Lignin-based Co-N3 monatomic catalyst prepared by three-stage pyrolysis method and application of lignin-based Co-N3 monatomic catalyst

The lignin-based Co-N3 single-atom catalyst prepared by a three-stage pyrolysis method solves the problem of unutilized lignin resources and achieves high conversion rate of HMF and high selectivity of FDCA, demonstrating the catalyst's performance under mild conditions. Highly efficient catalytic performance.

CN118767963APending Publication Date: 2024-10-15TIANJIN UNIV OF SCI & TECH

Patent Information

Application Number
CN202410755012.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Lignin resources have not been fully utilized, leading to resource waste and environmental pollution, and it is difficult to achieve efficient conversion of aromatic organic compounds such as 5-hydroxymethylfurfural (HMF) and 2,5-furandicarboxylic acid (FDCA) with existing technology. Conversion rate and selectivity.

Method used

A three-stage pyrolysis method was used to prepare the lignin-based Co-N3 single atom catalyst by enzymatically hydrolyzing lignin, ultrasonic mixing with sodium hydroxide, cobalt chloride hexahydrate, and anhydrous zinc chloride, followed by freeze-drying with melamine, and Multi-stage pyrolysis treatment is carried out in a nitrogen atmosphere, and finally soaked in hydrochloric acid to prepare a carbon-supported Co-N3 single-atom catalyst, which can be used to efficiently dehydrogenate and oxygenate HMF to prepare FDCA under mild conditions.

Benefits of technology

The 100% conversion rate of HMF and the high selectivity of FDCA were achieved, proving the alkali-resistant structure and efficient catalytic performance of the Co-N3 catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004889188380000051
    Figure BDA0004889188380000051
  • Figure HDA0004889188390000011
    Figure HDA0004889188390000011
  • Figure HDA0004889188390000021
    Figure HDA0004889188390000021
Patent Text Reader

Abstract

The invention relates to the technical field of lignin carbon-based monatomic catalyst preparation, mainly relates to a lignin-based Co-N3 monatomic catalyst prepared by a three-stage pyrolysis method and application thereof, and aims to solve the problem that a coordination structure of metal active sites of a monatomic catalyst is difficult to control. The monatomic catalyst loaded with unique Co-N3 configuration is successfully prepared. The method mainly comprises the following steps: preparing a nitrogen-doped metal-lignin precursor from lignin, cobalt salt and melamine as raw materials, subsequently pyrolyzing the precursor in a tubular furnace in three steps, regulating nitrogen release, and finally obtaining the monatomic catalyst with a definite Co-N3 configuration. The lignin-based Co-N3 monatomic catalyst prepared by the invention has excellent catalytic oxidation performance, and the conversion rate of 5-hydroxymethylfurfural can be 100% and the yield of 2, 5-furandicarboxylic acid can be 99.85% under the mild condition of 50 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of preparation of lignin carbon-based single-atom catalysts, and mainly to a three-stage pyrolysis method for preparing lignin-based Co-N3 single-atom catalysts and applications thereof. Background Art

[0002] Single atom catalysts (SACs) are one of the fastest growing research areas in catalysis. SACs have controllable coordination environments and atomic structures, providing an effective way to regulate the activity and selectivity of catalytic reactions. Various noble metal / non-noble metal catalysts were developed in the early days and fixed on metal oxide supports. In recent years, biomass-derived carbon materials have gradually attracted a lot of attention due to their higher specific surface area compared to metal oxides and the fact that the functional groups contained in them can interact with the target metal to form metal-biomass composites.

[0003] Lignin is the most abundant aromatic organic macromolecule in nature and the second most abundant biomass resource among lignocellulose components. Lignin contains abundant -OH groups, which can effectively interact with metal ions to form stable insoluble metal-lignin complexes. In addition, due to the coordination effect of lignin macromolecules, the target metal in the metal-lignin complex is quite stable at the corresponding anchoring sites, which is conducive to the formation of highly dispersed metal-based single-atom catalysts.

[0004] However, the commercial value of lignin has not been fully utilized at present. Most of it is used as low-value fuel or directly discharged, which not only wastes resources but also may pollute the environment. Summary of the invention

[0005] The purpose of the present invention is to provide a three-stage pyrolysis method for preparing a lignin-based Co-N3 single-atom catalyst and its application. The catalyst has a simple preparation process and low cost, and has a unique alkali-resistant structure of Co-N3, which can achieve a high conversion rate of 5-hydroxymethylfurfural (HMF) and a high selectivity of 2,5-furandicarboxylic acid (FDCA).

