A method for preparing a crystal rod and the crystal rod itself.

By introducing hydrogen-containing gas during the crystal rod preparation process, the problem of excessive oxygen content in monocrystalline silicon was solved, defects were reduced, resistivity and minority carrier lifetime were improved, and the efficiency and product quality of solar cells were enhanced.

CN117127249BActive Publication Date: 2026-11-10TIANJIN ZHONGHUAN SEMICON CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311132296.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-04
Publication Date
2026-11-10
Estimated Expiration
2043-09-04

AI Technical Summary

Technical Problem

Excessive oxygen content or short tail life in monocrystalline silicon products can affect product quality.

Method used

During the crystal rod preparation process, especially in the shoulder turning and equal diameter steps, hydrogen-containing gas is introduced, and the mass of hydrogen accounts for no more than 30% of the total gas mass.

Benefits of technology

Reducing the oxygen content of monocrystalline silicon decreases the formation of boron-oxygen complexes, increases the resistivity and minority carrier lifetime of the crystal, and improves the photoelectric conversion efficiency and product quality of solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117127249B_ABST
    Figure CN117127249B_ABST
Patent Text Reader

Abstract

This application discloses a method for preparing a crystal rod and the crystal rod itself, belonging to the field of single crystal growth technology. The method for preparing the crystal rod includes a shoulder-turning step and a diameter-equalizing step. During the shoulder-turning step and / or the diameter-equalizing step, a hydrogen-containing gas is introduced; the hydrogen-containing gas includes hydrogen gas, and the mass of the hydrogen gas is m. H The total mass of hydrogen-containing gas is m 总 , satisfying: m H / m 总 ≤30%. This application reduces the oxygen content of single crystals by introducing hydrogen gas during the crystal rod preparation process, thereby reducing defects inside the single crystal silicon. When pulling boron-doped single crystals, it can reduce the formation of boron-oxygen complexes and prevent the phenomenon of efficiency degradation in solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of single crystal growth technology, specifically relating to a method for preparing a crystal rod and the crystal rod itself. Background Technology

[0002] The characteristics of Czochralski single-crystal silicon products include oxygen content, minority carrier lifetime, carbon content, resistivity, defects, dislocations, etc. Excessive oxygen content at the head of a single-crystal silicon product or excessively low lifetime at the tail of the single crystal will affect product quality. Summary of the Invention

[0003] The purpose of this application is to provide a method for preparing crystal rods and crystal rods, which can solve the above-mentioned technical problems.

[0004] This application provides a method for preparing a crystal rod, including a shoulder-turning step and a diameter-equalizing step. During the shoulder-turning step and / or the diameter-equalizing step, a hydrogen-containing gas is introduced; the hydrogen-containing gas includes hydrogen gas, and the mass of the hydrogen gas is m. H The total mass of the hydrogen-containing gas is m 总 , satisfying: m H / m 总 ≤30%.

[0005] In some embodiments, the method for preparing the crystal rod further includes melting, welding, crystal pulling, and shoulder expansion steps, wherein the hydrogen-containing gas is introduced in any one or more of the melting, welding, crystal pulling, and shoulder expansion steps.

[0006] In some embodiments, the shoulder expansion step includes a shoulder growth to a target shoulder stage, and the shoulder expansion step includes a shoulder growth to a target shoulder length stage, wherein the shoulder length in the shoulder expansion step is L1, and the target shoulder length is L; in the stage of 0 < L1 ≤ 0.3L, the first crucible is controlled to rotate V1; in the stage of 0.3L < L1 ≤ L, the second crucible is controlled to rotate V2; satisfying: V1 > V2.

[0007] In some embodiments, the range of the first crucible rotation V1 is 9 r / min to 15 r / min.

[0008] In some embodiments, the range of the second crucible rotation V2 is 7 r / min to 12 r / min.

[0009] In some embodiments, during the shoulder expansion step, the shoulder length during the expansion process is L1, and the target shoulder length is L; wherein, in the stage of 0 < L1 ≤ 0.3L, the time for introducing the hydrogen-containing gas is T1; in the stage of 0.3L < L1 ≤ 0.6L, the time for introducing the hydrogen-containing gas is T2; in the stage of 0.6L < L1 ≤ L, the time for introducing the hydrogen-containing gas is T3; the total time for introducing the hydrogen-containing gas in the shoulder expansion step is T. 扩肩 T 扩肩=T1+T2+T3; satisfying: T2<T1.

[0010] In some embodiments, T2 < T3 is satisfied.

[0011] In some embodiments, T3 < T1 is satisfied.

[0012] In some embodiments, during the equal diameter step, in the stage of 0 < H1 ≤ 0.11H, the third crucible is controlled to rotate to V3; in the stage of 0.11H < H1 ≤ H, the fourth crucible is controlled to rotate to V4, satisfying: V3 > V4, H1 is the crystal pulling length, and H is the total length of the target crystal rod.

[0013] In some embodiments, the equal diameter step includes a first equal diameter stage, wherein the first equal diameter stage is: 0 < H1 ≤ 0.11H, and the hydrogen-containing gas is introduced during the first equal diameter stage, wherein H1 is the crystal pulling length and H is the total length of the target crystal rod.

[0014] In some embodiments, the equal diameter step includes a second equal diameter stage, a third equal diameter stage, and a fourth equal diameter stage; the second equal diameter stage is the 0.11H < H1 ≤ 0.33H stage; the third equal diameter stage is the 0.33H < H1 ≤ 0.77H stage; and the fourth equal diameter stage is the 0.77H < H1 ≤ H stage; the hydrogen-containing gas is introduced in any one or more of the second, third, and fourth equal diameter stages.

