Calcium-based desulfurizer, composition and preparation method thereof

Through the synergistic effect of calcined calcium-based composite raw materials and catalytic oxidation components, organic polymers, and phosphorus-containing elemental salts, a highly active calcium-based desulfurizer is formed, which solves the problems of low reactivity and pore clogging of calcium-based absorbents and improves desulfurization efficiency. efficiency and SO2 diffusion channel, achieving efficient SO2 removal.

CN117101400BActive Publication Date: 2024-10-11BEIJING YUZHI ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202311088710.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-25
Publication Date
2024-10-11
Estimated Expiration
2043-08-25

AI Technical Summary

Technical Problem

The gas-solid reaction rate of existing calcium-based absorbents is slow, leading to clogging and densification of pores, hindering the diffusion of molecules such as SO2, and reducing desulfurization efficiency.

Method used

After mixing and calcining calcium-based composite raw materials and catalytic oxidation components, organic polymers and phosphorus-containing elemental salts are added as additives. Through high-temperature activation and collaborative catalysis, a highly active calcium-based desulfurizer is formed to improve the reaction path and pore structure.

Benefits of technology

It significantly increases the specific surface area and sulfur capacity of the calcium-based desulfurizer, enlarges the SO2 diffusion channel, improves desulfurization efficiency, saves energy consumption and reduces CO2 emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117101400B_ABST
    Figure CN117101400B_ABST
Patent Text Reader

Abstract

The present invention relates to the fields of air pollution prevention and control, solid waste pollution disposal, resource recycling, and in particular to a calcium-based desulfurizer, and a composition and preparation method thereof. The calcium-based desulfurizer composition comprises: a calcium-based composite raw material, an auxiliary agent 1, and an auxiliary agent 2, wherein: the calcium-based composite raw material is a product of mixed calcination of a calcium-based raw material and a catalytic oxidation component; the auxiliary agent 1 is an organic polymer; and the auxiliary agent 2 is a salt containing a phosphorus element. The highly active calcium-based desulfurizer of the present invention has a specific surface area greater than 40 m 2 / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the fields of air pollution prevention and control, solid waste pollution disposal, resource recycling, and in particular to a calcium-based desulfurizer, and a composition and a preparation method thereof. Background Art

[0002] Dry desulfurization technology has become the first choice for my country to further reduce SO2 emissions and reduce flue gas treatment costs due to its advantages such as low cost and simple process. Among them, the more commonly used absorbent is calcium-based absorbent. The desulfurization reaction process of calcium hydroxide is a chemical reaction between gas molecules such as SO2 and O2 and solid particles of Ca(OH)2. The gas-solid reaction rate is slow, and the generated solid products such as CaSO3 and CaSO4 cover the surface of the desulfurizer, further hindering the diffusion of SO2, O2 and other molecules into the desulfurizer, resulting in pore blockage and surface densification of the calcium-based absorbent, so that a large number of effective solid phase components in the desulfurization product cannot be used. Therefore, how to improve the reaction activity of the calcium-based absorbent itself, thereby improving the gas-solid reaction characteristics of the absorbent and SO2 is the focus of research at this stage. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] The present invention is expected to at least partially solve one of the above technical problems.

[0005] (II) Technical solution

[0006] In the first aspect of the present invention, a calcium-based desulfurizer composition is provided, comprising: a calcium-based composite raw material, an auxiliary agent 1, and an auxiliary agent 2, wherein: the calcium-based composite raw material is a product of mixed calcination of a calcium-based raw material and a catalytic oxidation component; the auxiliary agent 1 is an organic polymer; and the auxiliary agent 2 is a salt containing the element phosphorus.

[0007] In some embodiments of the present invention, the calcium-based raw material is slaked lime or a material having a calcium hydroxide content greater than 80%.

[0008] In some embodiments of the present invention, the catalytic oxidation component is one or more of the following materials: metal oxides, non-metal oxides, and rare earth element compounds.

[0009] In some embodiments of the present invention, the organic polymer is one or more of the following materials: polyethylene glycol dimethyl ether, NN dimethylacetamide; the salt containing phosphorus element is one or more of the following materials: Na3PO4, Na2HPO4, NaH2PO4, K3PO4, K2HPO4, KH2PO4 and phosphomolybdate, phosphotungstate.

