Preparation and application method of fire-proof and extinguishing material for three-dimensional space in coal mines

Through the combination of modified retardant and composite foaming agent, an efficient fire prevention and extinguishing material is formed, which solves the problem of insufficient plugging performance of coal spontaneous combustion in coal mines and achieves efficient fire prevention and extinguishing effects, with a retardant rate of 83.28%-86.21%. , and reduce the spread of toxic gases.

CN117018528BActive Publication Date: 2024-10-11HUBEI YIZHI TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310761274.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-27
Publication Date
2024-10-11
Estimated Expiration
2043-06-27

AI Technical Summary

Technical Problem

Among the existing coal mine fire prevention and extinguishing technologies, the leakage plugging performance is poor and it is difficult to effectively suppress coal spontaneous combustion. The chemical resistance and thermal stability of traditional fire prevention and extinguishing materials are insufficient.

Method used

Using a combination of modified inhibitors, composite foaming agents and auxiliaries, the modified inhibitors are prepared through the chemical reaction of modified lignin, carboxyl-terminated organosilicon compounds and p-toluenesulfonic acid, combined with composite foaming agents and auxiliaries. The agent forms a high-efficiency fire prevention and extinguishing material, and forms a liquid film on the surface of the coal body through spraying construction, cutting off the contact between the coal body and oxygen, and blocking the spontaneous combustion of the coal body.

Benefits of technology

Significantly improves the resistance rate of fire-proof and extinguishing materials to 83.28%-86.21%, and achieves fire-proof and extinguishing functions by inhibiting the exothermic reaction of active groups in the coal body and isolating oxygen suffocation, significantly reducing the spread of toxic and harmful gases, and preventing gas and Water gas explodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a preparation method and application method of a fire-proof material for three-dimensional space in underground coal mines, which belongs to the technical field of fireproof materials. The preparation method of the fire-proof material includes the following steps: mixing and stirring a modified inhibitor, an auxiliary agent and water to obtain a main material; stirring a composite foaming agent and water at a high speed to obtain a foaming component; adding the foaming component to the main material, mixing and stirring to obtain the fire-proof material. The fire-proof material is covered on the surface of the coal body and gradually penetrates into the interior of the coal body as the liquid is precipitated. A chain reaction is carried out between the active groups in the coal body to produce a strong binding effect, thereby achieving the purpose of inhibiting the exothermic reaction between the active groups in the coal body. At the same time, the fire-proof material blocks the development of spontaneous combustion of the coal body, thereby finally achieving the purpose of inhibiting spontaneous combustion of the coal body. Finally, the fire-proof material prepared by the invention has a retardation rate of 83.28%-86.21%, and has excellent retardation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fireproof materials, and in particular relates to a preparation method and an application method of a fireproof and extinguishing material for three-dimensional space underground in a coal mine. Background Art

[0002] According to statistics, fires caused by spontaneous combustion of coal in my country account for more than 90% of the total number of coal mine fires.

[0003] The coal-oxygen complex theory of the cause of coal spontaneous combustion believes that coal spontaneous combustion is mainly caused by air infiltration into the loose coal body, and the oxygen in the air contacts the active structure on the surface of the coal molecules, causing physical adsorption, chemical adsorption and chemical reaction, while releasing heat. Under a certain heat storage environment, the coal body continues to heat up and reaches the ignition point temperature, which eventually leads to coal combustion. Among the various factors that cause coal spontaneous combustion, air infiltration (leakage) is one of the important factors.

