A wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material and preparation method thereof

By combining different proportions of multi-phase antiperovskite manganese nitrogen compounds with aluminum matrix, the negative thermal expansion temperature interval of antiperovskite manganese nitrogen compounds is expanded, and the antiperovskite manganese nitrogen compounds in the prior art is solved The problem of narrow expansion temperature range of /aluminum composite materials has achieved near zero expansion in a wide temperature zone and excellent mechanical and thermal conductivity.

CN116949313BActive Publication Date: 2024-11-12HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310958860.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-01
Publication Date
2024-11-12
Estimated Expiration
2043-08-01

AI Technical Summary

Technical Problem

The near-zero expansion temperature range of the existing anti-perovskite manganese nitrogen compound/aluminum composite materials is narrow, and the thermal expansion of the aluminum matrix cannot be effectively suppressed within a wide temperature range.

Method used

The composite material is prepared by pressure impregnation method of multi-phase reverse perovskite manganese nitrogen compound reinforcement and aluminum matrix. By combining different proportions of antiperovskite manganese nitrogen compounds, the negative thermal expansion temperature range is expanded to make it between 50 and 100℃. It has a negative thermal expansion coefficient within the range, achieving near-zero expansion effect in the wide temperature zone.

Benefits of technology

In the temperature range of -5~60℃, the average thermal expansion coefficient of the composite material is reduced to 0.40×10-6/℃, the bending strength can reach 211MPa, the thermal conductivity can reach 46W/(m·K), and it has excellent comprehensive performance .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116949313B_ABST
    Figure CN116949313B_ABST
Patent Text Reader

Abstract

A wide temperature range near-zero expansion multi-phase inverse perovskite manganese nitrogen compound / aluminum composite material and a preparation method thereof, relating to an aluminum-based composite material and a preparation method thereof. In order to solve the problem that the existing inverse perovskite manganese nitrogen compound / aluminum composite material has a narrow near-zero expansion temperature range, the wide temperature range near-zero expansion multi-phase inverse perovskite manganese nitrogen compound / aluminum composite material is composited by a multi-phase inverse perovskite manganese nitrogen compound reinforcement and a matrix metal; preparation: raw materials are weighed respectively according to the molecular formula of the inverse perovskite manganese nitrogen compound reinforcement, and sintered to obtain a variety of inverse perovskite manganese nitrogen compounds, and then pre-pressed and preheated and pressurized infiltrated to obtain a multi-phase inverse perovskite manganese nitrogen compound / aluminum composite material. The average thermal expansion coefficient of the prepared multi-phase inverse perovskite manganese nitrogen compound / aluminum composite material is only 0.40×10 ‑6 ℃ ‑1 , the bending strength reaches 211MPa and the thermal conductivity can reach 46W / (m·K).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an aluminum-based composite material and a preparation method thereof. Background Art

[0002] In recent years, with the development of science and technology, fields such as aerospace and electronic packaging have higher requirements for instrument performance. However, due to the nature of thermal expansion and contraction, traditional materials will change in size when the ambient temperature changes. On the one hand, this dimensional change will affect the structure of the instrument, thereby affecting the accuracy; on the other hand, the inconsistent thermal deformation between different materials will produce thermal stress, which is prone to fatigue in the long run and affects the service life of the instrument. Therefore, the development of near-zero expansion materials is a problem that needs to be solved urgently. Through composite material design, using reinforcements with negative thermal expansion to suppress the thermal expansion of metal matrices and organic matter is an effective means.

[0003] Antiperovskite manganese nitrogen compounds are known for their large magnetic volume effect. They will produce a large volume contraction at the magnetic transition temperature, resulting in negative thermal expansion. At present, by relaxing their magnetic transition behavior through element doping, it is possible to obtain -60 to -150×10 -6 ℃ -1 Thermal expansion properties of antiperovskite manganese nitrogen compounds. Due to its huge negative thermal expansion coefficient, antiperovskite manganese nitrogen compounds are considered to be ideal reinforcements for suppressing high thermal expansion materials such as metals and organics. At the same time, the elastic modulus of antiperovskite manganese nitrogen compounds can reach 150-200GPa, and the thermal conductivity can reach 1.8-4.0W / (m·K). The prepared composite materials can also have excellent mechanical properties and thermal conductivity. However, although the negative thermal expansion coefficient of a single antiperovskite manganese nitrogen compound is extremely large, its negative thermal expansion temperature range is relatively narrow. The prepared antiperovskite manganese nitrogen compound / aluminum composite material only achieves near-zero expansion in the temperature range of 10-15°C. Therefore, how to expand the near-zero expansion temperature range of antiperovskite manganese nitrogen compound / aluminum composite materials is currently a difficult problem. Summary of the invention