[0010] In some embodiments of the present invention, the mass ratio of the calcium-based composite raw material, the auxiliary agent 1, and the auxiliary agent 2 is between 1:0.01-0.1:0.01-0.1.

[0011] In some embodiments of the present invention, the calcium-based raw material is carbide slag.

[0012] In some embodiments of the present invention, the catalytic oxidation component includes: a material containing cerium and lanthanum.

[0013] In some embodiments of the present invention, the catalytic oxidation component includes: Al2O3 and SiO2, and the molar ratio of the two is between 1:1 and 1:1.2.

[0014] In a first aspect of the present invention, a method for preparing a calcium-based desulfurizing agent is provided, comprising:

[0015] Step A, mixing and grinding a calcium-based raw material and a catalytic oxidation component;

[0016] Step B, calcining the ground product at a temperature of 600 to 1000° C. for 1 to 4 hours to obtain a calcium-based composite raw material;

[0017] Step C, preparing a digestive solution using additives 1 and 2; wherein additive 1 is an organic polymer; and additive 2 is a salt containing phosphorus;

[0018] Step D, fully reacting the calcium-based composite raw material with the digestive fluid;

[0019] Step E, drying the digested material to obtain a calcium-based desulfurizer.

[0020] In some embodiments of the present invention, in step A, the calcium-based raw material is slaked lime or a material having a calcium hydroxide content greater than 80%.

[0021] In some embodiments of the present invention, the catalytic oxidation component is one or more of the following materials: metal oxides, non-metal oxides, and rare earth element compounds.

[0022] In some embodiments of the present invention, the catalytic oxidation component includes: Al2O3 and SiO2, and the molar ratio of the two is between 1:1 and 1:1.2; in step B, the calcium-based raw material and the catalyst component react as follows: Ca(OH)2+Al2O3+SiO2+H2O→(CaO) x (Al2O3) y (SiO2) z (H2O) w .

[0023] In some embodiments of the present invention, the calcium-based raw material is carbide slag; the catalytic oxidation component also includes: Fe2O3; CeO2; wherein the mass ratio of carbide slag, Fe2O3, Al2O3, SiO2, and CeO2 is: 1:0.01:0.02:0.01:0.01.

[0024] In some embodiments of the present invention, in step C, the mass ratio of the calcium-based composite raw material, the auxiliary agent 1, and the auxiliary agent 2 is between 1:0.01-0.1:0.01-0.1.

[0025] In some embodiments of the present invention, in step C, the organic polymer is one or more of the following materials: polyethylene glycol dimethyl ether, NN dimethylacetamide.

[0026] In some embodiments of the present invention, in step C, the salt containing phosphorus is one or more of the following materials: Na3PO4, Na2HPO4, NaH2PO4, K3PO4, K2HPO4, KH2PO4, phosphomolybdate, and phosphotungstate.

[0027] In some embodiments of the present invention, in step D, the mass ratio of the calcium-based composite raw material to the digestive fluid is 1:0.6 to 1:1.5, and the reaction time is controlled between 10 and 60 minutes.

[0028] In some embodiments of the present invention, in step E, the digested material is dried at a temperature of 100-400°C.

[0029] In the first aspect of the present invention, a calcium-based desulfurizer is provided. The calcium-based desulfurizer uses the above-mentioned road pavement gel material composition as a raw material; or the calcium-based desulfurizer is prepared by the above-mentioned preparation method.

[0030] (III) Beneficial effects

[0031] It can be seen from the above technical solution that the present invention has at least one of the following beneficial effects compared with the prior art:

[0032] (1) Increased specific surface area of ​​calcium-based desulfurizer

[0033] In the traditional calcium hydroxide production process, the specific surface area of ​​quicklime used as raw material is generally 2 to 4 m 2 / g, the specific surface area of ​​calcium hydroxide prepared by ordinary process digestion is 10~20m 2 / g. Moreover, the desulfurization effect of the catalytic oxidation component after mixing with ordinary calcium hydroxide at room temperature did not show significant improvement.

