Method for modifying interface of all-solid-state thin film lithium ion battery by piezoelectric material transition layer, all-solid-state thin film lithium ion battery
By introducing a piezoelectric material transition layer between the positive electrode film and the solid electrolyte film in an all-solid-state thin-film lithium-ion battery, the problems of interface instability and lithium-ion transport characteristics are solved, thereby improving battery performance.
Patent Information
- Application Number
- CN202210443531.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-04-25
AI Technical Summary
In all-solid-state thin-film lithium-ion batteries, chemical reactions exist at the cathode-electrolyte interface, leading to interface instability and poor lithium-ion transport characteristics, which limits the improvement of the battery's rate performance.
A piezoelectric material transition layer is introduced between the positive electrode film and the solid electrolyte film. The piezoelectric effect of the piezoelectric material is used to hinder chemical reactions and provide a fast lithium-ion transport channel.
It improves interface stability and electrochemical performance, significantly enhances lithium-ion transport kinetics, and improves the rate performance of the battery.
Smart Images

Figure CN116995307B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery technology, and more specifically to a method for modifying the interface of an all-solid-state thin-film lithium-ion battery with a piezoelectric material transition layer, and an all-solid-state thin-film lithium-ion battery. Background Technology
[0002] With the rapid development of microelectronics technology, miniaturized integrated circuit chips have an urgent need for correspondingly sized micro power supplies. They not only require higher energy density and power density, but also have higher requirements for small size and safety. Traditional battery systems cannot meet the needs of microelectronic systems for miniaturization and integration.
[0003] All-solid-state thin-film lithium-ion batteries are a new type of battery technology developed based on traditional lithium-ion batteries to meet these requirements. The working principle of all-solid-state thin-film lithium-ion batteries is similar to that of lithium-ion batteries: during charging, lithium ions are extracted from the positive electrode, and during discharging, lithium ions are inserted into the positive electrode material. Structurally, the solid electrolyte in all-solid-state thin-film lithium-ion batteries replaces the liquid electrolyte in lithium-ion batteries, and is formed by stacking a positive electrode, a solid electrolyte, and a negative electrode thin film on a substrate.
[0004] Since lithium-ion batteries rely solely on a planar electrode-electrolyte interface for lithium-ion transport, the interfacial lithium-ion transport characteristics are a crucial factor determining their electrochemical performance. Currently, the interface between the cathode film and the solid electrolyte film presents several challenges: it is prone to chemical reactions that form an unstable third phase, leading to significant interfacial impedance and continuous capacity decay during cycling; and the space charge layer effect at the two-phase interface, due to thermodynamic requirements for electrochemical potential balance, results in high interfacial resistance and poor lithium-ion transport characteristics, hindering rate performance improvements. Therefore, appropriate modification of the cathode-electrolyte interface is a potential method to improve the performance of all-solid-state thin-film lithium-ion batteries.
[0005] Currently, in all-solid-state thin-film lithium-ion batteries, the modification of the cathode-electrolyte interface mainly uses materials with poor electronic conductivity, such as Al2O3 and LiNbO3. Although these materials can hinder the chemical interaction between the cathode and electrolyte to improve interface stability and battery electrochemical performance when used as a modification layer, they cannot significantly improve the lithium-ion transport kinetics at the cathode-electrolyte interface, making it difficult to effectively improve its rate performance. Summary of the Invention
[0006] The purpose of this invention is to address the shortcomings of existing technologies by providing a method for modifying the interface of an all-solid-state thin-film lithium-ion battery with a piezoelectric material transition layer. By introducing a piezoelectric material transition layer between the positive electrode film and the solid electrolyte film, the lithium-ion transport kinetics at the positive electrode-electrolyte interface are effectively improved, thereby enhancing the rate performance of the battery, while simultaneously improving interface stability and the electrochemical performance of the battery.