[0004] Therefore, the traditional coal fire prevention and extinguishing technology mainly focuses on plugging, such as yellow mud grouting, loess filling and fly ash filling, which still have the problem of poor plugging performance. In the prior art, fire prevention and extinguishing materials have been developed that use chemical reagents to directly cover the coal body to form flame retardant substances. For example, Chinese patent CN112999558B discloses a coal mine underground fire prevention and extinguishing material and its preparation process. The fire prevention and extinguishing material is prepared by mixing polymer materials, fly ash, cross-linking agent composite materials, calcium sulfate whiskers, foaming agents, etc., with low raw material cost and simple preparation process. It uses the synergistic effect of various raw materials to carry out fire prevention and extinguishing in all directions, and finally prepares a fire prevention and extinguishing material with excellent chemical resistance and excellent thermal stability. Summary of the invention

[0005] The present invention provides a novel fire-proof and extinguishing material, aiming to improve the chemical resistance performance of the fire-proof and extinguishing material. Furthermore, the present invention discloses an application method of the fire-proof and extinguishing material, aiming to improve the application efficiency of the fire-proof and extinguishing material in the three-dimensional space of an underground coal mine.

[0006] The purpose of the present invention is to provide a preparation of a fire-proof and extinguishing material for a three-dimensional space in a coal mine;

[0007] Another object of the present invention is to disclose an application method of the above fire extinguishing material.

[0008] The purpose of the present invention can be achieved through the following technical solutions:

[0009] A method for preparing a three-dimensional space fire extinguishing material for underground coal mines comprises the following steps:

[0010] S1, mixing and stirring the modified inhibitor, the auxiliary agent and water to obtain the main material;

[0011] S2, stirring the composite foaming agent and water at high speed for 10 minutes to obtain a foaming component;

[0012] S3, adding the foaming component to the main material, mixing and stirring for 20 minutes to obtain a fire extinguishing material;

[0013] The modified inhibitor is prepared by the following steps:

[0014] Add modified lignin, carboxyl-terminated organosilicon compound and p-toluenesulfonic acid to N,N-dimethylformamide, raise the temperature to 85-90°C, reflux and stir to react for 4 hours, and after the reaction is completed, cool to 45-50°C and perform vacuum rotary evaporation to obtain a modified inhibitor.

[0015] Furthermore, the dosage ratio of the modified inhibitor, the auxiliary agent and water is 70g:1.2-1.5g:100mL;

[0016] The usage ratio of the composite foaming agent to water is 0.8-1.0 g:100 mL.

[0017] Furthermore, the auxiliary agent is prepared by mixing n-butanol, sodium benzoate and sodium dodecyl sulfate in a mass ratio of 1:1:1.

[0018] Furthermore, the composite foaming agent is compounded by sodium α-olefin sulfonate and a zwitterionic surfactant in a volume ratio of 7:3; the zwitterionic surfactant is one of cocamidopropyl betaine, stearamidopropyl betaine and lauramidopropyl betaine.

[0019] Furthermore, the dosage ratio of the N,N-dimethylformamide, the modified lignin, the carboxyl-terminated organosilicon compound and p-toluenesulfonic acid is 200 mL: 55-60 g: 22-23 g: 0.8-1.0 g.

[0020] Furthermore, the modified lignin is prepared by the following steps:

[0021] A1. Add half of the total amount of 37% formaldehyde aqueous solution and melamine to deionized water with stirring, heat to 85-90° C., stir and react for 2 hours to obtain a mixed solution;

[0022] A2. Add lignin to the mixed solution, stir for 30 minutes, then add the remaining 37% formaldehyde aqueous solution, stir for 30 minutes, then add 70wt% phytic acid aqueous solution, keep the temperature constant at 85-90°C, stir and react for 5 hours. After the reaction is completed, cool to room temperature, vacuum filter, collect the precipitate, wash the precipitate with deionized water to a pH value of 7.0, and dry the washed product at 80°C for 12 hours to obtain modified lignin.

[0023] Furthermore, the usage ratio of the deionized water, 37% formaldehyde aqueous solution, melamine, lignin, and 70wt% phytic acid aqueous solution is 300mL: 20mL: 1.2-1.25moL: 9.2-9.5g: 15.5-16.0mL.