[0006] To achieve the above object, the technical solution of the present invention is as follows:

[0007] In the first aspect, a three-stage pyrolysis method is used to prepare a lignin-based Co-N3 single-atom catalyst, which is prepared by the following method, specifically comprising the following steps:

[0008] Step 1, dissolving 0.3-1.5 g of enzymatically hydrolyzed lignin and 0.05-1.25 g of sodium hydroxide in 80 mL of deionized water, and ultrasonicating for 30-60 min to obtain a uniformly dispersed lignin solution;

[0009] Step 2: Dissolve 0.05-3.5 mmol of cobalt chloride hexahydrate and 1.0-3.5 mmol of anhydrous zinc chloride in 100-600 mL of deionized water, and obtain a uniformly dispersed Co 2+ / Zn 2+ Metal mixture;

[0010] Step 3: Use a peristaltic pump to pump Co 2+ / Zn 2+ The metal mixed solution is dropped into the lignin solution, the mixed solution is stirred at 300-700 rpm for 1-5 hours, then aged for 6-15 hours, and the supernatant is removed to obtain a lignin-metal complex;

[0011] Step 4, mixing the lignin-metal complex with 3 to 15 g of melamine, wherein the amount of melamine is 10 to 20 times the amount of the enzymatically hydrolyzed lignin, and mixing them evenly by ultrasonic-assisted stirring, placing them in an ultra-low temperature refrigerator for solidification, and then freeze-drying them to obtain a nitrogen-doped metal lignin precursor after drying;

[0012] Step 5: The precursor obtained in step 4 is pyrolyzed in a nitrogen atmosphere by first opening the main valve of the tubular furnace and introducing the precursor for 3 to 10 minutes. N2 is used to remove residual air in the quartz tube, and the tail pipe is passed into a beaker filled with water to observe the airflow rate. When the bubble emergence rate is stable, the temperature control program is set as follows: from room temperature to 400-600°C at a heating rate of 3-8°C / min, keep warm for 0.5-1.5h, to complete the first stage of pyrolysis; then, the temperature is increased to 750-950°C at a heating rate of 2-6°C / min, keep warm for 0.5-1.5h, to complete the second stage of pyrolysis; subsequently, the temperature is increased to 1000-1200°C at 5-10°C / min, keep warm for 1-5min, to complete the third stage of pyrolysis; finally, the temperature is lowered to room temperature, and the obtained pyrolysis product is soaked in 1-4M hydrochloric acid at 70-120°C for 5-12h, and the lignin-based carbon-loaded Co-N3 single atom catalyst is obtained after drying.

[0013] Secondly, a three-stage pyrolysis method is used to prepare lignin-based Co-N3 single-atom catalysts, and the lignin-based carbon-loaded Co-N3 single-atom catalysts are used to efficiently dehydrogenate and oxygenate HMF to prepare FDCA under mild conditions.

[0014] Furthermore, the lignin is one of alkali lignin, kraft lignin, purified enzymatic lignin, and organic solvent lignin.

[0015] Furthermore, the alkaline solution in step 1 is one of a potassium hydroxide solution and a sodium hydroxide solution.

[0016] Furthermore, the metal mixture in step 2 is Co 2+ / Zn2+ Metal mixture and Co 2+ / Cd 2+ A type of metal mixture.

[0017] Furthermore, the nitrogen source in step 4 is one of melamine, dicyandiamide and urea.

[0018] Furthermore, 0.2-1.0 mmol HMF, 0.5-1.5 mol / L sodium carbonate, 20-100 mg lignin-based Co-N3 catalyst and 20 mL water were mixed and added to a 50 mL high temperature and high pressure reactor; the reaction was carried out under the conditions of 1-5 bar O2 and 40-80°C for 2-6 hours. After the reaction, high performance liquid chromatography was used to analyze the contents of HMF and FDCA in the sample.

[0019] Beneficial effects:

[0020] Based on the structural characteristics of lignin, the present invention adopts a three-stage pyrolysis method to prepare a single-atom catalyst with a Co-N3 configuration. With the help of the unique alkali-resistant structure of Co-N3, a high conversion rate of HMF and a high selectivity of FDCA are achieved under mild conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 a, b, c, and d are TEM and HAADF-STEM images of the catalyst in Example 1 and the comparative example catalyst, respectively.