[0007] According to a first aspect of the present invention, a method for modifying the interface of an all-solid-state thin-film lithium-ion battery with a piezoelectric material transition layer is provided, comprising sequentially depositing a positive electrode current collector layer, a positive electrode thin film, a piezoelectric material transition layer, a solid electrolyte thin film, a negative electrode thin film, and a negative electrode current collector layer on a substrate.
[0008] By introducing a piezoelectric transition layer between the positive electrode film and the solid electrolyte film, the interface formed by the piezoelectric transition layer is modified to prevent chemical reactions between the positive electrode film and the solid electrolyte film. The piezoelectric effect of the piezoelectric transition layer is used to provide a channel for rapid lithium-ion transport at the interface.
[0009] Preferably, a thin film deposition method is used to sequentially deposit a positive electrode current collector layer, a positive electrode thin film, a piezoelectric material transition layer, a solid electrolyte thin film, a negative electrode thin film, and a negative electrode current collector layer on a substrate.
[0010] Preferably, the specific deposition process of the piezoelectric material transition layer is as follows:
[0011] The substrate with the deposited positive current collector layer and positive thin film was fixed and placed in the magnetron sputtering chamber, and the chamber was evacuated until the internal gas pressure reached 10. -4 Below Pa;
[0012] Argon and oxygen are introduced into the evacuated chamber, the working pressure in the chamber is adjusted, the radio frequency magnetron sputtering mode is selected, and the power is adjusted to the required level.
[0013] A piezoelectric material transition layer is sputtered onto the positive electrode thin film.
[0014] Preferably, the flow rate ratio of argon to oxygen is (1-10):1, the working pressure in the chamber is 0.5-3 Pa, and the magnetron sputtering power is 40-150 W.
[0015] Preferably, the thickness of the piezoelectric material transition layer is 10–30 nm, the sputtering rate of the piezoelectric material transition layer is 1 nm / min, and the sputtering time is selected according to the required thickness of the piezoelectric material transition layer.
[0016] In a second aspect of the present invention, an all-solid-state thin-film lithium-ion battery is provided, which is prepared by the method of modifying the interface of an all-solid-state thin-film lithium-ion battery according to the aforementioned piezoelectric material transition layer.
[0017] Preferably, the thickness of the piezoelectric material transition layer is 10–30 nm.
[0018] Preferably, the piezoelectric material includes any one or more of barium titanate, lead titanate, lead zirconate titanate, lithium niobate, and lithium tantalate.
[0019] Preferably, the material of the positive electrode film includes lithium cobalt oxide, lithium nickel oxide, ternary materials and derivatives with a layered structure, lithium manganese oxide, lithium-rich ternary materials and derivatives with a spinel structure, and lithium iron phosphate, polyanionic materials and derivatives with an olivine structure.
[0020] Preferably, the material of the solid electrolyte film includes any one or a combination of lithium phosphate, lithium silicate, lithium silicon phosphate, lithium phosphorus oxynitride, lithium silicon oxynitride, and lithium phosphorus silicon oxynitride.
[0021] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0022] 1. The method of modifying the interface of an all-solid-state thin-film lithium-ion battery with a piezoelectric material transition layer of the present invention introduces a piezoelectric material transition layer between the positive electrode film and the solid electrolyte film. The piezoelectric material is uniformly modified on the positive electrode-electrolyte interface in the form of a transition layer film. By utilizing the piezoelectric effect of the piezoelectric material, the chemical interaction between the positive electrode film and the solid electrolyte film is hindered, while the adverse effects of the space charge layer present at the electrode-electrolyte interface on lithium-ion migration are effectively eliminated, and a fast lithium-ion transport channel is provided at the interface.
[0023] 2. The all-solid-state thin-film lithium-ion battery obtained by the method of the present invention has a piezoelectric material transition layer that improves the stability of the interface after hindering the chemical interaction between the positive electrode film and the solid electrolyte film, thereby improving the electrochemical performance of the battery.