[0015] In some embodiments, the hydrogen-containing gas is introduced during the first equal diameter stage at time T4, during the second equal diameter stage at time T5, during the third equal diameter stage at time T6, and during the fourth equal diameter stage at time T7.

[0016] Among them, T4 < T5 = T7 < T6.

[0017] In some embodiments, the hydrogen content of the hydrogen-containing gas in the first isodiameter stage is higher than the hydrogen content of the hydrogen-containing gas in each of the second, third, and fourth isodiameter stages.

[0018] In some embodiments, the melting step includes feeding, refeeding and volatilization steps, wherein the feeding temperature is 300℃~1600℃.

[0019] In some embodiments, the re-addition temperature is 1400℃~1600℃;

[0020] In some embodiments, the evaporation temperature is 1460°C to 1480°C.

[0021] In some embodiments, the feeding time is 4h to 12h.

[0022] In some embodiments, the re-application time is 3h to 10h.

[0023] In some embodiments, the evaporation time is 0.3h to 3h.

[0024] In some embodiments, the melting step introduces a hydrogen-containing gas, wherein the hydrogen content in the hydrogen-containing gas is less than or equal to [amount missing].

[0025] In some embodiments, hydrogen-containing gas is introduced into the feeding stage, with a hydrogen content of less than or equal to 30%.

[0026] In some embodiments, the hydrogen-containing gas is introduced into the re-addition stage, with a hydrogen content of less than or equal to 20%, and the hydrogen-containing gas is introduced into the volatilization stage, with a hydrogen content of less than or equal to 20%.

[0027] In some embodiments, the welding step includes a high-temperature preheating stage and a low-temperature welding stage.

[0028] In some embodiments, the temperature of the high-temperature preheating stage is 1457°C to 1475°C.

[0029] In some embodiments, the temperature of the low-temperature welding stage is 1449°C to 1457°C.

[0030] In some embodiments, the crucible rotation speed during the welding step is in the range of 6 r / min to 15 r / min.

[0031] In some embodiments, the duration of the high-temperature preheating stage is 0.1h to 1h.

[0032] In some embodiments, the duration of the low-temperature welding stage is 0.1h to 4h.

[0033] In some embodiments, the welding step involves introducing a hydrogen-containing gas, wherein the hydrogen content in the hydrogen-containing gas is less than or equal to 15%.

[0034] In some embodiments, the boron and / or gallium content in the raw materials used to prepare the crystal rod is 0.007 mg / g to 0.8 mg / g.

[0035] In some embodiments, the phosphorus content in the raw materials used to prepare the crystal rod is 0.001 mg / g to 0.01 mg / g.

[0036] Accordingly, this application provides a crystal rod, which is prepared by the method described above.

[0037] The beneficial effects of this application are as follows: Compared with the prior art, this application provides a method for preparing a crystal rod, including a shoulder-turning step and a diameter equalization step, wherein a hydrogen-containing gas is introduced during the shoulder-turning step and / or the diameter equalization step; the hydrogen-containing gas includes hydrogen gas, and the mass of the hydrogen gas is m. H The total mass of hydrogen-containing gas is m 总 , satisfying: m H / m 总 ≤30%. This application reduces the oxygen content of single crystals by introducing hydrogen gas during the crystal rod preparation process, thereby reducing defects inside the single crystal silicon. When pulling boron-doped single crystals, it can reduce the formation of boron-oxygen complexes and prevent the phenomenon of efficiency degradation in solar cells. Attached Figure Description

[0038] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0039] Figure 1 This is a schematic diagram of the crystal rod fabrication structure of this application;

[0040] In the diagram, 100 represents the crystal rod, 200 represents the shoulder, and 300 represents the crucible. Detailed Implementation

[0041] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application. In addition, in the description of this application, the term "comprising" means "including but not limited to". The terms first, second, third, etc. are used only as illustrative purposes and do not impose numerical requirements or establish an order. Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is only for convenience and conciseness and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range. Additionally, whenever a numerical range is specified in this document, it means that any referenced number (fraction or integer) within the range is included.

[0042] The main source of oxygen impurities in single-crystal silicon is the incorporation of SiO produced by the reaction between the quartz crucible and the silicon raw material. At a high temperature of 1400℃, the silicon melt and the quartz crucible undergo a chemical reaction:

[0043] Si + SiO₂ → 2SiO SiO + Si → O

[0044] At high temperatures, most of the SiO evaporates from the free surface of the melt, while oxygen atoms enter the crystal rod through segregation after the SiO in the dispersion boundary layer at the solid-liquid interface decomposes.

[0045] Because silicon contains oxygen, it improves the mechanical strength of silicon wafers to some extent. During post-processing, high temperatures can form oxygen precipitates and corresponding defects, which can reduce dispersed carrier recombination centers and improve the utilization efficiency and photoelectric conversion efficiency of solar cells. However, if a large amount of oxygen impurity precipitates (>16 ppma) during the later stages of manufacturing, it will cause oxygen warping of the silicon wafer and create a large number of secondary defects, which will affect the performance of the cell to some extent and have a destructive effect.

[0046] This application replaces the argon gas introduced into the furnace during the original single crystal growth process with a hydrogen-containing gas, which reduces the oxygen content of the single crystal and thus reduces defects inside the single crystal silicon. In some embodiments, this application provides a method for preparing a crystal rod, including a shoulder-turning step and a diameter-equalizing step, wherein a hydrogen-containing gas is introduced during the shoulder-turning step and / or the diameter-equalizing step; the hydrogen-containing gas includes hydrogen gas, and the mass of the hydrogen gas is m. H The total mass of hydrogen-containing gas is m 总 , satisfying: m H / m 总 ≤30%.

