A method for degassing and packaging a battery cell, a soft-pack battery cell, and an electrical device thereof.
By combining serrated interlocking encapsulation with planar encapsulation, the sealing problem in the packaging process of soft-pack battery cells is solved, achieving flatness and reliability of the seal, reducing the risk of leakage, and improving the safety and service life of the battery cells.
Patent Information
- Application Number
- CN202311128843.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-04
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-09-04
AI Technical Summary
In the existing degassing and encapsulation process of soft-pack battery cells, pinholes or channels in the molten adhesive can easily occur, resulting in unsealed encapsulation and affecting product safety.
The method of combining serrated interlocking encapsulation with planar encapsulation is adopted. First, serrated interlocking encapsulation is performed to enhance the sealing performance of the aluminum-plastic film, and then planar encapsulation is performed to flatten the molten adhesive pinholes or channels, ensuring the flatness and reliability of the seal.
This improves the sealing and reliability of the battery cell, reduces the risk of leakage, and ensures the flatness and appearance quality of the seal.
Smart Images

Figure CN117175021B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of secondary batteries, specifically to a method for degassing and packaging battery cells, as well as a soft-pack battery cell and an electrical device. Background Technology
[0002] The outer shell of a soft-pack battery cell is made of aluminum-plastic film. The bare battery cell is wrapped in the aluminum-plastic film PP by heating and fusing it to form the battery cell. The battery cell process includes aluminum-plastic film punching, bare battery cell installation into the shell, top sealing, side sealing, battery cell baking, electrolyte injection, primary sealing, formation charging, degassing sealing, and battery cell formation. The degassing sealing process is mainly to remove excess gas or free electrolyte from inside the battery cell. Due to the presence of electrolyte during sealing, and the influence of electrolyte additives, infusible substances may sometimes form. This can cause molten glue pinholes or channels in the secondary seal during degassing sealing, leading to battery cell swelling and leakage, which affects product safety. Summary of the Invention
[0003] One of the objectives of this invention is to provide a cell degassing and encapsulation method to address the shortcomings of existing technologies. This method involves first performing a serrated interlocking encapsulation followed by a flat encapsulation to flatten out pinholes or channels in the molten adhesive, thereby sealing and fusing the aluminum layers between the aluminum-plastic films to ensure a tight and leak-proof encapsulation.
[0004] To achieve the above objectives, the present invention adopts the following technical solution:
[0005] A method for degassing and encapsulating a battery cell includes the following steps:
[0006] Step S1: Puncture the air bag of the aluminum-plastic film of the battery cell after it has been charged, draw a vacuum, heat the serrated end cap, and perform serrated interlocking sealing in the secondary sealing area.
[0007] Step S2: Perform planar encapsulation on the secondary encapsulation area of the aluminum-plastic film, and cut the air bag to obtain the finished battery cell.
[0008] This invention discloses a cell degassing and encapsulation method that combines serrated interlocking encapsulation with flat encapsulation. The serrated interlocking can compress and interlock the aluminum-plastic film (PP), resulting in good filling effect when the PP flows under heat. This can improve the problem of false sealing caused by abnormal electrolyte or the presence of infusible substances inside the cell in flat encapsulation. The flat end cap can be used to flatten the serrated seal, ensuring the flatness of the seal and avoiding affecting the width of the cell after folding. The combination of these two methods can improve the reliability of degassing and encapsulation, greatly reduce the risk of leakage, and not affect the appearance of the cell seal.
[0009] In step S1, the temperature for the serrated interlocking encapsulation is 160–220°C, the encapsulation time is 2–8 seconds, and the encapsulation pressure is 0.2–0.6 MPa. Setting a specific temperature during serrated interlocking encapsulation can improve the flow and filling effect of the PP adhesive in the aluminum-plastic film, thereby reducing the probability of pinholes or channels. Specifically, the temperature for serrated interlocking encapsulation can be 160°C, 180°C, 190°C, 200°C, 210°C, or 220°C, and the encapsulation pressure can be 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.5 MPa, or 0.6 MPa.
[0010] In step S1, the serrated interlocking seal has a serration width of 0.5–2 mm, a sawing depth of 0.1–0.5 mm, and a cap width of 2–10 mm. The serrations in the serrated interlocking seal need to be set with a certain serration depth and width to create a certain height difference between the aluminum-plastic films during interlocking, but this height difference will not cause damage to the aluminum-plastic films. Specifically, the serration width of the serrated interlocking seal can be 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, or 2 mm. The sawing depth can be 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, or 0.5 mm. The end cap width can be 2mm, 3mm, 4mm, 5mm, 6mm, 7mm, 8mm, 9mm, or 10mm.