[0024] Meanwhile, the presence of the piezoelectric material transition layer creates a positive electric field from the positive electrode to the negative electrode during charging, accelerating the migration of lithium ions from the positive electrode to the electrolyte; during discharging, it creates a negative electric field from the positive electrode to the negative electrode, accelerating the migration of lithium ions from the electrolyte to the positive electrode; this reduces the charge transfer impedance at the battery interface, significantly improves the lithium ion transport kinetics at the positive electrode-electrolyte interface, enhances the electrochemical reaction kinetics, and effectively improves the rate performance of all-solid-state thin-film lithium-ion batteries.
[0025] 3. The method of the present invention is simple, easy to master and control, conducive to industrial production, and has the prospect of further promotion and application. Attached Figure Description
[0026] Figure 1 This is a cross-sectional scanning electron microscope image of the all-solid-state thin-film lithium battery of Embodiment 1 of the present invention.
[0027] Figure 2 This is a comparison chart of the rate performance of Embodiments 1-3 and the comparative example of the present invention.
[0028] Figure 3 These are the AC impedance spectra of Embodiment 1 and the comparative example of the present invention. Detailed Implementation
[0029] To better understand the technical content of the present invention, specific embodiments are described below in conjunction with the accompanying drawings.
[0030] Various aspects of the invention are described in this disclosure with reference to the accompanying drawings, in which numerous illustrative embodiments are shown. The embodiments of this disclosure are not necessarily intended to encompass all aspects of the invention. It should be understood that the various concepts and embodiments described above, as well as those described below in more detail, can be implemented in any of a number of ways.
[0031] At present, there have been some research reports on piezoelectric materials in liquid lithium-ion batteries. The main purpose is to uniformly coat the surface of the positive electrode powder particles with piezoelectric materials, so as to inhibit the oxidation and decomposition of the electrolyte on the positive electrode surface and improve the lithium-ion diffusion coefficient and structural stability of the SEI film formed on the positive electrode surface.
[0032] This invention addresses the interface problems existing in all-solid-state thin-film lithium-ion batteries by providing a method for modifying the interface of all-solid-state thin-film lithium-ion batteries with a piezoelectric material transition layer. By introducing a piezoelectric material transition layer, the interface between the positive electrode film and the solid electrolyte film is modified, thereby improving the interface stability and electrochemical performance of the battery, as well as the rate performance of the battery.
[0033] In an exemplary embodiment of the present invention, a method for modifying the interface of an all-solid-state thin-film lithium-ion battery with a piezoelectric material transition layer is provided, comprising sequentially depositing a positive electrode current collector layer, a positive electrode thin film, a piezoelectric material transition layer, a solid electrolyte thin film, a negative electrode thin film, and a negative electrode current collector layer on a substrate;
[0034] By introducing a piezoelectric transition layer between the positive electrode film and the solid electrolyte film, the interface formed by the piezoelectric transition layer is modified to hinder the chemical reaction between the positive electrode film and the solid electrolyte film. The piezoelectric effect of the piezoelectric transition layer provides a channel for rapid lithium-ion transport at the interface, reduces the charge transfer impedance of the battery interface, and improves the electrochemical reaction kinetics.
[0035] In a preferred embodiment, a positive current collector layer, a positive electrode thin film, a piezoelectric material transition layer, a solid electrolyte thin film, a negative electrode thin film, and a negative current collector layer are sequentially deposited on a substrate using a thin film deposition method.
[0036] In a more preferred embodiment, the thin film deposition method includes at least one of magnetron sputtering, pulsed laser deposition, chemical vapor deposition, electron beam evaporation, and thermal evaporation, which can be selected according to the actual situation.
[0037] In a preferred embodiment, the specific deposition process of the piezoelectric material transition layer is as follows:
[0038] The substrate with the deposited positive current collector layer and positive thin film was fixed and placed in the magnetron sputtering chamber, and the chamber was evacuated until the internal gas pressure reached 10. -4 Below Pa;
[0039] Argon and oxygen are introduced into the evacuated chamber, the working pressure in the chamber is adjusted, the radio frequency magnetron sputtering mode is selected, and the power is adjusted to the required level.