[0034] The specific surface area of ​​the calcium-based composite raw material prepared by the raw material calcination method of the present invention is 10-20 m 2 / g, and the high-activity calcium-based desulfurizer prepared by the digestion liquid of the present invention has a specific surface area greater than 40m 2 / g. The reason is that the decomposition of calcium hydroxide is a dehydration process. The loss of -OH in the decomposition process will affect the form of calcium oxide crystals, change its microstructure, thereby increasing its specific surface area, which is conducive to the full progress of the subsequent digestion reaction. On the other hand, the calcination temperature of calcium hydroxide is relatively low, lower than the calcination temperature of limestone>1000℃, which can save energy consumption, and there will be no CO2 gas emissions during the calcination process, which is more economical and environmentally friendly.

[0035] (2) The reaction products of calcium-based raw materials and catalytic oxidation components improve the desulfurization reaction path

[0036] The catalytic oxidation component is mixed with calcium hydroxide and calcined to obtain a calcium-based composite raw material, which can fully stimulate its catalytic activity. The metal oxides activated by high temperature are dispersed on the particle surface of the calcium-based composite raw material. The crystal structure they form has the ability to adsorb and release oxygen. In the process of the desulfurizer and SO2 adsorption reaction, the adsorption reaction center is transferred from the Ca(OH)2 molecule to the surface of the metal oxide molecule, producing intermediate products, specifically:

[0037] Ca(OH)2+SiO2+H2O→(CaO) x (SiO2) y (H2O) z

[0038] Ca(OH)2+Al2O3+H2O→(CaO) x (Al2O3) y (H2O) z

[0039] Ca(OH)2+Al2O3+SiO2+H2O→(CaO) x (Al2O3) y (SiO2) z (H2O) w

[0040] They can effectively improve the path of the desulfurization reaction, avoid the direct reaction of SO2 and Ca(OH)2, form a dense product layer on the surface of the desulfurizer particles, hinder the diffusion of SO2 into the interior of the desulfurizer, and further cause the desulfurization reaction.

[0041] (3) Adding rare earth materials to increase the sulfur capacity of the desulfurizer

[0042] The rare earth elements added to the catalytic oxidation component have rich energy levels and a special 4f outer electron layer structure, which give it excellent chemical activity and characteristics. After being calcined together with metal oxides, the synergistic catalytic effect of the two can effectively improve the oxidation activity and desulfurization efficiency of the calcium-based desulfurizer. Compared with the calcium-based desulfurizer prepared from ordinary quicklime raw materials, the sulfur capacity can be increased by more than 50%.

[0043] (4) The addition of additives 1 and 2 further increases the specific surface area of ​​the calcium-based desulfurizer

[0044] The addition of additives 1 and 2 effectively avoided the problem of too small pore size distribution of the desulfurizer caused by the intense heat release during the digestion process. The addition of additives 1 and 2 increased the proportion of mesopores and macropores in the pore size distribution of the desulfurizer. The desulfurizer has more mesopores and macropores, which is beneficial to the diffusion of SO2 on the solid phase surface, promoting the improvement of the desulfurization effect, and enabling the effective components in the desulfurizer to continuously react with SO2 to improve the utilization rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 The present invention is a flow chart of a method for preparing a calcium-based desulfurizer according to an embodiment of the present invention.

[0046] Figure 2 Schematic diagram of the pore volume distribution of the calcium-based desulfurizer according to various embodiments of the present invention. DETAILED DESCRIPTION

[0047] The invention provides a calcium-based desulfurizer suitable for medium- and low-temperature dry desulfurization, and its purpose is to improve the specific surface area and sulfur capacity of the material through process and material optimization.

[0048] According to the first aspect of the present invention, the present invention first provides a calcium-based desulfurization agent composition, comprising: a calcium-based composite raw material, an auxiliary agent 1, and an auxiliary agent 2, wherein: the calcium-based composite raw material is a product of a mixture of a calcium-based raw material and a catalytic oxidation component and calcined; the auxiliary agent 1 is an organic polymer; and the auxiliary agent 2 is a salt containing a phosphorus element. The calcium-based composite raw material, the auxiliary agent 1, and the auxiliary agent 2 are mixed in a mass ratio of 1:0.01-0.1:0.01-0.1.

[0049] According to the second aspect of the present invention, a method for preparing a calcium-based desulfurizer based on the above desulfurizer composition is also provided. Figure 1 The flowchart of the preparation method of the calcium-based desulfurizer of the present invention is shown in FIG. Figure 1 As shown, the preparation method of the calcium-based desulfurizer of the present invention comprises:

[0050] Step A, mixing and grinding a calcium-based raw material and a catalytic oxidation component;

[0051] In this embodiment, the calcium-based raw material slaked lime comes from carbide slag. In addition, the calcium-based raw material can also be other materials with a slaked lime or calcium hydroxide content greater than 80%.