[0011] In step S1, the serration width of the serrated interlocking seal is 0.8–1.8 mm, the saw depth is 0.2–0.5 mm, and the end cap width is 4–8 mm.
[0012] In step S1, the number of serrations in the saw-shaped interlocking seal is 2 to 5. Setting a certain number of serrations ensures that the seal forms a sufficient number of raised and recessed edges, thereby improving the seal's tightness. Specifically, the number of serrations in the saw-shaped interlocking seal can be 2, 3, 4, or 5.
[0013] In step S1, the vacuum level during evacuation is -80 kPa to -100 kPa. Setting a specific vacuum level prevents air from entering and improves the sealing performance of the package. Specifically, the vacuum level can be -80 kPa, -85 kPa, -90 kPa, -95 kPa, or -100 kPa.
[0014] In step S2, the planar packaging temperature is 160–220°C, the time is 3–8 seconds, and the pressure is 0.2–0.6 MPa. Setting a specific packaging temperature allows the uneven edges to return to a flat state without affecting the packaged surface. Specifically, the planar packaging temperature can be 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, or 220°C. The planar packaging time can be 3 seconds, 4 seconds, 5 seconds, 6 seconds, 7 seconds, or 8 seconds.
[0015] In step S2, the planar encapsulation temperature is 180–210°C, the time is 3–8 seconds, and the pressure is 0.2–0.5 MPa.
[0016] The second objective of this invention is to provide a soft-pack battery cell with the advantages of good sealing performance and a flat encapsulation surface.
[0017] To achieve the above objectives, the present invention adopts the following technical solution:
[0018] A pouch cell is obtained by the aforementioned pouch cell degassing and encapsulation method. Traditional pouch cells use planar encapsulation, which makes it difficult to achieve a tight seal and easily leads to leakage. However, the serrated interlocking encapsulation combined with planar encapsulation of this invention increases the seal during encapsulation and ensures the flatness of the seal, without affecting the appearance of the cell seal.
[0019] A pouch cell can be a lithium-ion battery pouch cell, a sodium-ion battery pouch cell, a magnesium-ion battery pouch cell, a calcium-ion battery pouch cell, a potassium-ion battery pouch cell, etc. Preferably, the following secondary battery uses a lithium-ion battery pouch cell as an example. The lithium-ion battery pouch cell includes a positive electrode, a negative electrode, a separator, an electrolyte, and an aluminum-plastic film shell. The separator separates the positive electrode and the negative electrode, and the shell is used to house the positive electrode, the negative electrode, the separator, and the electrolyte.
[0020] The positive electrode includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector. The positive active material layer includes a positive active material, which may be, but is not limited to, a chemical formula such as Li. a Ni x Co y M z O 2-b N b(where 0.95≤a≤1.2, x>0, y≥0, z≥0, and x+y+z=1, 0≤b≤1, M is selected from one or more combinations of Mn and Al, and N is selected from one or more of F, P, and S) The positive electrode active material may also be, but is not limited to, LiCoO2, LiNiO2, LiVO2, LiCrO2, LiMn2O4, LiCoMnO4, Li2NiMn3O8, LiNi 0.5 Mn 1.5 One or more of O4, LiCoPO4, LiMnPO4, LiFePO4, and LiNiPO4 are used. The positive electrode active material can also be modified. Methods for modifying the positive electrode active material are known to those skilled in the art. For example, coating, doping, and other methods can be used to modify the positive electrode active material. The materials used for modification can be one or more combinations of Al, B, P, Zr, Si, Ti, Ge, Sn, Mg, Ce, and W, including but not limited to. The positive electrode current collector is typically a structure or component that collects current. The positive electrode current collector can be any material suitable for use as a positive electrode current collector in lithium-ion batteries. For example, the positive electrode current collector can be, but is not limited to, metal foil, and more specifically, aluminum foil, among others.
[0021] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the surface of the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, which may be one or more of the following: graphite, soft carbon, hard carbon, carbon fiber, mesophase carbon microspheres, silicon-based materials, tin-based materials, lithium titanate, or other metals that can form alloys with lithium. Specifically, the graphite may be selected from one or more of artificial graphite, natural graphite, and modified graphite; the silicon-based material may be selected from one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, and silicon alloys; and the tin-based material may be selected from one or more of elemental tin, tin oxide compounds, and tin alloys. The negative electrode current collector is typically a structure or component that collects current. The negative electrode current collector may be any material suitable for use as a negative electrode current collector in lithium-ion batteries, for example, it may be, but is not limited to, metal foil, and more specifically, copper foil.