[0004] In order to solve the problem that the existing antiperovskite manganese nitrogen compound / aluminum composite material has a narrow near-zero expansion temperature range, the present invention provides a wide temperature range near-zero expansion multi-antiperovskite manganese nitrogen compound / aluminum composite material and a preparation method thereof.

[0005] The wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material of the present invention is composited by a multi-phase perovskite manganese nitrogen compound reinforcement and a matrix metal; the volume fraction of the multi-phase perovskite manganese nitrogen compound reinforcement in the composite material is 20-70%;

[0006] The multi-phase perovskite manganese nitrogen compound reinforcement includes Mn3Zn1-x Sn x N, Mn3Zn 1-x Ge x N, Mn3Zn 1-x- y Sn x Si y N, Mn3Zn 1-x Si x N, Mn3Zn 1-x-y Sn x Mn y N、Mn3Cu 1-x Sn x N、Mn3Cu 1-x Ge x N、Mn3Cu 1-x-y Sn x Si y N、Mn3Cu 1-x Si x N、Mn3Cu 1-x-y Sn x Mn y At least two of N, where 0 <x<1,0<y<1,0<x+y<1;

[0007] The preparation method of the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material of the present invention is carried out according to the following steps:

[0008] 1. According to the molecular formula of the antiperovskite manganese nitrogen compound reinforcement Mn3Zn 1-x Sn x N, Mn3Zn 1-x Ge x N, Mn3Zn 1-x-y Sn x Si y N, Mn3Zn 1-x Si x N, Mn3Zn 1-x-y Sn x Mn y N、Mn3Cu 1-x Sn x N、Mn3Cu 1-x Ge x N、Mn3Cu 1-x- y Sn x Si y N、Mn3Cu 1-x Si x N、Mn3Cu 1-x-y Sn x Mn yAt least two of N are weighed as raw materials, and are pressed into blocks and vacuum sintered to obtain a plurality of antiperovskite manganese nitrogen compounds, wherein 0 <x<1,0<y<1,0<x+y<1;

[0009] 2. Mixing the multiple antiperovskite manganese nitrogen compounds obtained in step 1 to obtain a mixed powder, and then placing it in a cast iron mold for pre-pressing to obtain multiple antiperovskite manganese nitrogen compounds;

[0010] The multi-phase perovskite manganese nitrogen compound Mn3Zn 1-x Sn x N, Mn3Zn 1-x Ge x N, Mn3Zn 1-x-y Sn x Si y N, Mn3Zn 1-x Si x N, Mn3Zn 1-x-y Sn x Mn y N、Mn3Cu 1-x Sn x N、Mn3Cu 1-x Ge x N、Mn3Cu 1-x-y Sn x Si y N、Mn3Cu 1-x Si x N、Mn3Cu 1-x-y Sn x Mn y The mass fraction of N is 0 to 50%;

[0011] 3. placing the cast iron mold containing the multi-phase perovskite manganese nitrogen compound in step 2 in a furnace for preheating;

[0012] Fourth, pouring the molten matrix metal into a preheated iron mold, and then performing pressure infiltration, and finally cooling and demolding to obtain a multi-phase perovskite manganese nitrogen compound / aluminum composite material; the volume fraction of the multi-phase perovskite manganese nitrogen compound reinforcement in the composite material is 20-70%.