[0040] A piezoelectric material transition layer is sputtered onto the positive electrode thin film.
[0041] In a preferred embodiment, the flow rate ratio of argon to oxygen is (1-10):1, the working pressure in the chamber is 0.5-3 Pa, and the magnetron sputtering power is 40-150 W.
[0042] In a preferred embodiment, the thickness of the piezoelectric material transition layer is 10–30 nm, the sputtering rate of the piezoelectric material transition layer is 1 nm / min, and the sputtering time is selected according to the required thickness of the piezoelectric material transition layer.
[0043] In a preferred embodiment, the substrate material can be alumina, silicon wafer, mica sheet, etc. The substrate only serves as a substrate and has almost no impact on the battery performance in this invention. Conventional substrates in the art can be used.
[0044] It should be understood that the deposition processes of the positive electrode current collector layer, positive electrode thin film, solid electrolyte thin film, negative electrode thin film, and negative electrode current collector layer are common technical means in this field, and those skilled in the art can choose them as needed, so they will not be described in detail here.
[0045] In another exemplary embodiment of the present invention, an all-solid-state thin-film lithium-ion battery prepared according to the aforementioned method of modifying the interface of an all-solid-state thin-film lithium-ion battery with a piezoelectric material transition layer is provided.
[0046] In a preferred embodiment, the thickness of the piezoelectric material transition layer is 10–30 nm.
[0047] In a preferred embodiment, the piezoelectric material includes any one or more of barium titanate, lead titanate, lead zirconate titanate, lithium niobate, and lithium tantalate.
[0048] In a preferred embodiment, the material of the positive electrode film includes lithium cobalt oxide, lithium nickel oxide, ternary materials and derivatives with a layered structure, lithium manganese oxide, lithium-rich ternary materials and derivatives with a spinel structure, and lithium iron phosphate, polyanionic materials and derivatives with an olivine structure.
[0049] In a preferred embodiment, the material of the solid electrolyte film includes any one or a combination of lithium phosphate, lithium silicate, lithium silicon phosphate, lithium phosphorus oxynitride, lithium silicon oxynitride, and lithium phosphorus silicon oxynitride.
[0050] The present invention will be further illustrated by the following examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or purchased directly from the market.
[0051]
Example 1
[0052] All-solid-state thin-film battery of lithium-rich manganese oxide modified with barium titanate piezoelectric transition layer
[0053] (1) Select an alumina substrate and sputter a platinum current collector: platinum is the target material, the working gas is argon at 60 sccm, the working pressure of the cavity is 1 Pa, the DC magnetron sputtering power is 60 W, and the sputtering time is 10 min.
[0054] (2) Sputtering lithium-rich manganese oxide cathode film: lithium-rich manganese oxide is used as the target material, the working gas is argon and oxygen at 60 sccm and 20 sccm respectively, the working gas pressure of the cavity is 1 Pa, the RF sputtering power is 120 W, and the sputtering time is 6 h.
[0055] (3) Prepare barium titanate piezoelectric material target, fix the prepared lithium manganese oxide thin film with a tray and place it in the magnetron sputtering chamber.
[0056] (4) Evacuate the cavity until the internal air pressure reaches 10. -4 Below Pa.
[0057] (5) Argon and oxygen are introduced at flow rates of 60 sccm and 20 sccm respectively. The working pressure of the cavity is adjusted to 1 Pa. The radio frequency magnetron sputtering mode is selected and the power is adjusted to 100 W.
[0058] (6) The sputtering time is set to 20 min.
[0059] (7) Sputtering lithium phosphorus oxygen nitrogen solid electrolyte: lithium phosphate is used as the target material, the working gas is nitrogen at 80 sccm, the working pressure of the cavity is 1 Pa, the RF sputtering power is 120 W, and the sputtering time is 15 h.