[0047] In some embodiments, the hydrogen-containing gas is a mixture of hydrogen and argon.

[0048] In some embodiments, the hydrogen-containing gas is a mixture of hydrogen and nitrogen.

[0049] This application introduces hydrogen as a protective gas during the silicon single crystal pulling process. The silicon crystal is placed in a vacuum furnace, and during the heat treatment of the silicon crystal, the protective gas, which is a hydrogen-containing gas, is introduced into the vacuum furnace and flows over the surface of the silicon crystal. The mixture of hydrogen-containing gas and inert gas used in this application, when used to heat-treat the silicon crystal, significantly improves the minority carrier lifetime of the silicon crystal due to the passivation and gettering effects of hydrogen on impurities and defects within the silicon crystal. Simultaneously, it adjusts the uniformity of the radial and axial resistivity distribution of the silicon crystal, making the resistivity more uniform along the crystal radius and length directions. This method is simple to operate, easy to industrialize, and significantly improves product quality.

[0050] In some embodiments, the percentage of hydrogen gas by mass of the total hydrogen-containing gas is any value or a range of any two of the following: 5, 10, 15, 20, 25, 30.

[0051] In some embodiments, during the crystal rod preparation process, argon gas or hydrogen-containing gas is introduced, and the flow rate of the introduced gas is 20 slpm to 220 slpm.

[0052] In some embodiments, the inlet gas flow rate (slpm) is any value or a range of any two values ​​from 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220.

[0053] In some embodiments, the preparation of the crystal rod further includes the steps of melting, welding, crystal pulling, and shoulder expansion, wherein a hydrogen-containing gas is introduced in any one or more of the steps of melting, welding, crystal pulling, and shoulder expansion.

[0054] In some embodiments, the shoulder expansion step includes growing the shoulders to the target shoulder length stage, such as... Figure 1 As shown, during the shoulder expansion process, the shoulder length is L1, and the target shoulder length is L; in the stage of 0 < L1 ≤ 0.3L, the first crucible is controlled to rotate V1; in the stage of 0.3L < L1 ≤ L, the second crucible is controlled to rotate V2; satisfying: V1 > V2.

[0055] In some embodiments, the range of the first crucible rotation V1 is 9 r / min to 15 r / min, such that the first crucible rotation V1 (r / min) is any value or a range of any two values ​​among 9, 10, 11, 12, 13, 14, and 15.

[0056] In some embodiments, the range of the second crucible rotation V2 is 7 r / min to 12 r / min, and the value of the second crucible rotation V2 (r / min) is any value or a range of any two values ​​among 7, 8, 9, 10, 11, and 12.

[0057] In some embodiments, during the shoulder expansion step, the shoulder length during the expansion process is L1, and the target shoulder length is L; wherein, in the stage of 0 < L1 ≤ 0.3L, the time for introducing hydrogen-containing gas is T1; in the stage of 0.3L < L1 ≤ 0.6L, the time for introducing hydrogen-containing gas is T2; in the stage of 0.6L < L1 ≤ L, the time for introducing hydrogen-containing gas is T3; the total time for introducing hydrogen-containing gas in the shoulder expansion step is T. 扩肩 T 扩肩 =T1+T2+T3; satisfying: T2<T1.

[0058] In some embodiments, T2 < T3 is satisfied.

[0059] In some embodiments, T3 < T1 is satisfied.

[0060] In some embodiments, T1 ranges from 0.6h to 1.8h, such that T1(h) can be any value or a range of any two values ​​from 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8.

[0061] In some embodiments, T2 ranges from 0.3h to 1.5h, such that T2(h) takes any value or a range of any two values ​​from 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5.

[0062] In some embodiments, T3 ranges from 0.5h to 1.6h, such that T3(h) takes any value or a range of any two values ​​from 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6.

[0063] In some embodiments, in the stage of 0 < L1 ≤ 0.3 L, the hydrogen content in the hydrogen-containing gas is less than or equal to 15%, such that the hydrogen content (%) in the hydrogen-containing gas is any value among 5, 10, and 15 or a range of any two values.

[0064] In some embodiments, in the 0.3L < L1 ≤ 0.6L stage, the hydrogen content in the hydrogen-containing gas is less than or equal to 15%, such that the hydrogen content (%) in the hydrogen-containing gas is any value among 5, 10, and 15 or a range of any two values.

[0065] In some embodiments, in the 0.6L < L1 ≤ L stage, the hydrogen content in the hydrogen-containing gas is ≤15%, such that the hydrogen content (%) in the hydrogen-containing gas is any value among 5, 10, and 15 or a range of any two values.

[0066] In some embodiments, during the equal diameter step, in the stage of 0 < H1 ≤ 0.11H, the third crucible is controlled to rotate to V3; in the stage of 0.11H < H1 ≤ H, the fourth crucible is controlled to rotate to V4, satisfying: V3 > V4, H1 is the crystal pulling length, and H is the total length of the target crystal rod.

[0067] like Figure 1 As shown, during the crystal growth process, the crystal pulling length H1 is the length from the crucible liquid surface to the top of the crystal rod. The total length of the target crystal rod H is the total length of the crystal rod after crystal growth is completed.

[0068] In some embodiments, the range of the third crucible rotation V3 is 7 r / min to 12 r / min, and the value of the third crucible rotation V3 (r / min) is any value or a range of any two values ​​among 7, 8, 9, 10, 11, and 12.