[0013] The principles and beneficial effects of the present invention are:

[0014] 1. The present invention adopts a pre-process to prepare a plurality of antiperovskite manganese nitrogen compounds with negative thermal expansion in different temperature ranges, and then combines the plurality of antiperovskite manganese nitrogen compounds in a specific ratio, so that the negative thermal expansion temperature range of the antiperovskite manganese nitrogen compounds is expanded from a single-phase temperature range to a multi-phase temperature range; the obtained multi-phase antiperovskite manganese nitrogen compounds with near-zero expansion in a wide temperature range have a negative thermal expansion coefficient of -10 to -40×10 -6 / ℃.

[0015] 2. The composite material prepared by the pressure infiltration method is a multi-inverse perovskite manganese nitrogen compound / aluminum composite material. The various antiperovskite manganese nitrogen compounds in the composite material exert negative thermal expansion effects in different temperature ranges, thereby inhibiting the thermal expansion of the aluminum matrix in a wider temperature range, and realizing the design of a near-zero expansion material in a wide temperature range. The multi-inverse perovskite manganese nitrogen compound / aluminum composite material finally prepared has an average thermal expansion coefficient of only 0.40×10 -6 ℃ -1 At the same time, the bending strength can reach 211MPa and the thermal conductivity can reach 46W / (m·K), with excellent comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is a thermal expansion curve diagram in Example 1;

[0017] Figure 2 is the bending stress-strain curve of the multi-phase perovskite manganese nitrogen compound / aluminum composite material in Example 1;

[0018] Figure 3 Thermal expansion curve diagram in Example 2;

[0019] Figure 4 This is the thermal expansion curve diagram in Example 3. DETAILED DESCRIPTION

[0020] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any reasonable combination of the specific implementation modes.

[0021] Specific implementation method 1: In this implementation method, the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material is composited by a multi-phase perovskite manganese nitrogen compound reinforcement and a matrix metal; the volume fraction of the multi-phase perovskite manganese nitrogen compound reinforcement in the composite material is 20-70%;

[0022] The multi-phase perovskite manganese nitrogen compound reinforcement includes Mn3Zn 1-x Sn x N, Mn3Zn 1-x Ge x N, Mn3Zn1-x- y Sn x Si y N, Mn3Zn 1-x Si x N, Mn3Zn 1-x-y Sn x Mn y N、Mn3Cu 1-x Sn x N、Mn3Cu 1-x Ge x N、Mn3Cu 1-x-y Sn x Si y N、Mn3Cu 1-x Si x N、Mn3Cu 1-x-y Sn x Mn y At least two of N, where 0 <x<1,0<y<1,0<x+y<1。

[0023] The multi-phase perovskite manganese nitrogen compound with near-zero expansion in a wide temperature range has a negative thermal expansion coefficient of -10 to -40×10 -6 / ℃. In the multi-inverse perovskite manganese nitrogen compound / aluminum composite material of this embodiment, multiple antiperovskite manganese nitrogen compounds exert negative thermal expansion effects in different temperature ranges, thereby suppressing the thermal expansion of the aluminum matrix in a wider temperature range, and realizing the design of a near-zero expansion material in a wide temperature range. The average thermal expansion coefficient of the multi-inverse perovskite manganese nitrogen compound / aluminum composite material in the temperature range of -5 to 60℃ is only 0.40×10 -6 ℃ -1 At the same time, the bending strength can reach 211MPa and the thermal conductivity can reach 46W / (m·K), with excellent comprehensive performance.

[0024] Specific implementation method 2: This implementation method is different from the specific implementation method 1 in that the base metal is pure aluminum or aluminum alloy.

[0025] Specific embodiment three: The difference between this embodiment and specific embodiment two is that the aluminum alloy is one or a mixture of several of Al-Si alloy, Al-Cu alloy, Al-Mg alloy, Al-Si-Cu alloy, Al-Si-Mg alloy, Al-Cu-Mg alloy, Al-Zn-Cu alloy, Al-Zn-Mg-Cu alloy, Al-Be alloy, Al-Li alloy, and Al-Si-Cu-Mg alloy.