[0024] Furthermore, the carboxyl-terminated organosilicon compound is prepared by the following steps:

[0025] Add silane coupling agent KH-550 and succinic anhydride to N,N-dimethylformamide, stir for 3 hours, filter, wash the filter cake with anhydrous ethanol and distilled water three times respectively, and then dry to constant weight to obtain a carboxyl-terminated organosilicon compound. The structure of the carboxyl-terminated organosilicon compound is as follows:

[0026] .

[0027] Furthermore, the dosage ratio of the N,N-dimethylformamide, the silane coupling agent KH-550 and the succinic anhydride is 250mL:0.1moL:0.1moL.

[0028] As a preferred technical solution of the present invention, the method for applying the fire extinguishing material in the three-dimensional space of a coal mine comprises the following steps:

[0029] B1. Mix the above main ingredients and foaming components in a mass ratio of 1:1.2 and stir for 20 minutes to obtain a fire extinguishing material;

[0030] B2. Spraying of fire-proof and extinguishing materials is carried out, wherein the outlet direction of the spray gun is 45-55° to the plane of the coal body, the spraying pressure is 2.5-2.8MPa, the single spraying thickness is 3-5mm, the spraying cycle is 2-3 times, and the spraying interval time is 2h. After the spraying is completed, the application of the fire-proof and extinguishing materials is completed.

[0031] Beneficial effects of the present invention:

[0032] The fire-proof material prepared by the present invention is composed of a modified inhibitor, a composite foaming agent, an auxiliary agent and water. Through the detection of lignite ore samples, the fire-proof material prepared by the present invention has a retardation rate of 83.28%-86.21%, and has excellent retardation performance. In the preparation process of the modified inhibitor, the present invention first uses phytic acid to modify lignin through a Mannich chemical reaction, and grafts phytic acid onto lignin through melamine. Lignin contains abundant hydroxyl groups. The present invention introduces a triazine structure into the modified lignin. The present invention then uses a silane coupling agent KH-550 and succinic anhydride to undergo an amidation reaction to obtain an organosilicon compound containing a terminal carboxyl group. The modified lignin and the organosilicon compound containing a terminal carboxyl group undergo a polymerization reaction under the action of p-toluenesulfonic acid to obtain a modified inhibitor. The modified inhibitor prepared by the present invention has both silicon and nitrogen flame retardant properties. At the same time, the modified inhibitor has a hyperbranched structure and has a large spatial steric hindrance, which is helpful to improve the dispersion performance of the fire extinguishing material. Finally, the modified inhibitor contains a large amount of hydroxyl and triazine structures. The nitrogen elements in the hydroxyl and triazine structures can form coordination bonds with metal ions in the coal body, thereby improving the adsorption performance of the modified inhibitor and the coal body. The fire-proof and extinguishing material of the present invention covers the surface of the coal body and gradually penetrates into the interior of the coal body as the liquid is precipitated. The modified inhibitor in the fire-proof and extinguishing material undergoes a chain reaction with the active groups in the coal body (alkyl side chains, oxygen-containing groups, sulfur-containing groups and nitrogen-containing groups in the coal molecules, etc.), generating a strong binding effect, thereby achieving the purpose of inhibiting the exothermic reaction between the active groups in the coal body. At the same time, the modified inhibitor and the free radicals on the surface of the coal body (free radicals generated by the breakage of the side chains of the coal molecules during the low-temperature oxidation of coal) undergo a chemical reaction, thereby blocking the development of spontaneous combustion of the coal body. Through the above effects, the purpose of inhibiting the spontaneous combustion of the coal body is ultimately achieved, and the fire-proof and extinguishing function is achieved by inhibiting the spontaneous combustion of the coal body.