[0022] The electrolyte comprises an organic solvent, a lithium electrolyte salt, and additives. The lithium electrolyte salt can be LiPF6 and / or LiBOB used in high-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, and LiPF6 used in low-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, LiPF6, and LiTFSI used in overcharge-resistant electrolytes; or it can be at least one of LiClO4, LiAsF6, LiCF3SO3, and LiN(CF3SO2)2. The organic solvent can be a cyclic carbonate, including PC and EC; it can also be a chain carbonate, including DFC, DMC, or EMC; or it can be a carboxylic acid ester, including MF, MA, EA, MP, etc. The additives include, but are not limited to, at least one of film-forming additives, conductive additives, flame-retardant additives, overcharge-resistant additives, additives for controlling the H2O and HF content in the electrolyte, additives for improving low-temperature performance, and multifunctional additives.
[0023] The separator can be any material suitable for lithium-ion battery separators in the art, for example, it can be one or more of the following: polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester and natural fibers.
[0024] Preferably, the shell is made of stainless steel or aluminum-plastic film. More preferably, the shell is made of aluminum-plastic film.
[0025] The third objective of this invention is to provide an electrical device that has good safety and a long service life.
[0026] To achieve the above objectives, the present invention adopts the following technical solution:
[0027] An electrical device includes the aforementioned soft-pack battery cell. After a certain period of use, the volume pressure inside the battery cell increases, which can lead to leakage at the sealing edge. However, the battery cell of this invention has good sealing performance at the sealing edge, is firmly sealed, is not prone to leakage, has good safety, and a long service life.
[0028] The electrical device of the present invention can be any electrical device according to embodiments of the present invention. In some embodiments, the electrical device includes, but is not limited to: laptop computers, pen input computers, mobile computers, e-book players, portable telephones, portable fax machines, portable copiers, portable printers, stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini CDs, transceivers, electronic notebooks, calculators, memory cards, portable recorders, radios, backup power supplies, motors, automobiles, motorcycles, electric bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries or lithium-ion capacitors, etc.
[0029] Compared with the prior art, the beneficial effects of the present invention are as follows: The present invention provides a cell degassing and encapsulation method, which first performs serrated interlocking encapsulation, allowing the PP adhesive in the aluminum-plastic film to flow and fill under the serrated interlocking, thereby increasing the filling effect. Then, flat encapsulation is performed to flatten the pinholes or channels that appear in the molten adhesive during the serrated interlocking encapsulation, so that the aluminum layers between the aluminum-plastic films are sealed and fused together, resulting in a tight and leak-proof encapsulation. The combination of serrated interlocking encapsulation and flat encapsulation ensures the flatness and reliability of the seal. Attached Figure Description
[0030] Figure 1 This is a cross-sectional diagram of the serrated package using current technology.
[0031] Figure 2 This is a cross-sectional schematic diagram of the air bag after being processed using the cell degassing and encapsulation method of the present invention. Detailed Implementation
[0032] To make the technical solution and advantages of the present invention clearer, the present invention and its beneficial effects will be described in further detail below in conjunction with specific embodiments, but the embodiments of the present invention are not limited thereto.
[0033] Example 1
[0034] A method for degassing and encapsulating a battery cell includes the following steps:
[0035] Step S1: Puncture the air bag of the aluminum-plastic film of the battery cell after it has been charged, draw a vacuum, heat the serrated end cap, and perform serrated interlocking sealing in the secondary sealing area.
[0036] Step S2: Perform planar encapsulation on the secondary encapsulation area of the aluminum-plastic film, and cut the air bag to obtain the finished battery cell.
[0037] In step S1, the temperature of the serrated interlocking encapsulation is 200°C, the encapsulation time is 6 seconds, and the encapsulation pressure is 0.5 MPa.
[0038] In step S1, the serration width of the serrated interlocking seal is 1 mm, the saw depth is 0.4 mm, and the end cap width is 8 mm.
[0039] In step S1, the number of saw teeth in the saw-shaped interlocking encapsulation is 4.
[0040] In step S1, the vacuum level is -90 kPa.
[0041] In step S2, the planar packaging temperature is 180°C, the time is 5 seconds, and the pressure is 0.5 MPa.
[0042] Example 2
[0043] The difference from Example 1 is that in step S1, the serrated interlocking seal has a serration width of 0.8 mm, a saw depth of 0.3 mm, and a cap width of 7 mm.