[0026] Specific embodiment 4: The preparation method of the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material of this embodiment is carried out according to the following steps:

[0027] 1. According to the molecular formula of the antiperovskite manganese nitrogen compound reinforcement Mn3Zn 1-x Sn x N, Mn3Zn 1-x Ge x N, Mn3Zn 1-x-y Sn x Si y N, Mn3Zn 1-x Si x N, Mn3Zn 1-x-y Sn x Mn y N、Mn3Cu 1-x Sn x N、Mn3Cu 1-x Ge x N、Mn3Cu 1-x- y Sn x Si y N、Mn3Cu 1-x Si x N、Mn3Cu 1-x-y Sn x Mn y At least two of N are weighed as raw materials, and are pressed into blocks and vacuum sintered to obtain a plurality of antiperovskite manganese nitrogen compounds, wherein 0 <x<1,0<y<1,0<x+y<1;

[0028] 2. Mixing the multiple antiperovskite manganese nitrogen compounds obtained in step 1 to obtain a mixed powder, and then placing it in a cast iron mold for pre-pressing to obtain multiple antiperovskite manganese nitrogen compounds;

[0029] The multi-phase perovskite manganese nitrogen compound Mn3Zn 1-x Sn x N, Mn3Zn 1-x Ge x N, Mn3Zn 1-x-y Sn x Si y N, Mn3Zn 1-x Si x N, Mn3Zn 1-x-y Sn x Mn y N、Mn3Cu 1-x Sn x N、Mn3Cu 1-x Ge x N、Mn3Cu 1-x-y Sn x Si y N、Mn3Cu 1-x Six N、Mn3Cu 1-x-y Sn x Mn y The mass fraction of N is 0 to 50%;

[0030] 3. placing the cast iron mold containing the multi-phase perovskite manganese nitrogen compound in step 2 in a furnace for preheating;

[0031] Fourth, pouring the molten matrix metal into a preheated iron mold, and then performing pressure infiltration, and finally cooling and demolding to obtain a multi-phase perovskite manganese nitrogen compound / aluminum composite material; the volume fraction of the multi-phase perovskite manganese nitrogen compound reinforcement in the composite material is 20-70%.

[0032] 1. This embodiment adopts a pre-process to prepare a plurality of antiperovskite manganese nitrogen compounds with negative thermal expansion in different temperature ranges, and then combines the plurality of antiperovskite manganese nitrogen compounds in a specific ratio, so that the negative thermal expansion temperature range of the antiperovskite manganese nitrogen compounds is expanded from a single-phase temperature range to a multi-phase temperature range; the obtained multi-phase antiperovskite manganese nitrogen compounds with near-zero expansion in a wide temperature range have a negative thermal expansion coefficient of -10 to -40×10 -6 / ℃.

[0033] 2. This embodiment adopts the pressure infiltration method to prepare the composite material as a multi-inverse perovskite manganese nitrogen compound / aluminum composite material. The various antiperovskite manganese nitrogen compounds in the composite material exert negative thermal expansion effects in different temperature ranges, thereby suppressing the thermal expansion of the aluminum matrix in a wider temperature range, and realizing the design of a near-zero expansion material in a wide temperature range. The multi-inverse perovskite manganese nitrogen compound / aluminum composite material finally prepared has an average thermal expansion coefficient of only 0.40×10 -6 ℃ -1 At the same time, the bending strength can reach 211MPa and the thermal conductivity can reach 46W / (m·K), with excellent comprehensive performance.

[0034] Specific implementation mode five: This implementation mode is different from any one of specific implementation modes one to four in that: the raw material in step one is manganese dinitrogen, manganese tetranitrogen, zinc powder, tin powder, copper powder, germanium powder or silicon powder.

[0035] Specific embodiment 6: This embodiment is different from the specific embodiments 1 to 5 in that: the temperature of the vacuum sintering in step 1 is 700-1000°C; the vacuum degree of the vacuum sintering is 1×10 -5 Pa~1×10 -4 Pa.

[0036] Specific implementation method seven: This implementation method is different from any one of specific implementation methods one to six in that: the pre-pressing pressure in step two is 2 to 20 MPa.

[0037] Specific implementation eight: This implementation differs from any one of specific implementations one to seven in that: the preheating temperature in step three is 400-800° C.; the preheating time is 1-4 hours.

[0038] Specific embodiment 9: This embodiment is different from any one of specific embodiments 1 to 8 in that: the temperature of the molten base metal in step 4 is 700-900°C.