[0069] In some embodiments, the range of the fourth crucible rotation V4 is 6 r / min to 10 r / min, and the value of the fourth crucible rotation V4 (r / min) is any value among 6, 7, 8, 9, and 10 or a range of any two values.

[0070] In some embodiments, the equal diameter step includes a first equal diameter stage, wherein 0 < H1 ≤ 0.11H, and a hydrogen-containing gas is introduced during the first equal diameter stage, wherein H1 is the crystal pulling length and H is the total length of the target crystal rod.

[0071] In some embodiments, the equal diameter step includes a second equal diameter stage, a third equal diameter stage, and a fourth equal diameter stage; the second equal diameter stage is the 0.11H < H1 ≤ 0.33H stage; the third equal diameter stage is the 0.33H < H1 ≤ 0.77H stage; and the fourth equal diameter stage is the 0.77H < H1 ≤ H stage; hydrogen-containing gas is introduced into any one or more of the second, third, and fourth equal diameter stages.

[0072] In some embodiments, the time for introducing hydrogen-containing gas in the first equal diameter stage is T4, the time for introducing hydrogen-containing gas in the second equal diameter stage is T5, the time for introducing hydrogen-containing gas in the third equal diameter stage is T6, and the time for introducing hydrogen-containing gas in the fourth equal diameter stage is T7.

[0073] In some embodiments, hydrogen-containing gas is introduced into the first, second, third, and fourth equal diameter stages.

[0074] In some embodiments, the value of T4 is in the range of 5h to 9h, such as T4(h) being any value among 5, 6, 7, 8, and 9 or a range of any two values.

[0075] In some embodiments, the value of T5 is in the range of 8h to 16h, such that T5(h) is any value or a range of any two values ​​among 8, 9, 10, 11, 12, 13, 14, 15, and 16.

[0076] In some embodiments, the value of T6 is in the range of 16h to 24h, such that T6(h) is any value or a range of any two values ​​among 16, 17, 18, 19, 20, 21, 22, 23, and 24.

[0077] In some embodiments, the value of T7 is in the range of 9h to 15h, such that T7(h) is any value or a range of any two values ​​among 9, 10, 11, 12, 13, 14, and 15.

[0078] In some embodiments, the following condition is satisfied: T4 < T5 = T7 < T6.

[0079] In some embodiments, the hydrogen content in the hydrogen-containing gas introduced in the first equal diameter stage is less than or equal to 15%, such that the hydrogen content (%) in the hydrogen-containing gas introduced in the first equal diameter stage is any value or a range of any two values ​​among 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, and 15.

[0080] In some embodiments, the hydrogen content in the hydrogen-containing gas introduced in the second equal diameter stage is less than or equal to 10%, such that the hydrogen content (%) in the hydrogen-containing gas introduced in the second equal diameter stage is any value or a range of any two values ​​from 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10.

[0081] In some embodiments, the hydrogen content in the hydrogen-containing gas introduced in the third equal diameter stage is less than or equal to 10%, such that the hydrogen content (%) in the hydrogen-containing gas introduced in the third equal diameter stage is any value or a range of any two values ​​from 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10.

[0082] In some embodiments, the hydrogen content in the hydrogen-containing gas introduced in the fourth equal diameter stage is less than or equal to 10%, such that the hydrogen content (%) in the hydrogen-containing gas introduced in the fourth equal diameter stage is any value or a range of any two values ​​from 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10.

[0083] In some embodiments, the hydrogen content of the hydrogen-containing gas in the first isodiameter stage is higher than the hydrogen content in the second, third, and fourth isodiameter stages.

[0084] In some embodiments, hydrogen content in this application refers to the mass percentage of hydrogen in a hydrogen-containing gas.

[0085] In some embodiments, the melting step includes feeding, refeeding and volatilization steps, and the feeding temperature is 300℃~1600℃, such that the feeding temperature (℃) is any value or a range of any two values ​​among 300, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500 and 1600.

[0086] In some embodiments, the re-addition temperature is 1400℃~1600℃, such that the re-addition temperature (℃) is any value or a range of any two values ​​among 1400, 1450, 1500, 1550, and 1600.

[0087] In some embodiments, the evaporation temperature is 1460℃~1480℃, such that the evaporation temperature (℃) is any value among 1460, 1470, and 1480℃ or a range of any two values.

[0088] In some embodiments, the feeding time is 4h to 12h, such that the feeding time (h) is any value or a range of any two values ​​among 4, 5, 6, 7, 8, 9, 10, 11, and 12.

[0089] In some embodiments, the re-addition time is 3h to 10h, such that the re-addition time (h) takes any value from 3, 4, 5, 6, 7, 8, 9, 10 or a range of any two values.

[0090] In some embodiments, the evaporation time is 0.3h to 3h, such that the evaporation time (h) is any value or a range of any two values ​​among 0.3, 0.5, 1, 1.5, 2, 2.5, and 3.

[0091] In some embodiments, a hydrogen-containing gas is introduced during the melting step. The hydrogen content in the hydrogen-containing gas is less than or equal to 30%, such that the hydrogen content (%) is any value or a range of any two values ​​from 0, 5, 10, 15, 20, 25, and 30.

[0092] In some embodiments, hydrogen-containing gas is introduced during the feeding stage, with a hydrogen content of less than or equal to 30%, such as any value or a range of any two of the following: 0, 5, 10, 15, 20, 25, and 30.