[0044] The rest is the same as in Example 1, and will not be repeated here.
[0045] Example 3
[0046] The difference from Example 1 is that the serrated teeth of the sawtooth-shaped interlocking seal in step S1 have a width of 0.7 mm, a saw depth of 0.1 mm, and a cap width of 5 mm.
[0047] The rest is the same as in Example 1, and will not be repeated here.
[0048] Example 4
[0049] The difference from Example 1 is that in step S1, the serrated interlocking seal has a serration width of 0.5 mm, a saw depth of 0.2 mm, and a cap width of 4 mm.
[0050] The rest is the same as in Example 1, and will not be repeated here.
[0051] Example 5
[0052] The difference from Example 1 is that the serrated teeth of the sawtooth-shaped interlocking seal in step S1 have a width of 1.8 mm, a saw depth of 0.5 mm, and a cap width of 10 mm.
[0053] The rest is the same as in Example 1, and will not be repeated here.
[0054] Example 6
[0055] The difference from Example 1 is that the number of serrations in the saw-shaped interlocking encapsulation in step S1 is 2.
[0056] The rest is the same as in Example 1, and will not be repeated here.
[0057] Example 7
[0058] The difference from Example 1 is that the number of serrations in the saw-shaped interlocking encapsulation in step S1 is 3.
[0059] The rest is the same as in Example 1, and will not be repeated here.
[0060] Example 8
[0061] The difference from Example 1 is that the temperature of the serrated interlocking encapsulation in step S1 is 180°C, the encapsulation time is 6s, and the encapsulation pressure is 0.5mpa.
[0062] The rest is the same as in Example 1, and will not be repeated here.
[0063] Example 9
[0064] The difference from Example 1 is that the temperature of the serrated interlocking encapsulation in step S1 is 160°C, the encapsulation time is 6s, and the encapsulation pressure is 0.4MPa.
[0065] The rest is the same as in Example 1, and will not be repeated here.
[0066] Example 10
[0067] The difference from Example 1 is that the temperature of the serrated interlocking encapsulation in step S1 is 220°C, the encapsulation time is 5s, and the encapsulation pressure is 0.5MPa.
[0068] The rest is the same as in Example 1, and will not be repeated here.
[0069] Comparative Example 1
[0070] A method for degassing and encapsulating battery cells involves directly planar encapsulating the aluminum-plastic film of the battery cell after formation and charging.
[0071] The cells and secondary batteries obtained from Examples 1 to 10 and Comparative Example 1 were subjected to performance tests, and the test results are recorded in Table 1.
[0072] Cyclic performance test: At 25℃, the lithium-ion secondary battery was charged at a constant current of 1C to 4.25V, then charged at a constant voltage of 4.25V to a current of 0.05C, allowed to stand for 5 minutes, and then discharged at a constant current of 1C to 2.8V. This constitutes one charge-discharge cycle, and the discharge capacity of this cycle is the discharge capacity of the first cycle. The lithium-ion secondary battery was subjected to 800 charge-discharge cycles using the above method, and the discharge capacity of each cycle was recorded. Cycle capacity retention (%) = Discharge capacity of the 800th cycle / Discharge capacity of the first cycle × 100%.
[0073] Flatness: Take a measurement point on the sealing edge and calculate the average distance between the two aluminum layers in the aluminum-plastic film at the measurement point. The average value is the flatness. The better the sealing flatness, the smaller the flatness; the worse the sealing flatness, the higher the flatness.
[0074] Sealing performance: At 25℃, the lithium-ion secondary battery is charged to 4.25V at a constant current of 1C, then charged to 0.05C at a constant voltage of 4.25V, left to stand for 5 minutes, and then discharged to 2.8V at a constant current of 1C. This is one charge-discharge cycle. After the lithium-ion secondary battery has undergone 1000 charge-discharge cycles according to the above method, observe whether any bubbles emerge from the cell liquid.
