.

[0078] Example 9

[0079] The CDs / Rh6G@ZIF-8 aqueous solution prepared in Example 4 was prepared at a concentration of 8000 to control the maximum intensity of the carbon dot fluorescence peak; the same volume of CDs / Rh6G@ZIF-8 solution with the same concentration and the same volume of Hg 2+The solutions were mixed evenly and diluted to the same volume with the same pH buffer, 3 mL, Hg 2+ Final concentration 5×10 -7 mol / L、7.5×10 -7 mol / L、1×10 -6 mol / L、1.25×10 -6 mol / L、1.5×10 -6 mol / L, let it stand at room temperature for 10 min, use 360 ​​nm as the excitation wavelength, and observe and record the fluorescence emission spectrum of each group.

[0080] Fig. 9 CDs / Rh6G@ZIF-8 prepared in Example 4 and different concentrations of Hg 2+ Fluorescence emission spectra of the mixture; Fig.10 CDs / Rh6G@ZIF-8 prepared in Example 4 and different concentrations of Hg 2+ The linear relationship of the mixture is shown in Table 1. It can be seen that the CDs / Rh6G@ZIF-8 prepared in the present invention has a significant influence on the Hg 2+ The detection has a good linear relationship, a low detection limit and high sensitivity.

[0081] Simulated Hg 2+ The polluted wastewater samples were tested and the recovery rate was calculated. The results are shown in Table 1.

[0082] Table 1 CDs / Rh6G@ZIF-8 prepared in Example 4 Detection of Hg 2+ test

[0083]

[0084]

[0085] The fluorescent composite material prepared by CDs, dyes and metal organic frameworks in the present invention has a wide range of ultraviolet-visible absorption and fluorescence emission, and can adjust dual (multiple) fluorescence emission peaks according to needs. This fluorescent composite material has both the high stability of metal organic frameworks and the tunable excitation wavelength of CDs, and has been successfully used as a fluorescent probe. In addition, the composite material is also expected to be used in photocatalysis, anti-counterfeiting materials, pollutant degradation and LED luminescent materials.

Claims

1. A method for preparing a carbon dot / dye@metal organic framework composite material, characterized in that: The preparation method is specifically: The carbon dot / dye@metal organic framework composite material is CDs / Rh6G@ZIF-8, and the preparation method is as follows: 2-methylimidazole and zinc nitrate are dissolved in methanol respectively, and the obtained zinc nitrate solution is dripped into the 2-methylimidazole solution. After the dripping is completed, CDs and rhodamine 6G are immediately added, stirred and mixed, and then allowed to stand for 12 to 36 hours to obtain CDs / Rh6G@ZIF-8 orange-red powder; The mass ratio of 2-methylimidazole to CDs is 100:1-10; the mass ratio of CDs to rhodamine 6G is 1:0.48-0.51; The prepared carbon dots / dye@metal organic framework composites were used as ratiometric fluorescent probes to detect mercury ions.

2. The preparation method according to claim 1, characterized in that: The CDs have an emission wavelength of 350-700 nm.

3. A carbon dot / dye@metal organic framework composite material prepared by the preparation method according to claim 1 or 2.

4. An application of a carbon dot / dye@metal organic framework composite material prepared by the preparation method of claim 1 or 2, characterized in that: Used as a ratiometric fluorescent probe to detect mercury ions.