A method for quantitative parameter testing of hydrogen-induced crack sensitivity
By plotting the relationship curve between the crack resistance J value of steel plates and the crack length Δa and calculating the crack propagation energy, the problem that the influence of hydrogen environment cannot be considered in the existing technology is solved, and an accurate quantitative assessment of the risk of hydrogen-induced cracking in high-strength steel is achieved.
Patent Information
- Application Number
- CN202310914583.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-24
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-07-24
AI Technical Summary
Existing technologies cannot take into account the influence of the hydrogen environment during crack propagation, making it impossible to accurately assess the risk of hydrogen-induced cracking in high-strength steel.
By plotting the relationship between the crack resistance J value and crack length Δa of steel plates in air and accelerated simulated hydrogen environments, the energy required for crack propagation is calculated using integrals, and the hydrogen-induced cracking sensitivity quantification parameter HE is calculated by combining the first and second formulas, thus quantitatively assessing the risk of hydrogen-induced cracking.
It enables more accurate quantitative assessment of the risk of hydrogen-induced cracking under various operating conditions, overcoming the limitation of existing technologies that can only observe potential and strain rate after specimen necking.
Smart Images

Figure BDA0004357934130000021 
Figure FDA0004357934100000011 
Figure HDA0004357934170000011
Abstract
Description
Technical Field
[0001] The invention relates to the research field of hydrogen-induced crack performance of high-strength steel, and in particular to a method for evaluating hydrogen-induced crack sensitivity. Background Art
[0002] It is well known that hydrogen-induced cracking will only occur in high-strength steel when plastic deformation and hydrogen evolution occur simultaneously on the surface. At room temperature, the adsorption of atomic hydrogen on the metal surface may be caused by the electrochemical reduction of water during the corrosion process of steel or the application of a cathode potential below the thermodynamic threshold of hydrogen evolution. In fact, the sensitivity of hydrogen-induced cracking increases with the increase of the tensile properties of steel. In previous work, in slow strain rate tests, the effects of applied potential and strain rate on hydrogen-induced cracking of steel can only be observed after the specimen is necked. This method cannot accurately evaluate the sensitivity of hydrogen-induced cracking under various use environments, let alone quantitatively evaluate the sensitivity of hydrogen-induced cracking. The main reason is that in the ductile fracture of metals, plastic deformation dominates at the crack tip and the material's fracture resistance increases with the growth of the crack. At present, the conservation of fracture toughness in fracture mechanics must meet simple loading (proportional growth of each component of stress), and does not allow unloading or critical crack expansion, because critical expansion will lead to local stress relaxation. Therefore, the fracture toughness in fracture mechanics is currently only a criterion for crack initiation and cannot be used for the crack propagation process. It also does not take into account the influence of the hydrogen environment, so it is impossible to accurately evaluate the risk of hydrogen-induced cracks. Summary of the invention
[0003] In view of this, the present invention provides a method for quantitative parameter testing of hydrogen-induced crack sensitivity, which solves the problem that the influence of applied potential and strain rate on hydrogen-induced cracking of steel can only be observed after the specimen is necked, resulting in no consideration of the crack propagation process and the influence of the hydrogen environment, and therefore the risk of hydrogen-induced cracking cannot be accurately evaluated.
[0004] To achieve the above-mentioned purpose, the method for testing the quantitative parameters of hydrogen-induced crack sensitivity of the present invention comprises:
[0005] Draw a curve diagram of the relationship between the crack resistance J value and the crack length Δa of the steel plate under test in air and accelerated simulated hydrogen environment; in the relationship curve diagram, draw a passivation line using the first formula, the first formula is J=2e r Δa, where: e r is the sum of the ultimate strength and yield strength of the material; and parallel lines of the passivation line are drawn when Δa is 0.2 and 0.5 respectively;
[0006] The area enclosed by the relationship curve and the two parallel lines in air and accelerated simulated hydrogen environment is calculated by integration, and the energy S required for crack propagation in air is expressed by the area airand the energy S required for crack propagation in a simulated hydrogen accelerated environment environment ;
[0007] The quantitative parameter HE of hydrogen induced crack sensitivity is calculated by the second formula, and the second formula is:
[0008] In the present disclosure and possible embodiments, a curve of the relationship between the crack resistance J value and the crack length Δa is obtained by the potential drop method.
[0009] In the present disclosure and possible embodiments, the potential drop method includes:
[0010] The single-side notched bending specimens were pre-cracked using an electromagnetic testing machine until the initial crack length was equal to 50% of the specimen width.