[0075] Table 1
[0076]
[0077]
[0078] As shown in Table 1 above, the battery cells prepared using the degassing and encapsulation method of this invention exhibit excellent performance. After 800 charge-discharge cycles, they retain over 85% of their capacity. After 1000 charge-discharge cycles, no bubbles emerge when the cells are immersed in the test solution, and the cells do not crack. Furthermore, the flatness of the sealed edges is good, facilitating assembly and improving the battery's capacity retention. This invention's degassing and encapsulation method first performs serrated interlocking encapsulation, allowing the PP adhesive in the aluminum-plastic film to flow and fill under the serrated interlocking, increasing the filling effect. Then, flat encapsulation is performed to flatten any pinholes or channels appearing in the molten adhesive during the serrated interlocking encapsulation, ensuring a tight and leak-proof seal between the aluminum layers of the aluminum-plastic film. The combination of serrated interlocking encapsulation and flat encapsulation ensures the flatness and reliability of the seal. If only serrated encapsulation is used, the encapsulated appearance will have obvious grooves and unevenness, affecting the appearance. However, the battery cells with the combined serrated and flat encapsulation of this invention have a relatively flat sealed surface without obvious grooves, resulting in a good overall appearance. When the sealing area is cut, it can be seen from the cut surface that when only serrated sealing is used, the aluminum layers of the two aluminum-plastic films misalign during the serration process, such as... Figure 1 As shown, this can easily lead to packaging failure. However, this invention combines serrated and planar packaging, which not only flattens the seal and reduces its width, increasing energy density and improving packaging reliability, but also prevents the PP from being completely squeezed out. Figure 2 As shown, this improves the sealing performance of the package while maintaining a smooth appearance.
[0079] Comparing Examples 1 to 5, it can be seen that when the temperature of the serrated interlocking encapsulation in step S1 is 200°C, the encapsulation time is 6s, and the encapsulation pressure is 0.5MPa, the prepared battery cell has better performance.
[0080] Comparing Examples 1, 6, and 7, it can be seen that when the number of serrations in the serrated interlocking package is 4, the performance is better, providing good sealing without affecting the appearance of the battery cell.
[0081] Comparing Examples 1, 8, 9, and 10, it is found that when the temperature of the serrated interlocking encapsulation is set to 200°C, the encapsulation time is 6 seconds, and the encapsulation pressure is 0.5 MPa, the prepared battery cell is better, which can ensure both good encapsulation sealing and good sealing appearance.
[0082] Based on the disclosure and teachings of the foregoing specification, those skilled in the art can make changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments described above, and any obvious improvements, substitutions, or modifications made by those skilled in the art based on the present invention are within the scope of protection of the present invention. Furthermore, although some specific terms are used in this specification, these terms are only for convenience of explanation and do not constitute any limitation on the present invention.
Claims
1. A method for degassing and packaging a battery cell, characterized in that, Includes the following steps: Step S1: Puncture the air bag of the aluminum-plastic film of the battery cell after it has been charged, draw a vacuum, heat the serrated end cap, and perform serrated interlocking sealing in the secondary sealing area. Step S2: Perform planar encapsulation on the secondary encapsulation area of the aluminum-plastic film, and cut the air bag to obtain the finished battery cell.
2. The cell degassing and encapsulation method according to claim 1, characterized in that, In step S1, the temperature of the serrated interlocking encapsulation is 160–220°C, the encapsulation time is 2–8 seconds, and the encapsulation pressure is 0.2–0.6 MPa.
3. The cell degassing and encapsulation method according to claim 1, characterized in that, In step S1, the serrated mesh seal has a serration width of 0.5–2 mm, a saw depth of 0.1–0.5 mm, and a cap width of 2–10 mm.
4. The cell degassing and encapsulation method according to claim 3, characterized in that, In step S1, the serration width of the serrated interlocking seal is 0.8–1.8 mm, the saw depth is 0.2–0.5 mm, and the end cap width is 4–8 mm.
5. The cell degassing and encapsulation method according to claim 4, characterized in that, The number of serrations in the saw-shaped interlocking seal in step S1 is 2 to 5.
6. The cell degassing and encapsulation method according to claim 1, characterized in that, The vacuum level in step S1 is -80 kPa to -100 kPa.
7. The cell degassing and encapsulation method according to claim 1, characterized in that, In step S2, the planar packaging temperature is 160–220°C, the time is 3–8 seconds, and the pressure is 0.2–0.6 MPa.
8. The cell degassing and encapsulation method according to claim 1, characterized in that, In step S2, the planar packaging temperature is 180–210°C, the time is 3–8 seconds, and the pressure is 0.2–0.5 MPa.
9. A pouch cell, characterized in that, The battery cell is obtained by the degassing and encapsulation method according to any one of claims 1 to 8.
10. An electrical device, characterized in that, Includes the pouch cell as described in claim 9.
Citation Information
Patent Citations
Battery cell degassing packaging method, soft package battery cell and preparation method of soft package battery cell
CN114597500A
Method for improving aluminum plastic film packaging water resistance of soft package lithium battery and soft package lithium battery
CN116111195A