[0060] (8) Sputtering of lithium and copper current collectors: Lithium was prepared by thermal evaporation with a heating power of 20W. Copper was used as the target material, the working gas was argon at 60 sccm, the working pressure of the cavity was 1 Pa, the DC magnetron sputtering power was 50W, and the sputtering time was 10 min.
[0061]
Example 2
[0062] The difference between this embodiment and embodiment 1 is that the sputtering time in step (6) is 10 minutes, while the other steps are the same.
[0063]
Example 3
[0064] The difference between this embodiment and embodiment 1 is that the sputtering time in step (6) is 30 minutes, while the other steps are the same.
[0065]
Example 4
[0066] Lithium cobalt oxide all-solid-state thin-film battery modified with lead zirconate titanate piezoelectric transition layer
[0067] (1) Select an alumina substrate and sputter a platinum current collector: platinum is the target material, the working gas is argon at 60 sccm, the working pressure of the cavity is 1 Pa, the DC magnetron sputtering power is 60 W, and the sputtering time is 10 min.
[0068] (2) Sputtering lithium cobalt oxide cathode film: Lithium cobalt oxide is used as the target material, the working gas is argon and oxygen at 60 sccm and 20 sccm, the working gas pressure of the cavity is 1 Pa, the RF sputtering power is 150 W, and the sputtering time is 4 h.
[0069] (3) Prepare lead zirconate titanate piezoelectric material target, fix the prepared lithium cobalt oxide film with a tray and place it in the magnetron sputtering chamber.
[0070] (4) Evacuate the cavity until the internal air pressure reaches 10. -4 Below Pa.
[0071] (5) Argon and oxygen are introduced at flow rates of 40 sccm and 40 sccm respectively. The working pressure of the cavity is adjusted to 2 Pa. The radio frequency magnetron sputtering mode is selected and the power is adjusted to 150 W.
[0072] (6) The sputtering time is set to 10 min.
[0073] (7) Sputtering lithium silicon phosphate solid electrolyte: lithium silicon phosphate is used as the target material, the working gas is argon at 80 sccm, the working pressure of the cavity is 1 Pa, the RF sputtering power is 120 W, and the sputtering time is 15 h.
[0074] (8) Sputtering of lithium and copper current collectors: Lithium was prepared by thermal evaporation with a heating power of 20W. Copper was used as the target material, the working gas was argon at 60 sccm, the working pressure of the cavity was 1 Pa, the DC magnetron sputtering power was 50W, and the sputtering time was 10 min.
[0075]
Example 5
[0076] Lithium iron phosphate all-solid-state thin-film battery modified with lithium niobate piezoelectric transition layer
[0077] (1) Select an alumina substrate and sputter a platinum current collector: platinum is the target material, the working gas is argon at 60 sccm, the working pressure of the cavity is 1 Pa, the DC magnetron sputtering power is 60 W, and the sputtering time is 10 min.
[0078] (2) Sputtering lithium iron phosphate cathode film: lithium iron phosphate is used as the target material, the working gas is argon and oxygen at 60 sccm and 10 sccm, the working pressure of the cavity is 1 Pa, the RF sputtering power is 160 W, and the sputtering time is 4 h.
[0079] (3) Prepare lithium niobate piezoelectric material target, fix the prepared lithium iron phosphate film with a tray and place it in the magnetron sputtering chamber.
[0080] (4) Evacuate the cavity until the internal air pressure reaches 10. -4 Below Pa.
[0081] (5) Argon and oxygen are introduced at flow rates of 70 sccm and 10 sccm respectively. The working pressure of the cavity is adjusted to 0.5 Pa. The radio frequency magnetron sputtering mode is selected and the power is adjusted to 60 W.
[0082] (6) The sputtering time is set to 20 min.
[0083] (7) Sputtering lithium phosphorus silicon oxygen nitrogen solid electrolyte: lithium silicon phosphate is used as the target material, the working gas is nitrogen at 80 sccm, the working pressure of the cavity is 1 Pa, the RF sputtering power is 120 W, and the sputtering time is 15 h.