[0093] In some embodiments, hydrogen-containing gas is introduced during the re-injection stage, with a hydrogen content of less than or equal to 20%, such as any value or a range of any two of the following: 0, 5, 10, 15, and 20.

[0094] In some embodiments, hydrogen-containing gas is introduced during the volatilization stage, with a hydrogen content of less than or equal to 20%, such as any value or a range of any two of the following: 0, 5, 10, 15, and 20.

[0095] In some embodiments, the welding step includes a high-temperature preheating stage and a low-temperature welding stage.

[0096] In some embodiments, the temperature of the high-temperature preheating stage is 1457℃~1475℃, such that the temperature (℃) of the high-temperature preheating stage is any value or a range of any two values ​​among 1457, 1460, 1465, 1470, and 1475.

[0097] In some embodiments, the temperature of the low-temperature welding stage is 1449℃~1457℃, such that the temperature (℃) of the low-temperature welding stage is any value or a range of any two values ​​among 1449, 1450, 1451, 1452, 1453, 1454, 1455, 1456, and 1457.

[0098] In some embodiments, the crucible rotation speed in the welding step is in the range of 9 r / min to 15 r / min, such as the crucible rotation speed (r / min) being any value or a range of any two values ​​among 9, 10, 11, 12, 13, 14, and 15.

[0099] In some embodiments, the duration of the high-temperature preheating stage is 0.1h to 1h, such that the duration (h) of the high-temperature preheating stage is any value or a range of any two values ​​among 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and 1.0.

[0100] In some embodiments, the duration of the low-temperature welding stage is 0.1h to 4h, such that the duration (h) of the low-temperature welding stage is any value or a range of any two values ​​among 0.1, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, and 4.0.

[0101] In some embodiments, a hydrogen-containing gas is introduced during the welding step. The hydrogen content in the hydrogen-containing gas is less than or equal to 15%, such as any value of 0, 5, 10, or 15, or a range of any two values.

[0102] In some embodiments, the boron and / or gallium content in the raw materials used to prepare the crystal rod is 0.007 mg / g to 0.8 mg / g.

[0103] In some embodiments, the phosphorus content in the raw materials for preparing the crystal rods is 0.001 mg / g to 0.01 mg / g.

[0104] In some embodiments, the boron content (mg / g) in the raw material of monocrystalline silicon is any value or a range of any two values ​​from 0.007, 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8.

[0105] In some embodiments, the gallium content (mg / g) in the raw material of monocrystalline silicon is any value or a range of any two values ​​from 0.007, 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8.

[0106] In some implementations, the phosphorus content (mg / g) in the monocrystalline silicon raw material is taken as any value or a range of any two values ​​from 0.001, 0.005, and 0.01.

[0107] In this application, resistivity is the ratio of the product of the resistance and cross-sectional area of ​​the crystal rod to its length. It is a substance formed by silicon atoms in a certain arrangement. Silicon doped with phosphorus is n-type, and the more phosphorus doped, the more free electrons there are, the stronger the conductivity, and the lower the resistivity. Conversely, silicon doped with boron is p-type, and the more boron doped, the more holes generated by silicon can be replaced, the stronger the conductivity, and the lower the resistivity. The smaller the resistivity concentration, i.e. the ratio of the head to the tail, the better. This is beneficial to the crystal rod quality compliance rate and also directly affects the conversion efficiency of solar cells.

[0108] In this application, the content of boron, gallium or phosphorus refers to the ratio of the mass of boron, gallium or phosphorus to the mass of monocrystalline silicon raw material. Taking boron as an example, the mass of boron is M1 mg, the mass of monocrystalline silicon raw material is M2 g, and the boron content = M1 / M2 mg / g.

[0109] This application reduces the formation of boron-oxygen complexes and prevents the cell efficiency from degrading by introducing hydrogen gas during the crystal rod preparation process, especially when pulling boron-doped single crystals.

[0110] Accordingly, this application provides a crystal rod prepared by the above-described method. By introducing hydrogen-containing gas during the crystal rod preparation process, this application can reduce the oxygen content of monocrystalline silicon, thereby reducing internal defects, increasing the resistivity at the crystal tail, and improving minority carrier lifetime. This allows for an increase in the length of the pulled crystal rod, reducing the total time spent in the non-uniform diameter state, and increasing yield. Simultaneously, it can improve the conversion efficiency of solar cells. This application can reduce the generation and accumulation of oxides in the monocrystalline furnace, reducing the time and frequency of oxide cleaning after furnace shutdown, reducing manual labor, and enabling the monocrystalline furnace to start production faster, saving time and increasing yield. Furthermore, by controlling the parameters during the crystal rod preparation process, this application obtains high-quality monocrystalline silicon products for improving the efficiency of downstream battery modules.

[0111] Example 1:

[0112] The furnace charge consists of 500 kg of raw material, composed of 50% virgin polycrystalline silicon and 50% gallium-containing recycled material by mass percentage. The virgin polycrystalline silicon contains 0.5 mg of boron and 0.1 mg of phosphorus. The recycled material contains 5.5 mg of boron, and the bottom material contains 0.9 mg of phosphorus. Additionally, 86 g of boron doping is added.

[0113] The material was melted at 1500℃ for 8 hours, and a hydrogen-containing gas was introduced at a flow rate of 110 slpm. The hydrogen content in the hydrogen-containing gas was 20%, the argon content was 80%, and the crucible rotation speed was 3 r / min.

[0114] Re-addition: After melting, add 560 kg of raw polycrystalline silicon from the melting stage again at a temperature of 1500℃ for 7 hours. Then, introduce hydrogen gas at a flow rate of 110 slpm. The hydrogen gas contains 10% hydrogen and 90% argon. The crucible rotation speed is 6 r / min.