[0052] Among them, the catalytic oxidation component contains one or more of metal oxides (such as Fe2O3, Al2O3, MnO2, etc.), non-metallic oxides (such as SiO2) and rare earth element (mainly cerium and lanthanum) compounds; auxiliary agent 1 is an organic polymer, mainly ionic liquid polymer (such as polyethylene glycol dimethyl ether, NN dimethylacetamide, etc.); auxiliary agent 2 is mainly a salt containing phosphorus, such as Na3PO4, Na2HPO4, NaH2PO4, K3PO4, K2HPO4, KH2PO4 and phosphomolybdate, phosphotungstate, etc., one or more of which are selected.

[0053] Preferably, the catalytic oxidation component includes: Al2O3 and SiO2, and the molar ratio between the two is between 1:1 and 1:1.2.

[0054] More preferably, the catalytic oxidation components also include: Fe2O3 and CeO2, and the mass ratio of carbide slag, Fe2O3, Al2O3, SiO2, and CeO2 is: 1:0.01:0.02:0.01:0.01.

[0055] Specifically, the raw material with slaked lime or calcium hydroxide content greater than 80% (such as carbide slag) and the catalytic oxidation component are uniformly mixed in a ratio of 1:0.01-0.1 and ground to a particle size of ≤45 μm.

[0056] Step B, calcining the calcium-based composite raw material at a temperature of 700 to 1000° C. for 1 to 4 hours to obtain the calcium-based composite raw material;

[0057] The calcium-based composite raw material is a product of calcining a mixture of slaked lime and a catalytic oxidation component, and its main component is calcium oxide. Specifically, at a calcination temperature of 600 to 1000°C, the catalytic oxidation component and the calcium-based raw material undergo the following reaction:

[0058] Ca(OH)2+Al2O3+SiO2+H2O→(CaO) x (Al2O3) y (SiO2) z (H2O) w

[0059] Step C, preparing a digestive juice using auxiliary agent 1 and auxiliary agent 2, wherein the auxiliary agent 1 is an organic polymer; and the auxiliary agent 2 is a salt containing phosphorus;

[0060] Specifically, one or more of the additives 1 and 2 are preferably dissolved in water at a ratio of 1:0.01-0.1:0.01-0.1 to prepare the digestive solution.

[0061] Step D, fully reacting the calcium-based composite raw material with the digestive fluid;

[0062] Specifically, the calcium-based composite raw material and the prepared digestion water are added into a mixer for sufficient reaction, the mass ratio of the calcium-based composite raw material to the digestion liquid is 1:0.6-1.5, and the reaction time is controlled between 10 and 60 minutes.

[0063] Step E, drying the digested material to obtain a calcium-based desulfurizer.

[0064] Specifically, the digested material is dried at a temperature of 100 to 400° C. to obtain a highly active calcium-based desulfurizer.

[0065] According to the third aspect of the present invention, a calcium-based desulfurizer is also provided, which uses the above road pavement gel material composition as a raw material; or is prepared using the above preparation method.

[0066] Compared with the calcium-based desulfurizer of the prior art, the present invention has the following differences and beneficial effects:

[0067] (1) Increased specific surface area of ​​calcium-based desulfurizer

[0068] In the traditional calcium hydroxide production process, the specific surface area of ​​quicklime used as raw material is generally 2 to 4 m 2 / g, the specific surface area of ​​calcium hydroxide prepared by ordinary process digestion is 10~20m 2 / g. The specific surface area of ​​the calcium-based composite raw material prepared by the raw material calcination method described in this article is 10-20m 2 / g, and the high-activity calcium-based desulfurizer prepared by the digestion liquid of the present invention has a specific surface area greater than 40m 2 / g. The reason is that the decomposition of calcium hydroxide is a dehydration process. The loss of -OH in the decomposition process will affect the form of calcium oxide crystals, change its microstructure, thereby increasing its specific surface area, which is conducive to the full progress of the subsequent digestion reaction. On the other hand, the calcination temperature of calcium hydroxide is relatively low, lower than the calcination temperature of limestone>1000℃, which can save energy consumption, and there will be no CO2 gas emissions during the calcination process, which is more economical and environmentally friendly.