[0033] At the same time, the fire-proofing material of the present invention forms a liquid film on the surface of the coal body through the effect of the film-forming agent, thereby isolating the coal body from further contact with oxygen, achieving the purpose of inhibition through oxygen isolation and suffocation, and achieving the fire-proofing function through inhibition. At the same time, the formation of the liquid film can greatly reduce the diffusion of toxic and harmful gases, and play a role in inhibiting the combustion and explosion of gas and water gas.

[0034] Finally, the present invention discloses an application method of fire-proof and extinguishing materials. The application method of the present invention realizes efficient application of fire-proof and extinguishing materials in the three-dimensional space of underground coal mines by controlling parameters such as spray gun outlet direction, spraying pressure and spraying thickness. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] Preparation of modified lignin:

[0038] A1. Add 300 mL of deionized water into the reactor, then add 10 mL of 37% formaldehyde aqueous solution and 1.2 mol of melamine into the reactor with stirring, heat the reactor to 85°C, stir and react for 2 h to obtain a mixed solution;

[0039] A2. Add 9.2 g of lignin (alkaline lignin, a product of Shanghai MacLean Biochemical Technology Co., Ltd.) to the mixed solution, stir for 30 minutes, then add 10 mL of 37% formaldehyde aqueous solution, stir for 30 minutes, then add 15.5 mL of 70 wt % phytic acid aqueous solution (a product of Shanghai Aladdin Biochemical Technology Co., Ltd.), control the reactor temperature to be constant at 85°C, stir and react for 5 hours, after the reaction is completed, cool to room temperature, vacuum filter, collect the precipitate, wash the precipitate repeatedly with deionized water until the pH value of the washed filtrate reaches 7.0, and dry the washed product in a vacuum oven at 80°C for 12 hours to obtain modified lignin.

[0040] Example 2

[0041] Preparation of modified lignin:

[0042] A1. Add 300 mL of deionized water into the reactor, then add 10 mL of 37% formaldehyde aqueous solution and 1.22 mol of melamine into the reactor with stirring, heat the reactor to 88°C, stir and react for 2 h to obtain a mixed solution;

[0043] A2. Add 9.4 g of lignin (alkaline lignin, a product of Shanghai MacLean Biochemical Technology Co., Ltd.) to the mixed solution, stir for 30 minutes, then add 10 mL of 37% formaldehyde aqueous solution, stir for 30 minutes, then add 15.8 mL of 70 wt % phytic acid aqueous solution (a product of Shanghai Aladdin Biochemical Technology Co., Ltd.), control the reactor temperature to be constant at 88°C, stir and react for 5 hours, after the reaction is completed, cool to room temperature, vacuum filter, collect the precipitate, wash the precipitate repeatedly with deionized water until the pH value of the washed filtrate reaches 7.0, and dry the washed product in a vacuum oven at 80°C for 12 hours to obtain modified lignin.

[0044] Example 3

[0045] Preparation of modified lignin:

[0046] A1. Add 300 mL of deionized water into the reactor, then add 10 mL of 37% formaldehyde aqueous solution and 1.25 mol of melamine into the reactor with stirring, heat the reactor to 90°C, stir and react for 2 hours to obtain a mixed solution;

[0047] A2. Add 9.5 g of lignin (alkaline lignin, a product of Shanghai MacLean Biochemical Technology Co., Ltd.) to the mixed solution, stir for 30 minutes, then add 10 mL of 37% formaldehyde aqueous solution, stir for 30 minutes, then add 16.0 mL of 70 wt % phytic acid aqueous solution (a product of Shanghai Aladdin Biochemical Technology Co., Ltd.), control the reactor temperature to be constant at 90°C, stir and react for 5 hours, after the reaction is completed, cool to room temperature, vacuum filter, collect the precipitate, wash the precipitate repeatedly with deionized water until the pH value of the washed filtrate reaches 7.0, and dry the washed product in a vacuum oven at 80°C for 12 hours to obtain modified lignin.