[0115] Volatilization: The temperature is controlled at 1470℃, volatilization is carried out for 2 hours, hydrogen-containing gas is introduced, the flow rate of hydrogen-containing gas is 110 slpm, the hydrogen content in the hydrogen-containing gas is 10%, the argon content is 90%, and the crucible rotation speed is 6 r / min.

[0116] Fusion welding:

[0117] High-temperature preheating: Preheat at 1470℃ for 0.3h, introduce hydrogen-containing gas at a flow rate of 100slpm, the hydrogen content in the hydrogen-containing gas is 10%, the argon content is 90%, and the crucible rotation speed is 12r / min.

[0118] Low-temperature welding: Welding is carried out at 1450℃ for 2 hours, with hydrogen-containing gas introduced at a flow rate of 100 slpm. The hydrogen content in the hydrogen-containing gas is 5%, the argon content is 95%, and the crucible rotation speed is 12 r / min.

[0119] Crystal introduction: The crystal introduction temperature is maintained at 1450℃ for 1 hour. Hydrogen-containing gas is introduced at a flow rate of 100 slpm. The hydrogen content in the hydrogen-containing gas is 5%, the argon content is 95%, and the crucible rotation speed is 12 r / min.

[0120] Shoulder expansion: When the shoulder length is 0-75mm, control the pulling speed at 1.4mm / min for 1.2h, introduce hydrogen-containing gas at a flow rate of 100slpm, with a hydrogen content of 5% and an argon content of 95%, and the crucible rotation speed at 12r / min.

[0121] When the shoulder length is 75mm to 149mm, the pulling speed is controlled at 1.5mm / min, the time is 0.9h, hydrogen-containing gas is introduced at a flow rate of 100slpm, the hydrogen content is 5%, the argon content is 95%, and the crucible rotation speed is 10r / min.

[0122] When the shoulder length is 150mm~250mm, the pulling speed is controlled at 1.5mm / min, the time is 1h, hydrogen-containing gas is introduced, the flow rate of hydrogen-containing gas is 100slpm, the hydrogen content in the hydrogen-containing gas is 5%, the argon content is 95%, and the crucible rotation speed is 10r / min.

[0123] Shoulder rotation: During the shoulder rotation process, the power of the main heater is maintained at 50kW, the pulling speed is controlled at 1.2mm / min, the time is 0.2h, hydrogen-containing gas is introduced, the flow rate of the hydrogen-containing gas is 100slpm, the hydrogen content in the hydrogen-containing gas is 5%, the argon content is 95%, and the crucible rotation speed is 10r / min.

[0124] Equal diameter: When the length of the crystal rod is 0-500mm, the equal diameter time is 7h, hydrogen-containing gas is introduced at a flow rate of 100slpm, the hydrogen content in the hydrogen-containing gas is 15%, the argon content is 85%, the crucible rotation speed is 10r / min, and the heating power of the heater is maintained at 46KW.

[0125] When the length of the crystal rod is 500mm to 1500mm, the constant diameter time is 12h, hydrogen-containing gas is introduced at a flow rate of 100slpm, the hydrogen content in the hydrogen-containing gas is 10%, the argon content is 90%, the crucible rotation speed is 8r / min, and the heating power of the heater is maintained at 46KW.

[0126] When the length of the crystal rod is 1500mm to 3500mm, the constant diameter time is 20h, hydrogen-containing gas is introduced at a flow rate of 100slpm, the hydrogen content is 10%, the argon content is 90%, the crucible rotation speed is 8r / min, and the heating power of the heater is maintained at 49KW.

[0127] When the length of the crystal rod is 3500mm to 4500mm, the constant diameter time is 12h, hydrogen-containing gas is introduced at a flow rate of 100slpm, the hydrogen content is 10%, the argon content is 90%, the crucible rotation speed is 8r / min, and the heating power of the heater is maintained at 49KW.

[0128] The preparation parameters for Example 1 are shown in Table 1.

[0129] Table 1. Crystal rod preparation parameters for Example 1

[0130]

[0131]

[0132] Example 2: The preparation method is different from that of Example 1. The difference is that the time period of hydrogen gas passage is changed. The specific parameters are detailed in Table 2.

[0133] Table 2. Crystal rod preparation parameters for Example 2

[0134]

[0135]

[0136] Example 3: The preparation method is different from that of Example 1. The difference is that the time period of hydrogen gas passage is changed. The specific parameters are detailed in Table 3.

[0137] Table 3. Crystal rod preparation parameters for Example 3

[0138]

[0139]

[0140] Example 4: The preparation method is different from that of Example 1. The difference is that the time period of hydrogen gas passage is changed. The specific parameters are detailed in Table 4.

[0141] Table 4. Crystal rod preparation parameters in Example 4

[0142]

[0143] Example 5: The preparation method is different from that of Example 1. The difference is that the parameters of the hydrogen gas are changed. The specific parameters are detailed in Table 5.

[0144] Table 5. Crystal rod preparation parameters in Example 5

[0145]

[0146] Example 6: The preparation method is the same as in Example 1, except that the rotation speed of the first and second crucibles is controlled at 10 r / min.

[0147] Example 7: The preparation method is the same as in Example 1, except that during the shoulder expansion process, the processing time is controlled to be 1 hour in the shoulder length 0-75mm stage, the shoulder length 76mm-149mm stage, and the shoulder length 150mm-245mm stage, and the time for introducing hydrogen gas is controlled to be 1 hour.