[0011] In the present disclosure and possible embodiments, the crack length Δa is obtained by substituting the potential drop value into the Johnson formula. Based on the crack length Δa, the J integral is calculated using the standard formula to draw a relationship curve between the crack resistance J value of the steel plate in air and accelerated simulated hydrogen environment and the crack length Δa.
[0012] In the present disclosure and possible embodiments, the accelerated simulated hydrogen environment is prepared by constant potential polarization using an accelerated simulated hydrogen environment solution.
[0013] In the present disclosure and possible embodiments, the accelerated simulated hydrogen environment solution is an HCL solution.
[0014] The present invention has the following beneficial effects:
[0015] The method for testing the quantitative parameters of hydrogen-induced crack sensitivity of the present invention first calculates the relationship curve between the crack resistance J value and the crack length Δa in air and accelerated simulated hydrogen environment by integration. It can be seen that the relationship curve can take into account the influence of the hydrogen environment on the crack propagation process. Then, the energy S required for crack propagation in air is obtained by integrating the relationship curve and the first company. air and the energy S required for crack propagation in a simulated hydrogen accelerated environment environment , continue to use the second formula to obtain the quantitative parameter of hydrogen-induced crack sensitivity, and this quantitative parameter is proposed for the first time in the present invention, and further use this quantitative parameter to more accurately quantify and evaluate the risk of hydrogen-induced cracking under various use environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The above and other objects, features and advantages of the present disclosure will become more apparent through the following description of the embodiments of the present disclosure with reference to the accompanying drawings, in which:
[0017] Figure 1 is the size of the single-side notched bending specimen in the embodiment of the present invention;
[0018] Figure 2 is a curve diagram showing the relationship between the crack resistance J value and the crack length Δa in air and accelerated simulated hydrogen environment of an embodiment of the present invention;
[0019] Figure 3 is a passivation line diagram of an embodiment of the present invention;
[0020] Figure 4 is the energy S required for crack propagation in air and accelerated simulated hydrogen environment of the embodiment of the present invention;
[0021] Figure 5 It is the quantitative parameter HE of hydrogen induced crack sensitivity of 460LA of the embodiment of the present invention in 0.1 mol / L HCL solution, using constant potential polarization, and the voltages are -1V and -2V respectively. DETAILED DESCRIPTION
[0022] The present disclosure is described below based on embodiments, but it is worth noting that the present disclosure is not limited to these embodiments. In the detailed description of the present disclosure below, some specific details are described in detail. However, for the parts that are not described in detail, those skilled in the art can also fully understand the present disclosure.
[0023] In addition, those skilled in the art should understand that the drawings are only provided to illustrate the purpose, features and advantages of the present disclosure, and the drawings are not actually drawn to scale.
[0024] At the same time, unless the context clearly requires otherwise, the words "include", "comprises" and similar words throughout the specification and claims should be interpreted as inclusive rather than exclusive or exhaustive; that is, the meaning is "including but not limited to".
[0025] Example
[0026] 1. The relationship curve between the crack resistance J and the crack length Δa of 460LA was determined by using the potential drop method using a single-sided notched bending specimen.
[0027] All test samples were tested in air and 0.1 mol / L HCL solution, respectively. In this embodiment, 0.1 mol / L HCL solution was used to simulate the hydrogen acceleration environment by constant potential polarization, and the voltages were -1 V and -2 V, respectively. Of course, other solutions commonly used in the art can also be used to simulate the hydrogen acceleration environment, and the present disclosure is not limited to this.
[0028] Before using the fatigue testing machine for bending test, use an electromagnetic testing machine to test the single-side notched bending specimen (such as Figure 1) for pre-crack treatment until the initial crack length is equal to 50% of the specimen width. The bending test is carried out by displacement control at a speed of 0.001m / s. During the bending test, displacement, load, time and potential drop are collected. The crack length is obtained by using the potential drop value to enter the Qiaosen formula. According to the crack length, the J integral is calculated using the formula in the ASTM E813-89 standard. The specification determination of the above-mentioned single-sided notched bending specimen and the displacement control of the bending test are all in accordance with the ASTM E813-89 standard.
[0029] Using the bending test result data, the relationship curves of the crack resistance J value and the crack length Δa of 460LA in air, in a 0.1 mol / L HCL solution at a constant potential of -1 V and in a 0.1 mol / L HCL solution at a constant potential of -2 V were plotted, as shown in FIG. Figure 2 .