[0048] Example 4

[0049] Preparation of carboxyl-terminated organosilicon compounds:

[0050] Add 250 mL of N,N-dimethylformamide to the reactor, add 0.1 mol of silane coupling agent KH-550 and 0.1 mol of succinic anhydride, and stir for 3 hours. After stirring, filter and wash the filter cake three times with anhydrous ethanol and distilled water respectively, and finally dry at 80°C to constant weight to obtain a carboxyl-terminated organosilicon compound.

[0051] Example 5

[0052] Preparation of modified inhibitor:

[0053] Add 200 mL of N,N-dimethylformamide to the reactor, and continue to add 55 g of the modified lignin prepared in Example 1, 22 g of the terminal carboxyl organosilicon compound prepared in Example 4 and 0.8 g of p-toluenesulfonic acid. Heat the reactor to 85 ° C, reflux and stir to react for 4 hours. After the reaction is completed, cool to 45 ° C and evaporate under reduced pressure to obtain a modified inhibitor.

[0054] Example 6

[0055] Preparation of modified inhibitor:

[0056] Add 200 mL of N,N-dimethylformamide to the reactor, and continue to add 58 g of the modified lignin prepared in Example 2, 23 g of the terminal carboxyl organosilicon compound prepared in Example 4 and 0.9 g of p-toluenesulfonic acid. Heat the reactor to 88 ° C, reflux and stir to react for 4 hours. After the reaction is completed, cool to 47 ° C and evaporate under reduced pressure to obtain a modified inhibitor.

[0057] Example 7

[0058] Preparation of modified inhibitor:

[0059] Add 200 mL of N,N-dimethylformamide to the reactor, and continue to add 60 g of the modified lignin prepared in Example 3, 23 g of the terminal carboxyl organosilicon compound prepared in Example 4 and 1.0 g of p-toluenesulfonic acid. Heat the reactor to 90°C, reflux and stir to react for 4 hours. After the reaction is completed, cool to 50°C and evaporate under reduced pressure to obtain a modified inhibitor.

[0060] Example 8

[0061] Preparation of fire-fighting materials for three-dimensional space in coal mines:

[0062] S1. Add 70 g of the modified inhibitor prepared in Example 5, 1.2 g of the auxiliary agent and 100 mL of water into the reactor A, mix and stir for 20 min to obtain the main material, wherein the auxiliary agent is a mixture of a film-forming agent, n-butanol, a stabilizer, sodium benzoate and a surfactant, sodium dodecyl sulfate, in a mass ratio of 1:1:1;

[0063] S2, add 0.8g of composite foaming agent and 100mL of water to reactor B, stir at high speed for 10min, and the stirring rate is 2800r / min to obtain a foaming component, wherein the composite foaming agent is compounded by sodium α-olefin sulfonate and zwitterionic surfactant according to a volume ratio of 7:3, and the zwitterionic surfactant is cocamidopropyl betaine;

[0064] S3. Add the foaming component to the main material. The usage ratio of the foaming component to the main material is determined according to the actual situation of the usage scenario. Then mix and stir for 20 minutes to obtain the fire extinguishing material.

[0065] Example 9

[0066] Preparation of fire-fighting materials for three-dimensional space in coal mines:

[0067] S1. Add 70 g of the modified inhibitor prepared in Example 6, 1.4 g of the auxiliary agent and 100 mL of water into the reactor A, mix and stir for 20 min to obtain the main material, wherein the auxiliary agent is a mixture of a film-forming agent, n-butanol, a stabilizer, sodium benzoate and a surfactant, sodium dodecyl sulfate, in a mass ratio of 1:1:1;

[0068] S2, add 0.8-1.0g of composite foaming agent and 100mL of water to reactor B, stir at high speed for 10min, and the stirring rate is 3000r / min to obtain a foaming component, wherein the composite foaming agent is compounded by sodium α-olefin sulfonate and zwitterionic surfactant in a volume ratio of 7:3, and the zwitterionic surfactant is stearamidopropyl betaine;

[0069] S3. Add the foaming component to the main material. The usage ratio of the foaming component to the main material is determined according to the actual situation of the usage scenario. Then mix and stir for 20 minutes to obtain the fire extinguishing material.