[0022] Figure 2 a, b, c, and d are schematic diagrams of XANES and EXAFS spectral analysis of the catalyst in Example 1 and the comparative example catalyst. DETAILED DESCRIPTION

[0023] Example 1

[0024] A three-stage pyrolysis method is used to prepare a lignin-based Co-N3 single-atom catalyst, which is prepared by the following method, specifically comprising the following steps:

[0025] Step 1: 0.6 g of enzymatically hydrolyzed lignin and 0.98 g of sodium hydroxide were dissolved in 80 mL of deionized water, and ultrasonicated for 50 min to obtain a uniformly dispersed lignin solution.

[0026] Step 2: Dissolve 0.25 mmol of cobalt chloride hexahydrate and 1.25 mmol of anhydrous zinc chloride in 300 mL of deionized water and obtain a uniformly dispersed Co 2+ / Zn 2+ Metal mixture.

[0027] Step 3: Use a peristaltic pump to pump Co 2+ / Zn2+ The metal mixture was dropped into the lignin solution, and the mixture was stirred at 550 rpm for 1.5 h, then allowed to stand for aging for 7 h, and the supernatant was removed to obtain the lignin-metal complex.

[0028] Step 4: Mix the lignin-metal complex and 9 g of melamine evenly by ultrasonic-assisted stirring, place in an ultra-low temperature refrigerator for solidification, and then freeze-dry to obtain a nitrogen-doped metal lignin precursor.

[0029] Step 5, the precursor obtained in step 4 is pyrolyzed in a nitrogen atmosphere. First, the main valve of the tubular furnace is opened to pass 4min N2 to remove the residual air in the quartz tube, and the tail pipe is passed into a beaker filled with water to observe the airflow rate. When the bubble emergence rate is stable, the temperature control program is set. The temperature control program is as follows: from room temperature to 550℃ at a heating rate of 5℃ / min, keep warm for 1h, and complete the first stage of pyrolysis. Then, the temperature is increased to 900℃ at a heating rate of 5℃ / min, and kept warm for 1h to complete the second stage of pyrolysis. Subsequently, the temperature is increased to 1050℃ at 10℃ / min, and kept warm for 1min to complete the third stage of pyrolysis. Finally, it is cooled to room temperature, and the obtained pyrolysis product is soaked in 3M hydrochloric acid at 85℃ for 10h, and the lignin-based carbon-supported Co-N3 single-atom catalyst is obtained after drying.

[0030] Step 6, the lignin-based carbon-supported Co-N3 single-atom catalyst prepared above is applied to the efficient dehydrogenation and oxygenation of HMF to prepare FDCA under mild conditions. 0.35mmol HMF, 1.0mol / L sodium carbonate, 40mg lignin-based Co-N3 catalyst and 20mL water are mixed and added to a 50ml high-temperature and high-pressure reactor. The reaction is carried out under 2bar O2 and 50℃ for 5h, and the HMF conversion rate is measured to be 100%, and the yield of FDCA is 99.85%.

[0031] The present invention is further described with reference to the accompanying drawings, Example 1 and Comparative Example:

[0032] Figure 1 (a), (b), (c), and (d) are TEM and HAADF-STEM images of the catalyst of Example 1 and the catalyst of the comparative example, respectively. Figure 1 As can be seen in (b), the metallic cobalt atoms in the lignin-based carbon-supported Co-N3 single-atom catalyst are uniformly dispersed on the surface of the carrier, and no cobalt clusters appear.

[0033] Figure 2(a)(b)(c)(d) and Table 1 are XANES and EXAFS spectra of the catalyst of Example 1 and the comparative catalyst. Both catalysts have only one main peak, which can be attributed to the first coordination shell of Co-N. The metal Co-Co peak is negligible, and there are no other high shell peaks. These results strongly support the successful synthesis of lignin-based Co-N3 and Co-N4 single-atom catalysts.

[0034] Table 1

[0035]

[0036] Example 2

[0037] A three-stage pyrolysis method is used to prepare a lignin-based Co-N3 single-atom catalyst, which is prepared by the following method, specifically comprising the following steps:

[0038] Step 1: 0.7 g of enzymatically hydrolyzed lignin and 1.10 g of sodium hydroxide were dissolved in 80 mL of deionized water, and ultrasonicated for 30 min to obtain a uniformly dispersed lignin solution.

