At the same time, the brittle β in β-solidified high niobium TiAl alloy is eliminated. o Phase and detailed organization method
Through medium-temperature creep forming and heat treatment technology, the problem of brittle βo phase and coarse lamellar clusters in β-solidified high-niobium TiAl alloy is solved, and the efficient refinement of the alloy and the improvement of room temperature plasticity are achieved, which is suitable for promoting its development in the aerospace field. application.
Patent Information
- Application Number
- CN202311155122.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-09-07
AI Technical Summary
There are brittle βo phases and coarse lamellar clusters in β-solidified high-niobium TiAl alloys, which lead to poor room temperature plasticity. The existing elimination methods are inefficient and the structure refinement is unstable, which affects its application in the aerospace field.
Using medium-temperature, constant-load, slow-speed creep deformation technology combined with subsequent heat treatment, the massive βo phase is broken and the coarse lamellar clusters are transformed into fine equiaxed crystals, followed by heat treatment in a specific temperature range to completely eliminate the βo phase and refine it. organize.
It effectively eliminates the βo phase, significantly refines the alloy structure, improves room temperature plasticity, reduces energy consumption and improves process control accuracy, simplifies the production process, and promotes the engineering application of the alloy.
Smart Images

Figure CN117187724B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of β-solidified high-niobium TiAl alloys, and in particular to a method for simultaneously eliminating the brittle β-solidified high-niobium TiAl alloy. o Methods of refining organization. Background Art
[0002] Under the general background of energy conservation and emission reduction, the development of lightweight alloy materials has become one of the research hotspots in the aerospace field. The density of high niobium TiAl alloy is about half of that of nickel-based high-temperature alloy, and it has higher specific strength and specific stiffness, good high-temperature oxidation resistance and creep resistance. Therefore, high niobium TiAl alloy is considered to be the next generation of ideal high-temperature structural materials that are expected to replace nickel-based high-temperature alloys in the range of 650-850°C. Compared with ordinary γ-TiAl-based alloys, the operating temperature of high niobium TiAl alloys is increased by 60-100°C, and the room temperature strength is also increased by 300-500MPa. At present, β-solidified high niobium TiAl alloys have attracted much attention due to their uniform solidification structure and good high-temperature deformation ability. However, the high content of β-stabilizing elements retains a large amount of hard and brittle β in the room temperature structure of the alloy. o Phase, β o The β phase often becomes the source of crack initiation, which greatly deteriorates the room temperature plasticity of the alloy. Therefore, it is necessary to eliminate the brittle β o Based on a large number of literature search results, the current elimination of β in high niobium TiAl alloys o Phase methods are mainly long-term heat treatment and hot isostatic pressing. Through these two methods, β o The phase energy can be partially eliminated, but some residues still remain. Therefore, it is urgent to find a more efficient method that can completely eliminate β o Phase method.
[0003] On the other hand, the main method for manufacturing β-solidified high-niobium TiAl alloys is precision casting technology, which has relatively simple processes and equipment and a high degree of alloying. However, the cast high-niobium TiAl alloys often have large lamellar cluster sizes, which is not conducive to room temperature plasticity and thus hinders the further development of this alloy. In order to break through this bottleneck, the alloy structure needs to be effectively refined. However, the existing methods all have their own shortcomings. By introducing second-phase particles (such as borides and carbides), grain nucleation can be promoted to refine the structure, but this will lead to unstable refinement effects due to the uneven distribution of the second phase. Ultrafine grains can be prepared by powder metallurgy, but impurities will inevitably be mixed in during the powder mixing process, thereby affecting the final properties of the alloy. Grains can be refined by thermomechanical processing, but extremely high deformation temperatures will cause energy waste, high requirements on equipment, and poor controllability. Therefore, it is urgent to seek a better way to effectively refine the structure of high-niobium TiAl alloys.
[0004] Based on the above analysis, in order to improve the room temperature plasticity of β-solidified high-niobium TiAl alloy and promote its further engineering application, it is necessary to eliminate the brittle β o phase, and effectively refine the alloy structure. Summary of the invention
[0005] The present invention aims to solve the technical problem of poor room temperature plasticity of β-solidified high-niobium TiAl alloy and provide a method for simultaneously eliminating the brittle β in β-solidified high-niobium TiAl alloy. o Methods of refining organization.