[0039] Specific implementation method ten: This implementation method is different from any one of specific implementation methods one to nine in that: the pressure during the pressurized infiltration in step four is 20 to 40 MPa; the time during the pressurized infiltration is 10 to 30 minutes.

[0040] Embodiment 1:

[0041] The preparation method of the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material of this embodiment is carried out according to the following steps:

[0042] 1. According to the molecular formula of the antiperovskite manganese nitrogen compound reinforcement Mn3Zn 0.6 Sn 0.4 N, Mn3Zn 0.65 Sn 0.35 N, Mn3Zn 0.7 Sn 0.3 N, Mn3Zn 0.75 Sn 0.25 N, Mn3Zn 0.8 Sn 0.2 N were weighed, and briquetting and vacuum sintering were performed to obtain five antiperovskite manganese nitrogen compounds;

[0043] The raw materials are manganese dinitrogen, zinc powder and tin powder;

[0044] The vacuum sintering temperature is 850°C;

[0045] The vacuum degree of the vacuum sintering is 1×10 -5 Pa;

[0046] 2. Mix the multiple antiperovskite manganese nitrogen compounds obtained in step 1 to obtain a mixed powder, and then place it in a cast iron mold for pre-pressing to obtain a multi-antiperovskite manganese nitrogen compound; the mass ratio of each antiperovskite manganese nitrogen compound in the multi-antiperovskite manganese nitrogen compound is: Mn3Zn 0.6 Sn 0.4 N:Mn3Zn 0.65 Sn 0.35 N:Mn3Zn 0.7 Sn 0.3 N:Mn3Zn 0.75 Sn0.25 N:Mn3Zn 0.8 Sn 0.2 N = 0.35: 0.15: 0.23: 0.14: 0.13, the thermal expansion coefficient of the obtained perovskite manganese nitrogen compound is -30×10 -6 / ℃;

[0047] The size of the cast iron mold is 90 mm in diameter;

[0048] The pre-compression pressure is 5MPa;

[0049] 3. placing the cast iron mold containing the multi-phase perovskite manganese nitrogen compound in step 2 in a furnace for preheating;

[0050] The preheating temperature is 600°C;

[0051] The preheating time is 1h;

[0052] 4. pouring the molten matrix metal into a preheated iron mold, then performing pressure infiltration, and finally cooling and demoulding to obtain a multi-phase inverse perovskite manganese nitrogen compound / aluminum composite material; the volume fraction of the multi-phase inverse perovskite manganese nitrogen compound reinforcement in the composite material is 50%; the matrix alloy is an Al-Si alloy;

[0053] The temperature of the molten matrix metal is 800°C;

[0054] The pressure during the pressurized infiltration is 30MPa;

[0055] The time for the pressurized infiltration is 10 minutes.

[0056] Comparative Example: The preparation method of the single-phase reverse perovskite manganese nitrogen compound / aluminum composite material in this comparative example is different from that in Example 1 in that the reinforcement is a single-phase reverse perovskite manganese nitrogen compound Mn3Zn 0.7 Sn 0.3 N, other steps and parameters are the same as those in Example 1.

[0057] Figure 1 The thermal expansion curve of Example 1; in the figure, curve 1 is the single-phase reverse perovskite manganese nitrogen compound (Mn3Zn 0.7 Sn 0.3 N) / thermal expansion curve of the aluminum composite material; Curve 2 is the thermal expansion curve of the multi-phase perovskite manganese nitrogen compound / aluminum composite material prepared in step 4 of Example 1; Curve 3 is the thermal expansion curve of the multi-phase perovskite manganese nitrogen compound prepared in step 2 of Example 1; Figure 1 It can be seen that compared with the single-phase anti-perovskite manganese nitrogen compound / aluminum composite material, the temperature range of the near-zero expansion of the multi-phase designed anti-perovskite manganese nitrogen compound / aluminum composite material in Example 1 is expanded by 3 to 4 times. Figure 2 : is the bending stress-strain curve of the multi-inverse perovskite manganese nitrogen compound / aluminum composite material in Example 1. Example 1: First, a plurality of antiperovskite manganese nitrogen compounds with negative thermal expansion in different temperature ranges are prepared, and then the plurality of antiperovskite manganese nitrogen compounds are combined in a specific ratio, so that the multi-inverse perovskite manganese nitrogen compound has a negative thermal expansion coefficient of up to -30×10 -6 / ℃. The multi-phase perovskite manganese nitrogen compound / aluminum composite prepared by pressure infiltration inhibits the thermal expansion of the aluminum matrix in a wide temperature range. The thermal expansion coefficient of the composite material is only 0.40×10 -6 / ℃. At the same time, the bending strength can reach 211MPa and the thermal conductivity can reach 46W / (m·K), with excellent comprehensive performance.