[0148] Example 8: The preparation method is the same as in Example 1, except that during the equal diameter process, the rotation speed of the third and fourth crucibles is controlled to be 8 r / min.

[0149] Example 9: The preparation method is the same as in Example 1, except that during the constant diameter process, the step duration is controlled to be 9 hours and the hydrogen gas introduction time is 9 hours when the crystal rod length is 0-500 mm; the step duration is controlled to be 9 hours and the hydrogen gas introduction time is 9 hours when the crystal rod length is 500 mm-1500 mm; the step duration is controlled to be 20 hours and the hydrogen gas introduction time is 20 hours when the crystal rod length is 1500 mm-3500 mm; and the step duration is controlled to be 9 hours and the hydrogen gas introduction time is 9 hours when the crystal rod length is 3500 mm-4500 mm.

[0150] Example 10: The preparation method is the same as in Example 4, except that the hydrogen content in the hydrogen-containing gas introduced during the constant diameter process is 20%.

[0151] Comparative Example 1: The preparation method is the same as in Example 1, except that argon gas is introduced throughout the process.

[0152] Performance testing: The crystal rods prepared in Examples 1-10 and Comparative Example 1 were subjected to performance testing, and the testing methods are as follows.

[0153] Resistivity testing: The resistivity of the crystal rod was tested using a KDY~1A resistivity tester.

[0154] The method for testing oxygen content in the crystal rod tip is as follows: the oxygen content in the crystal rod tip is measured, and the test method is as described in GB / T1557~2018. The oxygen content in the crystal rod is tested using a Nicolet 6700 Fourier transform infrared spectrometer.

[0155] Lifetime testing: The minority carrier lifetime of the crystal rod was tested using a Sinton BLS-1 minority carrier lifetime tester.

[0156] Carbon content testing method: The carbon content in the crystal rod was tested using a Nicolet 6700 Fourier transform infrared spectrometer.

[0157] Defect testing method: The PL defect tester is used to test the defects of the crystal rod.

[0158] Table 6 Test Results

[0159]

[0160]

[0161] The results above show that the oxygen content in the crystal rods prepared by the furnaces in Examples 1-10 with hydrogen-containing gas is significantly lower than that in Comparative Example 1. This indicates that a hydrogen reduction reaction occurs after gas introduction, reducing the oxygen concentration at the solid-liquid interface and thus lowering the oxygen content in the single-crystal silicon. Simultaneously, it can improve minority carrier lifetime and pull number. Furthermore, the introduction of hydrogen-containing gas during the crystal rod preparation process in this application can reduce defects in single-crystal silicon.

[0162] Data from Examples 1 to 10 show that hydrogen is located at the bonding center of the B-Si bond in boron- or gallium-doped P-type single-crystal silicon. The distance between hydrogen and boron or gallium is 0.135 nm, while the distance to silicon is 0.164 nm, clearly indicating the potential to form B / G-H bonds. Theoretical calculations show that the stretching vibration of the B / G-H infrared spectrum (IR) is 2031 cm⁻¹. ~1 The oscillation length is 233cm. ~1 The experimentally measured stretching vibration of B to H was 1903 cm. ~1 When boron or gallium concentrations are low, i.e., resistivity is high (10–100 Ω·cm), boron or gallium combines with a single hydrogen atom or two hydrogen atoms. When resistivity is low (0–0.1 Ω·cm), boron or gallium combines with multiple hydrogen atoms (B–H⁸–12), thus weakening the acceptor properties of boron or gallium. Hydrogen impurities combine with boron or gallium to form H–B / G complexes, reducing the boron or gallium concentration in silicon and increasing resistivity. Other acceptor impurities, such as aluminum, phosphorus, and indium, can also form complexes with hydrogen, leading to increased resistivity. This allows for the fabrication of longer single crystal rods (silicon rods), improving product yield and quality.

[0163] As can be seen from the data in Examples 1 to 10, the solution of this application can significantly reduce the difference between the resistivity at the head and tail of the crystal rod, and improve the axial uniformity of the crystal rod.

[0164] The minority carrier lifetime mainly originates from harmful metal elements in various processes; the impact of a low minority carrier lifetime is that it directly affects the conversion efficiency of solar cells. This application introduces hydrogen-containing gas during the crystal rod preparation process to improve the minority carrier lifetime.

[0165] In the above embodiments, the descriptions of each embodiment have different focuses. For parts not described in detail in a certain embodiment, please refer to the relevant descriptions in other embodiments.

[0166] The preparation method of a crystal rod and the crystal rod provided in the embodiments of this application have been described in detail above. Specific examples have been used to illustrate the principle and implementation of this application. The description of the above embodiments is only for the purpose of helping to understand the method and core idea of ​​this application. At the same time, for those skilled in the art, there will be changes in the specific implementation and application scope based on the idea of ​​this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A method for preparing a crystal rod, comprising a shoulder widening step, a shoulder turning step, and a constant diameter step, characterized in that, During the equal diameter step, hydrogen-containing gas is introduced; or, during the shoulder turning step and the equal diameter step, hydrogen-containing gas is introduced. The hydrogen-containing gas includes hydrogen gas, and the mass of the hydrogen gas is m. H The total mass of the hydrogen-containing gas is m 总 , satisfying: m H / m 总 ≤30%; The shoulder expansion step includes growing the shoulder to the target shoulder length, where the shoulder length is L1 and the target shoulder length is L; in the stage of 0 < L1 ≤ 0.3L, the first crucible is controlled to rotate to V1; in the stage of 0.3L < L1 ≤ L, the second crucible is controlled to rotate to V2; satisfying: V1 > V2; In the shoulder expansion step, the hydrogen content in the hydrogen-containing gas is ≤15%; In the equal diameter step, during the stage of 0 < H1 ≤ 0.11H, the third crucible is controlled to rotate to V3; during the stage of 0.11H < H1 ≤ H, the fourth crucible is controlled to rotate to V4, satisfying: V3 > V4, where H1 is the crystal pulling length and H is the total length of the target crystal rod; The raw materials used to prepare the crystal rod include boron and / or gallium, or the raw materials used to prepare the crystal rod include phosphorus.