[0069] In the present invention, the purpose of high temperature calcination is to make calcium hydroxide react with the catalytic oxidation component at high temperature to generate a main component (CaO) x (Al2O3) y (SiO2) z (H2O) wThe calcium-based composite raw material is used for subsequent digestion. Different from the traditional high-temperature calcination of calcium carbonate to produce lime, the temperature at which the composite raw material of the present invention is calcined to produce the calcium-based composite raw material is lower, and the activity of the catalytic oxidation component can also be stimulated at this temperature.

[0070] The metal oxides activated by high temperature are dispersed on the particle surface of the calcium-based composite raw material. The crystal structure they form has the ability to adsorb and release oxygen. During the adsorption reaction of the desulfurizer and SO2, the adsorption reaction center is transferred from the Ca(OH)2 molecule to the surface of the metal oxide molecule, producing some intermediate products.

[0071] (2) The reaction products of calcium-based raw materials and catalytic oxidation components improve the desulfurization reaction path

[0072] The above-mentioned catalytic oxidation component does not significantly improve the desulfurization effect after being mixed with ordinary calcium hydroxide at room temperature. However, the catalytic oxidation component is mixed with calcium hydroxide and calcined to obtain a calcium-based composite raw material, which can fully stimulate its catalytic activity. The metal oxides activated by high temperature are dispersed on the particle surface of the calcium-based composite raw material. The crystal structure they form has the ability to adsorb and release oxygen. In the process of the adsorption reaction between the desulfurizer and SO2, the adsorption reaction center is transferred from the Ca(OH)2 molecule to the surface of the metal oxide molecule, producing some intermediate products, such as:

[0073] Ca(OH)2+SiO2+H2O→(CaO) x (SiO2) y (H2O) z

[0074] Ca(OH)2+Al2O3+H2O→(CaO) x (Al2O3) y (H2O) z

[0075] Ca(OH)2+Al2O3+SiO2+H2O→(CaO) x (Al2O3) y (SiO2)z(H2O) w

[0076] They can effectively improve the path of the desulfurization reaction, avoid the direct reaction of SO2 and Ca(OH)2, form a dense product layer on the surface of the desulfurizer particles, hinder the diffusion of SO2 into the interior of the desulfurizer, and further cause the desulfurization reaction.

[0077] (3) Adding rare earth materials to increase the sulfur capacity of the desulfurizer

[0078] The rare earth elements added to the catalytic oxidation components have rich energy levels and special 4f outer electron layer structure, which give them excellent chemical activity and characteristics. Their good oxygen storage capacity can play a good catalytic role, and their large ion radius can improve the dispersibility of catalytic oxidation components such as Fe2O3, Al2O3, and SiO2. After co-calcination with metal oxides, the synergistic catalytic effect of the two can effectively improve the oxidation activity and desulfurization efficiency of the calcium-based desulfurizer. Compared with the calcium-based desulfurizer prepared from ordinary quicklime raw materials, the sulfur capacity can be increased by more than 50%.

[0079] (4) The addition of additives 1 and 2 further increases the specific surface area of ​​the calcium-based desulfurizer

[0080] The addition of additives 1 and 2 effectively avoided the problem of too small pore size distribution of the desulfurizer caused by the intense heat release during the digestion process. The addition of additives 1 and 2 increased the proportion of mesopores and macropores in the pore size distribution of the desulfurizer. The desulfurizer has more mesopores and macropores, which is beneficial to the diffusion of SO2 on the solid phase surface, promoting the improvement of the desulfurization effect, and enabling the effective components in the desulfurizer to continuously react with SO2 to improve the utilization rate.

[0081] Various aspects of the calcium-based desulfurizer of the present invention are introduced below in conjunction with specific examples.