[0006] At the same time, the brittle β in β-solidified high niobium TiAl alloy is eliminated. o The method of refining the organization is carried out in the following steps:
[0007] 1. According to the atomic percentage composition: Al is 42% to 48%, Nb is 5% to 10%, Cr is 0.5% to 2%, V is 0.5% to 2.5% and the balance is Ti, pure Ti rods, sponge Ti particles, high-purity Al blocks, high-purity Cr particles, Al-Nb master alloy particles and Al-V master alloy particles are weighed respectively; the weighed metal raw materials are ultrasonically cleaned and then placed in a drying oven for drying;
[0008] 2. Melting: ① Place the metal raw materials processed in step 1 into a copper crucible in a water-cooled copper crucible vacuum induction shell melting furnace. The order of placing the metal raw materials is: pure Ti rods are evenly erected around the inner wall of the copper crucible, sponge Ti particles are spread on the bottom of the copper crucible, high-purity Cr particles, Al-Nb master alloy particles and Al-V master alloy particles are laid on the sponge Ti particles in turn, and high-purity Al blocks are placed on the top; then close the furnace door; ② Perform vacuum treatment: when the vacuum degree is lower than 5Pa, fill the furnace with high-purity argon gas until the pressure in the furnace is 800Pa, and then perform a second vacuum. When the vacuum degree is lower than 5Pa again, fill the furnace with high-purity argon gas until the pressure in the furnace is 800Pa; ③ Heating and melting: The heating power is controlled to be 10-35kW. When the high-purity Al block is melted, the heating power is increased to 40-60kW. When the pure Ti rod is melted and poured toward the center, the heating power is further increased to 80-90kW. When all the metal raw materials are completely melted to form an alloy melt, the heating power is maintained for 10-15min, and electromagnetic stirring is performed; ④ the heating is stopped, and the alloy melt is solidified and cooled to room temperature in the copper crucible, and the heating power is increased to 60-80kW again, maintained for 5-10min, and a secondary remelting is performed; ⑤ the alloy melt is poured into a preheated stainless steel mold; it is cooled to room temperature to obtain an alloy ingot, high-purity argon gas is filled into the furnace, the furnace door is opened, and the mold and the alloy ingot are taken out;
[0009] 3. Stress relief treatment: placing the alloy ingot obtained in step 2 into a heat treatment furnace, heating it up with the furnace, keeping it at 900-960° C. for 35-50 hours, and then cooling it to room temperature with the furnace to obtain a high niobium TiAl alloy ingot;
[0010] 4. Creep forming: cut a number of cylinders from the high niobium TiAl alloy ingot obtained in step 3, perform surface grinding, ultrasonic cleaning, and obtain cylindrical samples; place the cylindrical sample in the exact center between the upper and lower pressure heads of the electronic creep endurance tester, and fix three K-type thermocouples on the upper pressure head, the lower pressure head, and the vicinity of the cylindrical sample for real-time temperature monitoring and temperature correction; apply a preload to fix the cylindrical sample; close the insulation furnace, heat up at a rate of 17 to 25°C / min, and when the forming temperature reaches 900 to 975°C, keep it warm for 40 to 70 minutes; then, load at a rate of 120 to 200N / s to a forming load of 8000 to 12000N, maintain the load for 2 to 5 hours, control the total compressive strain to be 65% to 85%, then remove the load within 1 to 4 seconds, cool to room temperature with the furnace, and obtain a high niobium TiAl alloy round cake sample;
[0011] 5. Determine the heat treatment temperature: Use differential scanning calorimetry to analyze the high niobium TiAl alloy round cake sample obtained in step 4 and measure the α phase transformation temperature T α ;
[0012] 6. Heat treatment process: The high niobium TiAl alloy round cake sample obtained in step 4 is placed in a heat treatment furnace, and then the temperature is raised in a stepwise manner: the temperature is raised to 560-610°C at a rate of 10-16°C / min and maintained for 1-5 minutes; then the temperature is raised to the target temperature (T at a rate of 8-13°C / min). α -20)~(T α +15)℃ and keep it for 10-40min; then cool it to room temperature to obtain a high niobium TiAl alloy with fine lamellar structure.
[0013] The creep forming proposed by the present invention is carried out in a heat preservation furnace throughout the entire process, providing a constant temperature condition and avoiding the adverse effects of temperature reduction. Moreover, the creep forming is carried out at a relatively low temperature (<1000° C.), reducing energy consumption. In addition, the creep forming has a slow deformation rate, which can avoid cracking of the alloy.
[0014] The present invention proposes a method of using creep forming technology under medium temperature, constant load and slow speed conditions combined with subsequent heat treatment process to simultaneously eliminate brittle β o First, the blocky β o The phase is crushed and dispersed, and the coarse lamellar clusters are transformed into fine equiaxed crystals. Then, an appropriate heat treatment system is applied to complete the β ophase is eliminated and the fine equiaxed crystals are transformed into fine lamellar clusters.
[0015] Beneficial effects of the present invention:
[0016] The present invention ingeniously utilizes creep forming means under medium temperature, constant load and slow speed conditions to transform large-sized block β in cast β-solidified high-niobium TiAl alloy into o The phase is crushed and dispersed, and the coarse lamellar clusters are transformed into fine equiaxed crystals. This method makes up for the disadvantages of other conventional thermomechanical processing, reduces energy consumption and improves control accuracy.