[0058] Embodiment 2:

[0059] The preparation method of the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material of this embodiment is carried out according to the following steps:

[0060] 1. According to the molecular formula of the antiperovskite manganese nitrogen compound reinforcement Mn3Zn 0.7 Sn 0.2 Mn 0.1 N and Mn3Zn 0.53 Sn 0.27 Si 0.2 N respectively weighed the raw materials, and carried out briquetting and vacuum sintering respectively to obtain two kinds of antiperovskite manganese nitrogen compounds;

[0061] The raw materials are manganese dinitrogen, zinc powder, tin powder and silicon powder;

[0062] The vacuum sintering temperature is 800°C;

[0063] The vacuum degree of the vacuum sintering is 1×10 -5 Pa;

[0064] 2. Mixing the multiple antiperovskite manganese nitrogen compounds obtained in step 1 to obtain a mixed powder, and then placing it in a cast iron mold for pre-pressing to obtain multiple antiperovskite manganese nitrogen compounds;

[0065] The multi-phase perovskite manganese nitrogen compound Mn3Zn 0.7 Sn 0.2 Mn 0.1 N and Mn3Zn 0.53 Sn 0.27 Si 0.2 The mass fraction of N is 50%;

[0066] The size of the cast iron mold is 60 mm in diameter;

[0067] The pre-compression pressure is 10MPa;

[0068] 3. placing the cast iron mold containing the multi-phase perovskite manganese nitrogen compound in step 2 in a furnace for preheating;

[0069] The preheating temperature is 500°C;

[0070] The preheating time is 2h;

[0071] Fourth, pouring the molten matrix metal into a preheated iron mold, then performing pressure infiltration, and finally cooling and demolding to obtain three types of multi-phase inverse perovskite manganese nitrogen compound / aluminum composite materials (double inverse perovskite manganese nitrogen compound / aluminum composite materials); wherein the volume fraction of the multi-phase inverse perovskite manganese nitrogen compound reinforcement in the composite material is 35%, 50% and 60% respectively; the matrix alloy is Al-Si alloy;

[0072] The temperature of the molten matrix metal is 800°C;

[0073] The pressure during the pressurized infiltration is 30MPa;

[0074] The time for the pressurized infiltration is 10 minutes.

[0075] Example 2: A variety of antiperovskite manganese nitrogen compounds with negative thermal expansion in different temperature ranges are prepared, and then two antiperovskite manganese nitrogen compounds are combined in a specific ratio so that the negative thermal expansion coefficient of the antiperovskite manganese nitrogen compound can reach -25×10 -6 / ℃. The double-opposite perovskite manganese nitrogen compound / aluminum composites with different volume fractions were prepared by pressure infiltration, which suppressed the thermal expansion of the aluminum matrix in a wide temperature range. Figure 3 In the figure, curve 1 is the thermal expansion curve of the 35 vol.% bicontrast perovskite manganese nitrogen compound / aluminum composite material, curve 2 is the thermal expansion curve of the 50 vol.% bicontrast perovskite manganese nitrogen compound / aluminum composite material, and curve 3 is the thermal expansion curve of the 60 vol.% bicontrast perovskite manganese nitrogen compound / aluminum composite material. In the temperature range of -25 to 50 ° C, the thermal expansion coefficient of the 35 vol.% bicontrast perovskite manganese nitrogen compound / aluminum composite material is only 6×10 -6 / ℃; the thermal expansion coefficient of 50vol.% bi-opposite perovskite manganese nitrogen compound / aluminum composite material is only 1×10 -6 / ℃; the thermal expansion coefficient of 60vol.% bi-opposite perovskite manganese nitrogen compound / aluminum composite material is only -2×10 -6 / ℃;