[0039] Step 2: Dissolve 0.15 mmol of cobalt chloride hexahydrate and 1.35 mmol of anhydrous zinc chloride in 350 mL of deionized water and obtain a uniformly dispersed Co 2+ / Zn 2+ Metal mixture.

[0040] Step 3: Use a peristaltic pump to pump Co 2+ / Zn 2+ The metal mixture is dropped into the lignin solution, the mixture is stirred at 450 rpm for 2 hours, and then aged for 7 hours. The supernatant is removed to obtain the lignin-metal complex.

[0041] Step 4, after the lignin-metal complex and 15 g of melamine are mixed evenly by ultrasonic-assisted stirring, the mixture is placed in an ultra-low temperature refrigerator for solidification and then freeze-dried to obtain a nitrogen-doped metal lignin precursor after drying.

[0042] Step 5, the precursor obtained in step 4 is pyrolyzed in a nitrogen atmosphere. First, the main valve of the tubular furnace is opened to pass N2 for 3 minutes to remove the residual air in the quartz tube, and the tail pipe is passed into a beaker filled with water to observe the airflow rate. When the bubble emergence rate is stable, the temperature control program is set. The temperature control program is as follows: from room temperature to 550°C at a heating rate of 5°C / min, keep warm for 1h, and complete the first stage of pyrolysis. Then, the temperature is increased to 900°C at a heating rate of 5°C / min, and kept warm for 1h to complete the second stage of pyrolysis. Subsequently, the temperature is increased to 1050°C at 10°C / min, and kept warm for 1min to complete the third stage of pyrolysis. Finally, it is cooled to room temperature, and the obtained pyrolysis product is soaked in 3M hydrochloric acid at 85°C for 10h, and the lignin-based carbon-supported Co-N3 single-atom catalyst is obtained after drying.

[0043] Step 6, the lignin-based carbon-supported Co-N3 single-atom catalyst prepared above is applied to the efficient dehydrogenation and oxygenation of HMF to prepare FDCA under mild conditions. 0.2mmol HMF, 0.8mol / L sodium carbonate, 50mg lignin-based Co-N3 catalyst and 20mL water are mixed and added to a 50ml high-temperature and high-pressure reactor. The reaction is carried out under 3bar O2 and 65℃ for 5h, and the HMF conversion rate is measured to be 100%, and the yield of FDCA is 98.97%.

[0044] Example 3

[0045] A three-stage pyrolysis method is used to prepare a lignin-based Co-N3 single-atom catalyst, which is prepared by the following method, specifically comprising the following steps:

[0046] Step 1: 0.5 g of enzymatically hydrolyzed lignin and 1.15 g of sodium hydroxide were dissolved in 80 mL of deionized water, and ultrasonicated for 30 min to obtain a uniformly dispersed lignin solution.

[0047] Step 2: Dissolve 0.35 mmol of cobalt chloride hexahydrate and 1.15 mmol of anhydrous zinc chloride in 500 mL of deionized water and obtain a uniformly dispersed Co 2+ / Zn 2+ Metal mixture.

[0048] Step 3: Use a peristaltic pump to pump Co 2+ / Zn 2+ The metal mixture is dropped into the lignin solution, the mixture is stirred at 600 rpm for 2 hours, and then aged for 8 hours. The supernatant is removed to obtain the lignin-metal complex.

[0049] Step 4: After the lignin-metal complex and 6 g of melamine are mixed evenly by ultrasonic-assisted stirring, the mixture is placed in an ultra-low temperature refrigerator for solidification and then freeze-dried to obtain a nitrogen-doped metal lignin precursor.

[0050] Step 5, the precursor obtained in step 4 is pyrolyzed in a nitrogen atmosphere. First, the main valve of the tubular furnace is opened to pass N2 for 3 minutes to remove the residual air in the quartz tube, and the tail pipe is passed into a beaker filled with water to observe the airflow rate. When the bubble emergence rate is stable, the temperature control program is set. The temperature control program is as follows: from room temperature to 550°C at a heating rate of 5°C / min, keep warm for 1h, and complete the first stage of pyrolysis. Then, the temperature is increased to 900°C at a heating rate of 5°C / min, and kept warm for 1h to complete the second stage of pyrolysis. Subsequently, the temperature is increased to 1050°C at 10°C / min, and kept warm for 1min to complete the third stage of pyrolysis. Finally, it is cooled to room temperature, and the obtained pyrolysis product is soaked in 3M hydrochloric acid at 85°C for 10h, and the lignin-based carbon-supported Co-N3 single-atom catalyst is obtained after drying.