[0030] 2. Use the first formula: J = 2e r Δa, where er is the sum of the ultimate strength and yield strength of the material, equal to 1115.5MPa, and a passivation line is drawn in the relationship curve between the crack resistance J value and the crack length Δa.
[0031] Continue to draw two lines parallel to the passivation line when Δa = 0.2 and Δa = 0.5, such as Figure 3 .
[0032] The energy S required for crack extension in air, in a 0.1 mol / L HCL solution at a constant potential of -1 V, and in a 0.1 mol / L HCL solution at a constant potential of -2 V was obtained respectively. That is, the area enclosed by the relationship curve between the crack resistance J value and the crack length Δa under different environments and the two lines Δa = 0.2 and Δa = 0.5 was calculated by integration, as shown in Figure 4 .
[0033] 3. Through the second formula: Where S environment Substitute the energy required for crack extension in a 0.1 mol / L HCL solution at a constant potential of -1 V and in a 0.1 mol / L HCL solution at a constant potential of -2 V, S air Substituting the energy required for crack propagation in air, the quantitative parameter HE of hydrogen-induced crack sensitivity at a constant potential of -1V in 0.1mol / L HCL solution and a constant potential of -2V in 0.1mol / L HCL solution is calculated, as Figure 5 .
[0034] The larger the quantitative parameter HE of hydrogen-induced crack sensitivity is, the greater the risk of hydrogen-induced cracking of the material under the use environment.
[0035] The evaluation method of the present invention overcomes the current problem that the effects of applied potential and strain rate on hydrogen-induced cracking of steel can only be observed after the specimen is necked, and proposes an experimental procedure for determining quantitative parameters of hydrogen-induced crack sensitivity, thereby being able to more accurately quantify and evaluate the risks of hydrogen-induced cracking under various use environments.
[0036] The above-described embodiments are only embodiments of the present disclosure, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the present disclosure. It should be noted that, for a person of ordinary skill in the art, without departing from the concept of the present disclosure, several variations, equivalent substitutions, improvements, etc. may be made, all of which fall within the scope of protection of the present disclosure. Therefore, the scope of protection of the present disclosure shall be subject to the attached claims.
Claims
1. A method for testing the quantitative parameters of hydrogen-induced crack sensitivity. It is characterized in that include: Draw a curve of the relationship between the crack resistance J value and the crack length Δa of the steel plate under test in air and accelerated simulated hydrogen environment; In the relationship curve diagram, the passivation line is drawn using the first formula, where the first formula is J=2e r Δa, where: e r is the sum of the ultimate strength and yield strength of the material; and parallel lines of the passivation line are drawn when Δa is 0.2 and 0.5 respectively; The area enclosed by the relationship curve and the two parallel lines in air and accelerated simulated hydrogen environment is calculated by integration, and the energy S required for crack propagation in air is expressed by the area air and the energy S required for crack propagation in a simulated hydrogen accelerated environment environment ; The quantitative parameter HE of hydrogen induced crack sensitivity is calculated by the second formula, and the second formula is:
2. The method for quantitative parameter testing of hydrogen induced crack sensitivity according to claim 1, Features: The relationship curve between the crack resistance J value and the crack length Δa was obtained by the potential drop method.
3. The method for quantitative parameter testing of hydrogen induced crack sensitivity according to claim 2, It is characterized in that The potential drop method comprises: The single-side notched bending specimens were pre-cracked using an electromagnetic testing machine until the initial crack length was equal to 50% of the specimen width.
4. The method for quantitative parameter testing of hydrogen induced crack sensitivity according to claim 2 or 3, Features: The crack length Δa is obtained by substituting the potential drop value into the Johnson formula. According to the crack length Δa, the J integral is calculated using the standard formula to draw a curve of the relationship between the crack resistance J value of the steel plate in air and accelerated simulated hydrogen environment and the crack length Δa.
5. The method for quantitative parameter testing of hydrogen induced crack sensitivity according to claim 4, Features: The accelerated simulated hydrogen environment is prepared by constant potential polarization using an accelerated simulated hydrogen environment solution.
6. The method for quantitative parameter testing of hydrogen induced crack sensitivity according to claim 5, Features: The accelerated simulated hydrogen environment solution is an HCL solution.
Citation Information
Patent Citations
Hydrogen embrittlement evaluation method
CN107764663A