[0076] Embodiment 3:

[0077] The preparation method of the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material of this embodiment is carried out according to the following steps:

[0078] 1. According to the molecular formula of the antiperovskite manganese nitrogen compound reinforcement Mn3Zn 0.8 Sn 0.2 N, Mn3Zn 0.77 Sn 0.23 N and Mn3Zn 0.7 Sn 0.3 N were weighed, and the raw materials were pressed and vacuum sintered to obtain three antiperovskite manganese nitrogen compounds;

[0079] The raw materials are manganese dinitrogen, zinc powder and tin powder;

[0080] The vacuum sintering temperature is 750°C;

[0081] The vacuum degree of the vacuum sintering is 1×10 -5 Pa;

[0082] 2. Mixing the multiple antiperovskite manganese nitrogen compounds obtained in step 1 to obtain a mixed powder, and then placing it in a cast iron mold for pre-pressing to obtain multiple antiperovskite manganese nitrogen compounds;

[0083] The mass ratio of each antiperovskite manganese nitrogen compound in the multi-antiperovskite manganese nitrogen compound is: Mn3Zn 0.8 Sn 0.2 N:Mn3Zn 0.77 Sn 0.23 N:Mn3Zn 0.7 Sn 0.3 N = 0.33: 0.33: 0.33;

[0084] The size of the cast iron mold is 60 mm in diameter;

[0085] The pre-compression pressure is 5MPa;

[0086] 3. placing the cast iron mold containing the multi-phase perovskite manganese nitrogen compound in step 2 in a furnace for preheating;

[0087] The preheating temperature is 540°C;

[0088] The preheating time is 2h;

[0089] 4. pouring the molten matrix metal into a preheated iron mold, then performing pressure infiltration, and finally cooling and demoulding to obtain a multi-phase inverse perovskite manganese nitrogen compound / aluminum composite material; the volume fraction of the multi-phase inverse perovskite manganese nitrogen compound reinforcement in the composite material is 50%; the matrix alloy is an Al-Si alloy;

[0090] The temperature of the molten matrix metal is 800°C;

[0091] The pressure during the pressurized infiltration is 30MPa;

[0092] The time for the pressurized infiltration is 10 minutes.

[0093] Figure 4 is a thermal expansion curve diagram in Example 3; Figure 4 In the figure, curve 1 is the thermal expansion curve of the multi-phase inverse perovskite manganese nitrogen compound obtained in step 2; curve 2 is the thermal expansion curve of the multi-phase inverse perovskite manganese nitrogen compound / aluminum composite material obtained in step 4; the multi-phase inverse perovskite manganese nitrogen compound obtained in step 2 has a negative thermal expansion coefficient of up to -14×10 -6 / ℃. The multi-phase perovskite manganese nitrogen compound / aluminum composite material obtained in step 4 has a thermal expansion coefficient of only 1×10 -6 / ℃.

Claims

1. A near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material in a wide temperature range, characterized in that: The wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material is composited by a multi-phase perovskite manganese nitrogen compound reinforcement and a matrix metal; the volume fraction of the multi-phase perovskite manganese nitrogen compound reinforcement in the composite material is 20-70%; The multi-phase perovskite manganese nitrogen compound reinforcement includes Mn3Zn 1-x Sn x N, Mn3Zn 1-x Ge x N, Mn3Zn 1-x- y Sn x Si y N, Mn3Zn 1-x Si x N, Mn3Zn 1-x-y Sn x Mn y N、Mn3Cu 1-x Sn x N、Mn3Cu 1-x Ge x N、Mn3Cu 1-x-y Sn x Si y N、Mn3Cu 1-x Si x N、Mn3Cu 1-x-y Sn x Mn y At least two of N, where 0 <x<1,0<y<1,0<x+y<1; The multi-phase perovskite manganese nitrogen compound Mn3Zn 1-x Sn x N, Mn3Zn 1-x Ge x N, Mn3Zn 1-x-y Sn x Si y N, Mn3Zn 1- x Si x N, Mn3Zn 1-x-y Sn x Mn y N、Mn3Cu 1-x Sn x N、Mn3Cu 1-x Ge x N、Mn3Cu 1-x-y Sn x Si y N、Mn3Cu 1-x Si x N、Mn3Cu 1-x-y Sn x Mn y The mass fraction of N is 0 to 50%.