[0082] Example 1

[0083] Weigh 500g of quicklime raw material, recorded as calcium-based raw material 1, grind the calcium-based raw material 1 to a particle size of ≤45μm, mix it evenly with pure water at a mass ratio of 1:0.9, and stir for 40min to obtain slaked lime, recorded as comparative example 1; weigh 500g of comparative example 1 and put it into a muffle furnace, calcine it at 650°C for 3h, recorded as calcium-based raw material 2, digest it with the same mass ratio and stirring method as above to obtain slaked lime, recorded as calcium-based desulfurizer 1, and test their specific surface areas respectively, and obtain the following results:

[0084] Table 1 Data comparison of calcium hydroxide prepared from different calcium-based raw materials

[0085]

[0086] Example 2

[0087] The slaked lime and Fe2O3 were mixed evenly in a ratio of 1:0.01, ground to a particle size of ≤45 μm, put into a muffle furnace, and calcined at 650°C for 3 h to obtain a calcium-based composite raw material. 300 g of the calcium-based composite raw material was weighed and digested with pure water in a mass ratio of 1:0.9, and stirred for 40 min to obtain a calcium-based desulfurizer 2.

[0088] Example 3

[0089] Mix slaked lime, Fe2O3 and Al2O3 in a mass ratio of 1:0.01:0.02, and repeat the steps of Example 2 to obtain a calcium-based desulfurizer 3.

[0090] Example 4

[0091] Mix slaked lime with Fe2O3, Al2O3 and SiO2 in a mass ratio of 1:0.01:0.02:0.01, and repeat the steps of Example 2 to obtain a calcium-based desulfurizer 4.

[0092] Example 5

[0093] Mix slaked lime with Fe2O3, Al2O3, SiO2 and CeO2 in a mass ratio of 1:0.01:0.02:0.01:0.01, and repeat the steps of Example 2 to obtain a calcium-based desulfurizer 5.

[0094] Example 6

[0095] Mix slaked lime with Fe2O3, Al2O3, SiO2, and CeO2 in a mass ratio of 1:0.01:0.02:0.01:0.01, grind to a particle size of ≤45μm, put into a muffle furnace, and calcine at 650°C for 3h to obtain a calcium-based composite raw material. Dissolve NN dimethyldiethanolamine in pure water in a ratio of 1:0.01 to prepare a digestion solution. Mix the calcium-based composite raw material and the digestion solution in a ratio of 1:0.9, and stir for 40min to obtain a calcium-based desulfurizer 6.

[0096] Example 7

[0097] Repeat the steps of Example 6, dissolve NN dimethyldiethanolamine and phosphomolybdate in pure water at a ratio of 1:0.01:0.01 to prepare a digestion solution, mix the calcium-based composite raw material and the digestion solution at a ratio of 1:0.9, stir for 40 minutes, and obtain a calcium-based desulfurizer 7.

[0098] Example 8

[0099] Mix carbide slag with Fe2O3, Al2O3, SiO2 and CeO2 in a mass ratio of 1:0.01:0.02:0.01:0.01, and repeat the steps of Example 7 to obtain a calcium-based desulfurizer 8.

[0100] The calcium-based desulfurizer prepared in the above examples was subjected to desulfurization evaluation under coking flue gas. The results are shown in Table 2. The pore volume distribution of some calcium-based desulfurizers is shown in Table 2. Figure 2 .

[0101] Coking flue gas test conditions: temperature: 220℃, SO2: 1600mg / Nm 3 , NO x :800mg / Nm3 , CO2: 8%, O2: 6%, H2O: 15%.

[0102] Table 2 Comparison of high activity calcium hydroxide data

[0103]

[0104] Under the synergistic effect of the catalytic oxidation components and various additives, the specific surface area of ​​the calcium-based desulfurizer can reach 45cm 3 / g or more, pore volume>0.2m 2 / g, the sulfur capacity is increased to 24%, which is better than most calcium-based desulfurizers on the market in dry desulfurization. After replacing slaked lime with carbide slag, the performance of calcium-based desulfurizer is further improved.

[0105] At this point, the various embodiments of the present invention have been introduced. According to the above description, those skilled in the art should have a clear understanding of the present invention.

[0106] It should be noted that, unless explicitly indicated to the contrary, the numerical parameters in the specification and claims of the present invention may be approximate values ​​and may be changed according to the content of the present invention. Specifically, all the numbers indicating the content of the composition, reaction conditions, etc. recorded in the specification and claims should be understood to be modified by the term "about" in all cases, and the meaning of the expression is to include a change of ±10% from a specific number in some embodiments.

[0107] Those skilled in the art should understand that in the claims and description of the present invention, the word "comprising" does not exclude the existence of elements (or steps) not listed in the claims. The word "a" or "an" preceding an element (or step) does not exclude the existence of multiple such elements (or steps).