[0070] Example 10

[0071] Preparation of fire-fighting materials for three-dimensional space in coal mines:

[0072] S1. Add 70 g of the modified inhibitor prepared in Example 7, 1.5 g of the auxiliary agent and 100 mL of water into the reactor A, mix and stir for 20 min to obtain the main material, wherein the auxiliary agent is a mixture of a film-forming agent, n-butanol, a stabilizer, sodium benzoate and a surfactant, sodium dodecyl sulfate, in a mass ratio of 1:1:1;

[0073] S2. Add 1.0 g of a composite foaming agent and 100 mL of water to the reactor B, stir at high speed for 10 min at a stirring rate of 3200 r / min to obtain a foaming component, wherein the composite foaming agent is prepared by compounding sodium α-olefin sulfonate and a zwitterionic surfactant in a volume ratio of 7:3, and the zwitterionic surfactant is lauramide propyl betaine;

[0074] S3. Add the foaming component to the main material. The usage ratio of the foaming component to the main material is determined according to the actual situation of the usage scenario. Then mix and stir for 20 minutes to obtain the fire extinguishing material.

[0075] Comparative Example 1

[0076] Comparative Example 1 is the control group of Example 8, in which the modified lignin prepared in Example 1 in the process of preparing the modified inhibitor in Example 5 in Example 8 is replaced with lignin, and the other raw materials and their preparation methods remain unchanged, and finally a fire extinguishing material is obtained.

[0077] Comparative Example 2

[0078] Comparative Example 2 is the control group of Example 8, in which the carboxyl-terminated organosilicon compound prepared in Example 4 in the process of preparing the modified inhibitor in Example 5 in Example 8 is deleted, and the remaining raw materials and their preparation methods remain unchanged, and finally a fire extinguishing material is obtained.

[0079] Comparative Example 3

[0080] Comparative Example 3 is the control group of Example 9, in which the modified inhibitor in step S1 of Example 9 is deleted, and the remaining raw materials and the preparation method thereof remain unchanged, and finally a fire extinguishing material is obtained.

[0081] Comparative Example 4

[0082] Comparative Example 4 is the control group of Example 10, in which the film-forming agent n-butanol in Example 10 is deleted, and the remaining raw materials and the preparation method thereof remain unchanged, and finally a fire extinguishing material is obtained.

[0083] The performance test of the fire extinguishing materials prepared in Examples 8 to 10 and Comparative Examples 1 to 4 was carried out. The test process is as follows. The test results are shown in Table 1:

[0084] Coal sample (lignite): Collect coal from underground mines, crush the coal, pass through a 300-mesh sieve, and divide the sieved coal powder into seven groups. Each group is then divided into two parts. Remember the A and B coal samples to complete the screening of the coal samples. The metal ion content of each sample is shown in the following table:

[0085]

[0086] Original coal sample and inhibited coal sample: Coal sample A in the seven groups of coal samples remains unchanged and is recorded as original coal sample; Coal sample B in the seven groups of coal samples is subjected to inhibitor treatment, and the inhibitor treatment process is as follows:

[0087] The main material and foaming component prepared in Example 9 were stirred and mixed at a mass ratio of 1:1.2 for 20 minutes to obtain an anti-fire extinguishing material; the anti-fire extinguishing material was evenly sprayed on the surface of the B coal sample in the seven groups of coal samples, the spraying pressure was 2.7 MPa, the single spraying thickness was 4 mm, the cycle spraying was repeated 3 times, and the spraying interval time was 2 hours. For the first spraying, it is necessary to ensure that the anti-fire extinguishing material covers the surface of the coal sample. After the spraying is completed, it is left to stand for 12 hours and recorded as the inhibited coal sample.