2. The wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material according to claim 1, characterized in that: The base metal is pure aluminum or aluminum alloy.

3. The wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material according to claim 2, characterized in that: The aluminum alloy is one or a mixture of Al-Si alloy, Al-Cu alloy, Al-Mg alloy, Al-Si-Cu alloy, Al-Si-Mg alloy, Al-Cu-Mg alloy, Al-Zn-Cu alloy, Al-Zn-Mg-Cu alloy, Al-Be alloy, Al-Li alloy, and Al-Si-Cu-Mg alloy.

4. The method for preparing the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material according to claim 1, characterized in that: The preparation method of the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material is carried out according to the following steps:

1. According to the molecular formula of the antiperovskite manganese nitrogen compound reinforcement Mn3Zn 1-x Sn x N, Mn3Zn 1-x Ge x N, Mn3Zn 1-x- y Sn x Si y N, Mn3Zn 1-x Si x N, Mn3Zn 1-x-y Sn x Mn y N、Mn3Cu 1-x Sn x N、Mn3Cu 1-x Ge x N、Mn3Cu 1-x-y Sn x Si y N、Mn3Cu 1-x Si x N、Mn3Cu 1-x-y Sn x Mn y At least two of N are weighed as raw materials, and are pressed into blocks and vacuum sintered to obtain a plurality of antiperovskite manganese nitrogen compounds, wherein 0 <x<1,0<y<1,0<x+y<1; 2. Mixing the multiple antiperovskite manganese nitrogen compounds obtained in step 1 to obtain a mixed powder, and then placing it in a cast iron mold for pre-pressing to obtain multiple antiperovskite manganese nitrogen compounds; The multi-phase perovskite manganese nitrogen compound Mn3Zn 1-x Sn x N, Mn3Zn 1-x Ge x N, Mn3Zn 1-x-y Sn x Si y N, Mn3Zn 1- x Si x N, Mn3Zn 1-x-y Sn x Mn y N、Mn3Cu 1-x Sn x N、Mn3Cu 1-x Ge x N、Mn3Cu 1-x-y Sn x Si y N、Mn3Cu 1-x Si x N、Mn3Cu 1-x-y Sn x Mn y The mass fraction of N is 0 to 50%; 3. placing the cast iron mold containing the multi-phase perovskite manganese nitrogen compound in step 2 in a furnace for preheating; Fourth, pouring the molten matrix metal into a preheated iron mold, and then performing pressure infiltration, and finally cooling and demolding to obtain a multi-phase perovskite manganese nitrogen compound / aluminum composite material; the volume fraction of the multi-phase perovskite manganese nitrogen compound reinforcement in the composite material is 20-70%.

5. The method for preparing the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material according to claim 4, characterized in that: The raw material in step 1 is manganese dinitrogen, manganese tetranitrogen, zinc powder, tin powder, copper powder, germanium powder or silicon powder.

6. The method for preparing the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material according to claim 4, characterized in that: The temperature of the vacuum sintering in step 1 is 700-1000°C; the vacuum degree of the vacuum sintering is 1×10 -5 Pa~1×10 -4 Pa.

7. The method for preparing the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material according to claim 4, characterized in that: The pre-pressing pressure in step 2 is 2-20 MPa.

8. The method for preparing the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material according to claim 4, characterized in that: The preheating temperature in step 3 is 400-800° C. and the preheating time is 1-4 hours.

9. The method for preparing the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material according to claim 4, characterized in that: In step 4, the temperature of the molten base metal is 700-900°C.

10. The method for preparing the wide temperature range near-zero expansion multi-phase perovskite manganese nitrogen compound / aluminum composite material according to claim 4, characterized in that: The pressure during the pressurized infiltration in step 4 is 20 to 40 MPa; the time during the pressurized infiltration is 10 to 30 minutes.