[0108] For certain implementations, if they are not the key content of the present invention and are well known to ordinary technicians in the relevant technical field, they are not described in detail in the drawings or text of the specification due to space limitations. At this time, they can be understood by referring to the relevant prior art. In addition, the purpose of providing the above embodiments is only to make the present invention meet legal requirements, and the present invention can be implemented in many different forms and should not be interpreted as limited to the embodiments described herein. In addition, the above definitions of each element and method are not limited to the various specific structures, shapes or methods mentioned in the embodiments, and ordinary technicians in this field can simply change or replace them.

[0109] Similarly, it should be understood that in order to simplify the present invention, in the above description of the exemplary embodiments of the present invention, the various features of the present invention are sometimes grouped together into a single embodiment, figure, or description thereof. However, the method of the invention should not be interpreted as reflecting the following intention: the claimed invention requires more features than the features explicitly stated in each claim. More specifically, as reflected in the claims, each inventive aspect is less than all the features of the previous single embodiment. Moreover, the embodiments can be mixed and matched with each other or with other embodiments based on design and reliability considerations, that is, the technical features in different embodiments can be freely combined to form more embodiments. Therefore, the claims following the specific embodiment are hereby explicitly incorporated into the specific embodiment, wherein each claim itself serves as a separate embodiment of the present invention.

[0110] The above specific embodiments provide a detailed description of the objectives, technical means and beneficial effects of the present invention. It should be understood that the purpose of the detailed description is to enable those skilled in the art to understand the present invention more clearly, and it is not used to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a calcium-based desulfurizer, characterized in that: include: Step A, mixing and grinding a calcium-based raw material and a catalytic oxidation component, wherein the calcium-based raw material is a material having a content of more than 80% of slaked lime or calcium hydroxide; the catalytic oxidation component comprises: Al2O3 and SiO2, and the molar ratio of the two is between 1:1 and 1:1.2; Step B, calcining the ground product at a temperature of 600-1000° C. for 1-4 hours to obtain a calcium-based composite raw material, wherein the calcium-based raw material reacts with the catalytic oxidation component as follows: Ca(OH)2+Al2O3+SiO2+H2O→(CaO) x (Al2O3) y (SiO2) z (H2O) w ; Step C, preparing a digestive juice using auxiliary agent 1 and auxiliary agent 2; wherein the auxiliary agent 1 is an organic polymer; and the auxiliary agent 2 is a salt containing phosphorus; Step D, fully reacting the calcium-based composite raw material with the digestive fluid; Step E, drying the digested material to obtain a calcium-based desulfurizer.

2. The preparation method according to claim 1, characterized in that: The calcium-based raw material is carbide slag; The catalytic oxidation component also includes: Fe2O3; CeO2; Among them, the mass ratio of carbide slag, Fe2O3, Al2O3, SiO2 and CeO2 is: 1:0.01:0.02:0.01:0.

01.

3. The preparation method according to claim 1, characterized in that: In the step C, The mass ratio of the calcium-based composite raw material, the auxiliary agent 1 and the auxiliary agent 2 is between 1:0.01-0.1:0.01-0.1; and / or The organic polymer is one or more of the following materials: polyethylene glycol dimethyl ether, NN dimethylacetamide; and / or The salt containing phosphorus element is one or more of the following materials: Na3PO4, Na2HPO4, NaH2PO4, K3PO4, K2HPO4, KH2PO4, phosphomolybdate and phosphotungstate.

4. The preparation method according to claim 1, characterized in that: In the step D, the mass ratio of the calcium-based composite raw material to the digestive fluid is 1:0.6 to 1:1.5, and the reaction time is controlled between 10 and 60 minutes; and / or In the step E, the digested material is dried at a temperature of 100 to 400°C.

5. A calcium-based desulfurizer, characterized in that: The calcium-based desulfurizer is prepared by the preparation method described in any one of claims 1 to 4.

Citation Information

Cited By

  • Manganese-lanthanum double-element gradient doped calcium-based desulfurizing agent and preparation method thereof

    CN121892079A

  • Desulfurizing agent for efficient flue gas desulfurization and preparation method thereof

    CN122352023A

  • A desulfurizer for high-efficiency flue gas desulfurization and a preparation method thereof

    CN122352023B