[0084] (8) Sputtering of lithium and copper current collectors: Lithium was prepared by thermal evaporation with a heating power of 20W. Copper was used as the target material, the working gas was argon at 60 sccm, the working pressure of the cavity was 1 Pa, the DC magnetron sputtering power was 50W, and the sputtering time was 10 min.
[0085]
Example 6
[0086] Lithium manganese oxide all-solid-state thin-film battery modified with lead titanate piezoelectric transition layer
[0087] (1) Select an alumina substrate and sputter a platinum current collector: platinum is the target material, the working gas is argon at 60 sccm, the working pressure of the cavity is 1 Pa, the DC magnetron sputtering power is 60 W, and the sputtering time is 10 min.
[0088] (2) Sputtering lithium manganese oxide cathode film: Lithium manganese oxide is used as the target material, the working gas is argon and oxygen at 60 sccm and 20 sccm, the working gas pressure of the cavity is 1 Pa, the RF sputtering power is 100 W, and the sputtering time is 4 h.
[0089] (3) Prepare lead titanate piezoelectric material target, fix the prepared lithium manganese oxide film with a tray and place it in the magnetron sputtering chamber.
[0090] (4) Evacuate the cavity until the internal air pressure reaches 10. -4 Below Pa.
[0091] (5) Argon and oxygen are introduced at flow rates of 100 sccm and 10 sccm respectively. The working pressure of the cavity is adjusted to 3 Pa. The radio frequency magnetron sputtering mode is selected and the power is adjusted to 40 W.
[0092] (6) The sputtering time is set to 30 min.
[0093] (7) Sputtering lithium phosphate solid electrolyte: lithium phosphate is used as the target material, the working gas is argon at 80 sccm, the working pressure of the cavity is 1 Pa, the RF sputtering power is 120 W, and the sputtering time is 15 h.
[0094] (8) Sputtering of lithium and copper current collectors: Lithium was prepared by thermal evaporation with a heating power of 20W. Copper was used as the target material, the working gas was argon at 60 sccm, the working pressure of the cavity was 1 Pa, the DC magnetron sputtering power was 50W, and the sputtering time was 10 min.
[0095]
Example 7
[0096] Lithium nickel oxide all-solid-state thin-film battery modified with lithium tantalate piezoelectric transition layer
[0097] (1) Select an alumina substrate and sputter a platinum current collector: platinum is the target material, the working gas is argon at 60 sccm, the working pressure of the cavity is 1 Pa, the DC magnetron sputtering power is 60 W, and the sputtering time is 10 min.
[0098] (2) Sputtering lithium nickelate cathode film: lithium nickelate is used as the target material, the working gas is argon and oxygen at 60 sccm and 20 sccm, the working gas pressure of the cavity is 1 Pa, the RF sputtering power is 120 W, and the sputtering time is 5 h.
[0099] (3) Prepare lithium tantalate piezoelectric material target, fix the prepared lithium nickelate film with a tray and place it in the magnetron sputtering chamber.
[0100] (4) Evacuate the cavity until the internal air pressure reaches 10. -4 Below Pa.
[0101] (5) Argon and oxygen are introduced at flow rates of 60 sccm and 20 sccm respectively. The working pressure of the cavity is adjusted to 2 Pa. The radio frequency magnetron sputtering mode is selected and the power is adjusted to 120 W.
[0102] (6) The sputtering time is set to 10 min.
[0103] (7) Sputtering lithium silicate solid electrolyte: Lithium silicate is used as the target material, the working gas is argon at 80 sccm, the working pressure of the cavity is 1 Pa, the RF sputtering power is 120 W, and the sputtering time is 15 h.
[0104] (8) Sputtering of lithium and copper current collectors: Lithium was prepared by thermal evaporation with a heating power of 20W. Copper was used as the target material, the working gas was argon at 60 sccm, the working pressure of the cavity was 1 Pa, the DC magnetron sputtering power was 50W, and the sputtering time was 10 min.