[0051] Step 6, the lignin-based carbon-supported Co-N3 single-atom catalyst prepared above is applied to the efficient dehydrogenation and oxygenation of HMF to prepare FDCA under mild conditions. 0.85mmol HMF, 1.5mol / L sodium carbonate, 60mg lignin-based Co-N3 catalyst and 20mL water are mixed and added to a 50ml high-temperature and high-pressure reactor. The reaction is carried out under 4bar O2 and 70℃ for 5h, and the HMF conversion rate is measured to be 100%, and the yield of FDCA is 99.31%.

[0052] Comparative Example

[0053] This comparative example provides a two-stage pyrolysis method for preparing a lignin-based Co-N4 single-atom catalyst, which is prepared by the following method, specifically comprising the following steps:

[0054] Step 1: 0.6 g of enzymatically hydrolyzed lignin and 1.0 g of sodium hydroxide were dissolved in 80 mL of deionized water, and ultrasonicated for 30 min to obtain a uniformly dispersed lignin solution.

[0055] Step 2: Dissolve 0.15 mmol of cobalt chloride hexahydrate and 1.35 mmol of anhydrous zinc chloride in 250 mL of deionized water and obtain a uniformly dispersed Co 2+ / Zn 2+ Metal mixture.

[0056] Step 3: Use a peristaltic pump to pump Co 2+ / Zn 2+ The metal mixture is dropped into the lignin solution, and the mixture is stirred at 600 rpm for 2.5 hours, then aged for 8 hours, and the supernatant is removed to obtain the lignin-metal complex.

[0057] Step 4: Mix the lignin-metal complex and 9 g of melamine evenly by ultrasonic-assisted stirring, place in an ultra-low temperature refrigerator for solidification, and then freeze-dry to obtain a nitrogen-doped metal lignin precursor.

[0058] Step 5, the precursor obtained in step 4 is pyrolyzed in a nitrogen atmosphere. First, the main valve of the tubular furnace is opened to pass N2 for 5 minutes to remove the residual air in the quartz tube, and the tail pipe is passed into a beaker filled with water to observe the airflow rate. When the bubble emergence rate is stable, the temperature control program is set. The temperature control program is as follows: from room temperature to 550°C at a heating rate of 5°C / min, keep warm for 1h, and complete the first stage of pyrolysis. Subsequently, the temperature is raised to 900°C at a heating rate of 5°C / min, and kept warm for 1h to complete the second stage of pyrolysis. Finally, it is cooled to room temperature, and the obtained pyrolysis product is soaked in 3M hydrochloric acid at 85°C for 10h, and the lignin-based carbon-supported Co-N4 single-atom catalyst is obtained after drying.

[0059] Step 6, applying the lignin-based carbon-supported Co-N4 single-atom catalyst to the HMF dehydrogenation and oxygenation reaction: Consistent with the catalytic scheme in Example 1, the measured HMF conversion rate reached 84.71% and the FDCA yield reached 44.69%.