[0088] Heat treatment: 50g of each of seven raw coal samples and seven inhibitory coal samples were placed in a heat treatment tank. Compressed air (oxygen content was 21%) was introduced at a rate of 80mL / min. The twelve heat treatment tanks were heated at a rate of 0.8℃ / min at the same time until 150℃. Gas samples were collected in the heat treatment tanks to measure the volume fraction (%) of CO gas.

[0089] Retardation rate: refers to the ratio of the difference in CO gas volume fraction between the original coal sample and the inhibited coal sample to the CO gas volume fraction of the inhibited coal sample under the same conditions, calculated as follows:

[0090] E=(AB)*100% / A;

[0091] Where: E is the inhibition rate, %;

[0092] A is the volume fraction of CO gas in the raw coal sample, %;

[0093] B is the volume fraction of CO gas in the inhibited coal sample, %.

[0094] Table 1

[0095]

[0096] It can be seen from Table 1 that the fire-proofing material prepared by the present invention can significantly reduce the amount of CO gas released during the spontaneous combustion and oxidation of the coal body, and achieve the fire-proofing function by inhibiting the spontaneous combustion and oxidation of the coal body.

[0097] Embodiment 11

[0098] A method for applying a fire extinguishing material in a three-dimensional space underground in a coal mine comprises the following steps:

[0099] B1. The main material and the foaming component prepared in Example 8 were mixed in a mass ratio of 1:1.2, poured into a SJ400 mixer, and stirred for 20 minutes to obtain a fire extinguishing material;

[0100] B2. Inject the fire-proof material into the JP60-R sprayer and then carry out the spraying construction. During spraying, the outlet direction of the spray gun is 45° to the plane of the coal body, the spraying pressure is 2.5MPa, the single spraying thickness is 3mm, the cycle spraying is repeated 3 times, and the spraying interval time is 2h. For the first spraying, it is necessary to ensure that the fire-proof material covers the surface of the coal body. After the spraying is completed, the application of the fire-proof material is completed.

[0101] Example 12

[0102] A method for applying fire-fighting materials in a three-dimensional space underground in a coal mine comprises the following steps:

[0103] B1. The main material and the foaming component prepared in Example 9 were mixed in a mass ratio of 1:1.2, poured into a SJ400 mixer, and stirred for 20 minutes to obtain a fire extinguishing material;

[0104] B2. Inject the fire-proof material into the JP60-R sprayer and then carry out the spraying construction. During spraying, the outlet direction of the spray gun is 50° to the coal body plane, the spraying pressure is 2.7MPa, the single spraying thickness is 4mm, the cycle spraying is repeated 3 times, and the spraying interval time is 2h. For the first spraying, it is necessary to ensure that the fire-proof material covers and wraps the coal body surface. After the spraying is completed, the application of the fire-proof material is completed.

[0105] Embodiment 13

[0106] A method for applying fire-fighting materials in a three-dimensional space underground in a coal mine comprises the following steps:

[0107] B1. The main material and the foaming component prepared in Example 10 were mixed in a mass ratio of 1:1.2, poured into a SJ400 mixer, and stirred for 20 minutes to obtain a fire extinguishing material;

[0108] B2. Inject the fire-proof material into the JP60-R sprayer and then carry out the spraying construction. During spraying, the outlet direction of the spray gun is 55° to the plane of the coal body, the spraying pressure is 2.8MPa, the single spraying thickness is 5mm, the cycle spraying is repeated twice, and the spraying interval time is 2h. For the first spraying, it is necessary to ensure that the fire-proof material covers the surface of the coal body. After the spraying is completed, the application of the fire-proof material is completed.