[0105] [Comparative Example]
[0106] The difference in this comparative example 1 is that the sputtering time in step (6) is 0 min, while the other steps are the same.
[0107] SEM
[0108] Cross-sectional scanning electron microscope (SEM) images of the all-solid-state thin-film lithium-ion battery constructed in Example 1 are shown below. Figure 1 As shown
[0109] from Figure 1 Information such as the thickness and growth rate of each component film can be obtained. The top 2.5 μm thick layer is the lithium metal and copper metal current collector, the next 2.5 μm thick layer is the lithium phosphorus oxygen nitrogen solid electrolyte, then there is a 20 nm thick barium titanate transition layer and a 470 nm thick lithium-rich manganese oxide cathode, and at the bottom are the cathode current collector and the alumina substrate.
[0110] Therefore, it can be proven that the present invention has successfully prepared an all-solid-state thin-film lithium-ion battery with a piezoelectric material transition layer modification.
[0111] Since the barium titanate transition layer was sputtered for only 20 minutes and was only 20 nm thick, the barium titanate transition layer was almost invisible in the entire all-solid-state thin-film battery. However, the connection between the positive electrode and the solid electrolyte film was very tight, and no obvious interface appeared.
[0112] The above results demonstrate that the piezoelectric material transition layer is nanoscale and highly dense, and its introduction does not alter the original structure of the all-solid-state thin-film battery, thus ensuring battery performance. On the other hand, it indicates that the introduction of the transition layer can prevent the solid electrolyte from directly contacting the positive electrode during sputtering, thereby hindering the chemical interaction between the positive electrode and the electrolyte, and improving interface stability and the electrochemical performance of the battery.
[0113] Ratio performance
[0114] Rate performance tests were conducted on the all-solid-state thin-film lithium-ion batteries of Examples 1, 2, 3, and the comparative example. The results are as follows: Figure 2 As shown.
[0115] As can be seen, the initial specific capacities of Examples 1, 2, and the comparative example at a current density of 0.5C are similar, all around 120 mAh / g. However, as the current density increases, the advantages of the barium titanate transition layer modification gradually become apparent. At 5C, the specific capacities of Examples 1 and 2 both exceed those of the comparative example, i.e., the unmodified lithium manganese oxide material, with Example 1 showing better performance.
[0116] Example 3 differs from the others in that it exhibits a significant capacity loss at low current densities, with a specific capacity of only 90 mAh / g at 0.5C. However, its rate performance is excellent, with a specific capacity of around 80 mAh / g at a current density of 5C, which is even higher than the capacity under the other three conditions.
[0117] Therefore, the following conclusions can be drawn: the introduction of barium titanate transition layer can utilize the piezoelectric effect of the modification layer material to effectively eliminate the adverse effects of the space charge layer at the electrode-electrolyte interface on lithium ion migration, and can provide a fast lithium ion transport channel at the interface, thereby greatly improving the rate performance of lithium-rich manganese oxide in all-solid-state thin-film batteries.
[0118] When the thickness of the barium titanate transition layer is less than 30 nm, its rate performance increases with the increase of the thickness of the barium titanate transition layer. However, at low current densities, an excessively thick barium titanate transition layer will inhibit the release of its capacity, specifically manifested as a sharp decrease in specific capacity when the barium titanate thickness exceeds 20 nm.
[0119] Therefore, without affecting its capacity under low current density, the deposition of a 20 nm thick barium titanate transition layer in Example 1 is the optimal modification condition.
[0120] Charge transfer impedance at the battery interface
[0121] Charge transfer impedance tests were performed on the all-solid-state thin-film lithium-ion batteries of Example 1 and the comparative example. The current density during the test was 0.5C, and the results are as follows. Figure 3 As shown.