Claims

1. A three-stage pyrolysis method for preparing lignin-based Co-N3 single-atom catalyst, characterized in that: The method is prepared by the following steps: Step 1, dissolving 0.3-1.5 g of enzymatically hydrolyzed lignin and 0.05-1.25 g of sodium hydroxide in 80 mL of deionized water, and ultrasonicating for 30-60 min to obtain a uniformly dispersed lignin solution; Step 2: Dissolve 0.05-3.5 mmol of cobalt chloride hexahydrate and 1.0-3.5 mmol of anhydrous zinc chloride in 100-600 mL of deionized water, and obtain a uniformly dispersed Co 2+ / Zn 2+ Metal mixture; Step 3: Use a peristaltic pump to pump Co 2+ / Zn 2+ The metal mixed solution is dropped into the lignin solution, the mixed solution is stirred at 300-700 rpm for 1-5 hours, then aged for 6-15 hours, and the supernatant is removed to obtain a lignin-metal complex; Step 4, mixing the lignin-metal complex with 3 to 15 g of melamine, wherein the amount of melamine is 10 to 20 times the amount of the enzymatically hydrolyzed lignin, and mixing them evenly by ultrasonic-assisted stirring, placing them in an ultra-low temperature refrigerator for solidification, and then freeze-drying them to obtain a nitrogen-doped metal lignin precursor after drying; Step 5: The precursor obtained in step 4 is pyrolyzed in a nitrogen atmosphere by first opening the main valve of the tubular furnace and introducing the precursor for 3 to 10 minutes. N2 is used to remove residual air in the quartz tube, and the tail pipe is passed into a beaker filled with water to observe the airflow rate. When the bubble emergence rate is stable, the temperature control program is set as follows: from room temperature to 400-600°C at a heating rate of 3-8°C / min, keep warm for 0.5-1.5h, to complete the first stage of pyrolysis; then, the temperature is increased to 750-950°C at a heating rate of 2-6°C / min, keep warm for 0.5-1.5h, to complete the second stage of pyrolysis; subsequently, the temperature is increased to 1000-1200°C at 5-10°C / min, keep warm for 1-5min, to complete the third stage of pyrolysis; finally, the temperature is lowered to room temperature, and the obtained pyrolysis product is soaked in 1-4M hydrochloric acid at 70-120°C for 5-12h, and the lignin-based carbon-loaded Co-N3 single atom catalyst is obtained after drying.

2. The three-stage pyrolysis method for preparing lignin-based Co-N3 single-atom catalyst according to claim 1, characterized in that: The lignin is one of alkali lignin, kraft lignin, purified enzymatic lignin, and organic solvent lignin.

3. The three-stage pyrolysis method for preparing lignin-based Co-N3 single-atom catalyst according to claim 1, characterized in that: The alkaline solution in step 1 is one of potassium hydroxide solution and sodium hydroxide solution.

4. The three-stage pyrolysis method for preparing lignin-based Co-N3 single-atom catalyst according to claim 1, characterized in that: The metal mixture in step 2 is Co 2+ / Zn 2+ Metal mixture and Co 2+ / Cd 2+ A type of metal mixture.

5. The three-stage pyrolysis method for preparing lignin-based Co-N3 single-atom catalyst according to claim 1, characterized in that: The nitrogen source in step 4 is one of melamine, dicyandiamide and urea.

6. The three-stage pyrolysis method for preparing lignin-based Co-N3 single-atom catalyst according to claim 1, characterized in that: 0.2-1.0 mmol 5-hydroxymethylfurfural, 0.5-1.5 mol / L sodium carbonate, 20-100 mg lignin-based Co-N3 catalyst and 20 mL water were mixed and added to a 50 mL high temperature and high pressure reactor; the mixture was reacted for 2-6 hours at 1-5 bar O2 and 40-80°C. After the reaction, high performance liquid chromatography was used to analyze the contents of 5-hydroxymethylfurfural and 2,5-furandicarboxylic acid in the sample.

7. An application of the three-stage pyrolysis method for preparing lignin-based Co-N3 single-atom catalyst according to any one of claims 1 to 6, characterized in that: The lignin-based carbon-supported Co-N3 single-atom catalyst was applied to efficiently dehydrogenate and oxygenate 5-hydroxymethylfurfural to produce 2,5-furandicarboxylic acid under mild conditions.

Citation Information

Patent Citations

  • High loading capacity metal single atom proton exchange membrane fuel cell catalytic materials, and preparation method thereof

    CN109390597A

  • Preparation method of rare-earth-metal-doped carbon-based oxygen reduction electrocatalyst

    CN112563517A

  • Method for preparing monatomic catalyst by using lignin-metal complex aerogel as precursor

    CN113750998A

  • Carbon material loaded with tin single atoms and clusters as well as preparation method and application of carbon material

    CN117023564A

  • Se-M diatomic catalyst as well as preparation method and application thereof

    CN117913294A

Cited By

  • Nitrogen-doped carbon-loaded molybdenum-based monatomic catalyst as well as preparation method and application thereof

    CN121551044A

  • Method for preparing water-soluble lignin chelated calcium fertilizer based on iron-manganese double-site catalyst

    CN122141716A

  • Method for preparing water-soluble lignin chelated calcium fertilizer based on iron-manganese double site catalyst

    CN122141716B