[0109] It should be noted that, in this article, terms such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0110] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the invention, and the scope of the invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a three-dimensional space fire extinguishing material in a coal mine, characterized in that: The following steps are involved: S1, mixing and stirring the modified inhibitor, the auxiliary agent and water to obtain the main material; S2, stirring the composite foaming agent and water at high speed for 10 minutes to obtain a foaming component; S3, adding the foaming component to the main material, mixing and stirring for 20 minutes to obtain a fire extinguishing material; The dosage ratio of the modified inhibitor, the auxiliary agent and water is 70g:1.2-1.5g:100mL; the dosage ratio of the composite foaming agent and water is 0.8-1.0g:100mL; The modified inhibitor is prepared by the following steps: Add modified lignin, carboxyl-terminated organosilicon compound and p-toluenesulfonic acid to N,N-dimethylformamide, raise the temperature to 85-90°C, reflux and stir to react for 4 hours, and after the reaction is completed, cool to 45-50°C and perform vacuum rotary evaporation to obtain a modified inhibitor; The dosage ratio of the N,N-dimethylformamide, modified lignin, carboxyl-terminated organosilicon compound and p-toluenesulfonic acid is 200 mL: 55-60 g: 22-23 g: 0.8-1.0 g; The auxiliary agent is prepared by mixing n-butanol, sodium benzoate and sodium dodecyl sulfate in a mass ratio of 1:1:1; The modified lignin is prepared by the following steps: A1. Add half of the total amount of 37% formaldehyde aqueous solution and melamine to deionized water with stirring, heat to 85-90° C., stir and react for 2 hours to obtain a mixed solution; A2, add lignin to the mixed solution, stir for 30 minutes, then add the remaining 37% formaldehyde aqueous solution, stir for 30 minutes, then add 70wt% phytic acid aqueous solution, keep the temperature constant at 85-90°C, stir and react for 5 hours, after the reaction is completed, cool to room temperature, vacuum filter, collect the precipitate, wash the precipitate with deionized water until the pH value is 7.0, and dry the washed product at 80°C for 12 hours to obtain modified lignin; The usage ratio of the deionized water, 37% formaldehyde aqueous solution, melamine, lignin, and 70wt% phytic acid aqueous solution is 300mL: 20mL: 1.2-1.25moL: 9.2-9.5g: 15.5-16.0mL; The carboxyl-terminated organosilicon compound is prepared by the following steps: adding silane coupling agent KH-550 and succinic anhydride to N,N-dimethylformamide, stirring for 3 hours, filtering, washing the filter cake with anhydrous ethanol and distilled water three times respectively, and drying to constant weight to obtain a carboxyl-terminated organosilicon compound; the chemical structural formula of the carboxyl-terminated organosilicon compound is shown below: 。 2. The method for preparing a three-dimensional space fire extinguishing material in a coal mine according to claim 1, characterized in that: The composite foaming agent is prepared by compounding sodium α-olefin sulfonate and a zwitterionic surfactant in a volume ratio of 7:3; the zwitterionic surfactant is one of cocamidopropyl betaine, stearamidopropyl betaine and lauramidopropyl betaine.

3. The method for preparing a three-dimensional fire-proof material for underground coal mines according to claim 1, characterized in that: The dosage ratio of the N,N-dimethylformamide, the silane coupling agent KH-550 and the succinic anhydride is 250mL:0.1moL:0.1moL.

4. A method for applying fire-fighting materials in three-dimensional space underground in coal mines, characterized in that: The fire extinguishing material prepared by any one of claims 1 to 3, the application method comprises the following steps: B1, mixing the main material and the foaming component at a mass ratio of 1:1.2 for 20 minutes to obtain the fire extinguishing material; B2. Spraying of fire-proof and extinguishing materials is carried out, wherein the outlet direction of the spray gun is 45-55° to the plane of the coal body, the spraying pressure is 2.5-2.8MPa, the single spraying thickness is 3-5mm, the spraying cycle is 2-3 times, and the spraying interval time is 2h. After the spraying is completed, the application of the fire-proof and extinguishing materials is completed.