[0122] An AC impedance spectrum consists of a semicircle representing charge transfer impedance and a diagonal line representing lithium-ion diffusion impedance. Figure 3 As can be seen, the semicircle diameter of Example 1 is significantly smaller than that of the comparative example, indicating that the charge transfer impedance of Example 1 is much smaller than that of the comparative example. This demonstrates that the addition of the barium titanate transition layer reduces the charge transfer impedance at the battery interface, improves the electrochemical reaction kinetics, and thus enhances the overall electrochemical performance of the all-solid-state thin-film battery.
[0123] This further demonstrates that the all-solid-state thin-film lithium-ion battery obtained by the method of the present invention can provide a fast lithium-ion transport channel at the interface, thereby reducing the charge transfer impedance at the battery interface, improving electrochemical reaction kinetics, and effectively enhancing the rate performance of the all-solid-state thin-film lithium-ion battery.
[0124] While the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the invention. Those skilled in the art can make various modifications and refinements without departing from the spirit and scope of the invention. Therefore, the scope of protection of the present invention shall be determined by the claims.
Claims
1. A method for modifying the interface of an all-solid-state thin-film lithium-ion battery with a piezoelectric material transition layer, characterized in that, This includes the sequential deposition of a positive electrode current collector layer, a positive electrode thin film, a piezoelectric material transition layer, a solid electrolyte thin film, a negative electrode thin film, and a negative electrode current collector layer on a substrate. The solid electrolyte film is made of any one or a combination of lithium phosphate, lithium silicate, lithium silicon phosphate, lithium phosphorus oxynitride, lithium silicon oxynitride, and lithium phosphorus silicon oxynitride. The piezoelectric material includes any one or more of barium titanate, lead titanate, and lead zirconate titanate; the thickness of the piezoelectric material transition layer is 10~30 nm; the specific deposition process of the piezoelectric material transition layer is as follows. The substrate with the deposited positive current collector layer and positive thin film was fixed and placed in the magnetron sputtering chamber, and the chamber was evacuated until the internal gas pressure reached 10. -4 Below Pa; Argon and oxygen are introduced into the evacuated chamber, the working pressure in the chamber is adjusted, the radio frequency magnetron sputtering mode is selected, and the power is adjusted to the required level. The flow rate ratio of argon to oxygen is (1~10):1, the working pressure in the chamber is 0.5~3Pa, and the magnetron sputtering power is 40~150 W. A piezoelectric transition layer was sputtered onto the positive electrode film at a sputtering rate of 1 nm / min. By introducing a piezoelectric transition layer between the positive electrode film and the solid electrolyte film, the interface formed by the piezoelectric transition layer is modified to prevent chemical reactions between the positive electrode film and the solid electrolyte film. The piezoelectric effect of the piezoelectric transition layer is used to provide a channel for rapid lithium-ion transport at the interface.
2. The method for modifying the interface of an all-solid-state thin-film lithium-ion battery with a piezoelectric material transition layer according to claim 1, characterized in that, A positive electrode current collector layer, a positive electrode thin film, a piezoelectric material transition layer, a solid electrolyte thin film, a negative electrode thin film, and a negative electrode current collector layer are sequentially deposited on a substrate using a thin film deposition method.
3. The method for modifying the interface of an all-solid-state thin-film lithium-ion battery with a piezoelectric material transition layer according to claim 1, characterized in that, The sputtering time of piezoelectric materials is selected based on the required thickness of the piezoelectric material transition layer.
4. An all-solid-state thin-film lithium-ion battery prepared by a method for modifying the interface of an all-solid-state thin-film lithium-ion battery with a piezoelectric material transition layer according to any one of claims 1-3.
5. The all-solid-state thin-film lithium-ion battery according to claim 4, characterized in that, The materials of the cathode film include lithium cobalt oxide, lithium nickel oxide, ternary materials and derivatives with layered structures, lithium manganese oxide, lithium-rich ternary materials and derivatives with spinel structures, and lithium iron phosphate, polyanionic materials and derivatives with olivine structures.
Citation Information
Patent Citations
Lithium battery
CN101388470A
Lithium battery positive plate and solid electrolyte combined plate and preparation method thereof
CN111916836A