2. The method for preparing a crystal rod according to claim 1, characterized in that, The method for preparing the crystal rod further includes the steps of melting, welding, crystal pulling, and shoulder expansion, wherein the hydrogen-containing gas is introduced in any one or more of the steps of melting, welding, crystal pulling, and shoulder expansion.

3. The method for preparing a crystal rod according to claim 2, characterized in that, In the shoulder expansion step, the shoulder length is L1, and the target shoulder length is L; Specifically, in the stage where 0 < L1 ≤ 0.3 L, the time for introducing the hydrogen-containing gas is T1; in the stage where 0.3 L < L1 ≤ 0.6 L, the time for introducing the hydrogen-containing gas is T2; in the stage where 0.6 L < L1 ≤ L, the time for introducing the hydrogen-containing gas is T3; the total time for introducing the hydrogen-containing gas in the expansion step is T. 扩肩 T 扩肩 =T1+T2+T3; Satisfy: T2 < T1; And / or, satisfying: T2 < T3; And / or, satisfying: T3 < T1.

4. The method for preparing a crystal rod according to claim 1, characterized in that, The rotation speed of the first crucible, V1, ranges from 9 r / min to 15 r / min. And / or, the range of the second crucible rotation V2 is 7 r / min to 12 r / min.

5. The method for preparing a crystal rod according to claim 1, characterized in that, The equal diameter step includes a first equal diameter stage, wherein 0 < H1 ≤ 0.11H, and hydrogen-containing gas is introduced during the first equal diameter stage, wherein H1 is the crystal pulling length.

6. The method for preparing a crystal rod according to claim 5, characterized in that, The equal diameter step includes a second equal diameter stage, a third equal diameter stage, and a fourth equal diameter stage; the second equal diameter stage is the 0.11H < H1 ≤ 0.33H stage; the third equal diameter stage is the 0.33H < H1 ≤ 0.77H stage; and the fourth equal diameter stage is the 0.77H < H1 ≤ H stage; the hydrogen-containing gas is introduced in any one or more of the second, third, and fourth equal diameter stages.

7. The method for preparing a crystal rod according to claim 6, characterized in that, The hydrogen-containing gas is introduced at time T4 in the first equal diameter stage, at time T5 in the second equal diameter stage, at time T6 in the third equal diameter stage, and at time T7 in the fourth equal diameter stage; satisfying: T4 < T5 = T7 < T6. And / or, the hydrogen content of the hydrogen-containing gas in the first isodiameter stage is higher than the hydrogen content of the hydrogen-containing gas in each of the second, third, and fourth isodiameter stages.

8. The method for preparing a crystal rod according to claim 2, characterized in that, The melting process includes feeding, refeeding and volatilization steps, and the feeding temperature is 300℃~1600℃; And / or, the re-addition temperature is 1400~1600℃; and / or, the volatilization temperature is 1460℃~1480℃.

9. The method for preparing a crystal rod according to claim 8, characterized in that, The feeding time is 4~12 hours; And / or, the re-application time is 3h~10h; And / or, the evaporation time is 0.3h to 3h.

10. The method for preparing a crystal rod according to claim 8, characterized in that, The melting step involves introducing a hydrogen-containing gas, wherein the hydrogen content in the hydrogen-containing gas is less than or equal to 30%. And / or, during the feeding stage, hydrogen-containing gas is introduced, with a hydrogen content of less than or equal to 30%; And / or, during the re-injection stage, hydrogen-containing gas is introduced, with a hydrogen content of less than or equal to 20%, and during the volatilization stage, hydrogen-containing gas is introduced, with a hydrogen content of less than or equal to 20%.

11. The method for preparing a crystal rod according to claim 2, characterized in that, The welding process includes a high-temperature preheating stage and a low-temperature welding stage; the temperature of the high-temperature preheating stage is 1457℃~1475℃, and the temperature of the low-temperature welding stage is 1449℃~1457℃. And / or, the crucible rotation speed in the welding step is in the range of 6 r / min ~ 15 r / min; And / or, in the welding step, a hydrogen-containing gas is introduced, wherein the hydrogen content in the hydrogen-containing gas is less than or equal to 15%; And / or, the duration of the high-temperature preheating stage is 0.1h to 1h; and / or, the duration of the low-temperature welding stage is 0.1h to 4h.

12. The method for preparing a crystal rod according to claim 1, characterized in that, The boron and / or gallium content in the raw materials used to prepare the crystal rod is 0.007 mg / g to 0.8 mg / g, or... The phosphorus content in the raw materials used to prepare the crystal rod is 0.001 mg / g to 0.01 mg / g.

13. A crystal rod, characterized in that, The crystal rod is prepared by the method described in any one of claims 1 to 12.

Citation Information

Patent Citations

  • Preparation of low oxygen content silicon crystal

    CN101435105A

  • Large-size monocrystalline silicon rod crystallization and quality improvement process method in large thermal field environment

    CN112301420A

  • Crystal pulling method

    CN115404541A