[0017] The present invention performs subsequent heat treatment on the creep-formed β-solidified high-niobium TiAl alloy to control the heat treatment temperature (T α -20)~(T α +15)℃. There are two reasons for choosing this temperature range: on the one hand, within this range, β o The phase is unstable and decomposes, which can completely eliminate the β o phase; on the other hand, within this range, most of the equiaxed γ grains will be transformed into α grains, and will be transformed into lamellar structures during the subsequent cooling phase transformation process, thereby transforming the fine equiaxed crystals into fine lamellar clusters. Compared with the coarse lamellar clusters in the cast alloy, significant tissue refinement is achieved. In addition, by controlling the heat treatment time, near-lamellar or full-lamellar structures can be flexibly obtained by heat treatment within this temperature range, and these two structures show different alloy properties, each with its own advantages, which can be regulated according to actual needs. The heat treatment in the present invention is a single-step process, which greatly simplifies the process, and the cooling method is furnace cooling, which avoids cracking caused by fast cooling speed.
[0018] The present invention proposes a creep forming combined with heat treatment method which can simultaneously eliminate the brittle β in β-solidified high niobium TiAl alloy. o The operation method is simple, the controllability is strong, the production cycle is short, and the room temperature plasticity of the alloy is greatly improved. This is of great significance for promoting the engineering application of β-solidified high-niobium TiAl alloy.
[0019] The invention is used for preparing beta-solidified high-niobium TiAl alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a microstructure photograph of the high niobium TiAl alloy ingot after stress relief annealing in step 3 of Example 1; Figure 1 (a) is an optical microscope image, Figure 1 (b) is a scanning electron microscope image. Figure 1 (c) Yes Figure 1 (b) Local magnified image of the white box area;
[0021] Figure 2 This is a microstructure photograph of the high niobium TiAl alloy after creep forming in step 4 of Example 1; Figure 2 (a) is a scanning electron microscope image. Figure 2 (b) Yes Figure 2 (a) Local magnified image of the white box area;
[0022] Figure 3 This is a microstructure photograph of the high niobium TiAl alloy after heat treatment in step 6 of Example 1; Figure 3 (a) is an optical microscope image, Figure 3 (b) is a scanning electron microscope image. Figure 3 (c) Yes Figure 3 (b) Local magnified image of the white box area;
[0023] Figure 4 This is a microstructure photograph of the high niobium TiAl alloy ingot after stress relief annealing in step 3 of Example 2; Figure 4 (a) is an optical microscope image, Figure 4 (b) is a scanning electron microscope image. Figure 4 (c) Yes Figure 4 (b) Local magnified image of the white box area;
[0024] Figure 5 This is a microstructure photograph of the high niobium TiAl alloy after creep forming in step 4 of Example 2; Figure 5 (a) is a scanning electron microscope image. Figure 5 (b) Yes Figure 5 (a) Local magnified image of the white box area;
[0025] Figure 6 This is a microstructure photograph of the high niobium TiAl alloy after heat treatment in step 6 of Example 2; Figure 6 (a) is an optical microscope image, Figure 6 (b) is a scanning electron microscope image. Figure 6 (c) Yes Figure 6 (b) A local enlarged image of the white box area. DETAILED DESCRIPTION
[0026] Specific implementation method 1: This implementation method simultaneously eliminates the brittle β in the β-solidified high niobium TiAl alloy o The method of refining the organization is carried out in the following steps:
[0027] 1. According to the atomic percentage composition: Al is 42% to 48%, Nb is 5% to 10%, Cr is 0.5% to 2%, V is 0.5% to 2.5% and the balance is Ti, pure Ti rods, sponge Ti particles, high-purity Al blocks, high-purity Cr particles, Al-Nb master alloy particles and Al-V master alloy particles are weighed respectively; the weighed metal raw materials are ultrasonically cleaned and then placed in a drying oven for drying;
[0028] 2. Melting: ① Place the metal raw materials processed in step 1 into a copper crucible in a water-cooled copper crucible vacuum induction shell melting furnace. The order of placing the metal raw materials is: pure Ti rods are evenly erected around the inner wall of the copper crucible, sponge Ti particles are spread on the bottom of the copper crucible, high-purity Cr particles, Al-Nb master alloy particles and Al-V master alloy particles are laid on the sponge Ti particles in turn, and high-purity Al blocks are placed on the top; then close the furnace door; ② Perform vacuum treatment: when the vacuum degree is lower than 5Pa, fill the furnace with high-purity argon gas until the pressure in the furnace is 800Pa, and then perform a second vacuum. When the vacuum degree is lower than 5Pa again, fill the furnace with high-purity argon gas until the pressure in the furnace is 800Pa; ③ Heating and melting: The heating power is controlled to be 10-35kW. When the high-purity Al block is melted, the heating power is increased to 40-60kW. When the pure Ti rod is melted and poured toward the center, the heating power is further increased to 80-90kW. When all the metal raw materials are completely melted to form an alloy melt, the heating power is maintained for 10-15min, and electromagnetic stirring is performed; ④ the heating is stopped, and the alloy melt is solidified and cooled to room temperature in the copper crucible, and the heating power is increased to 60-80kW again, maintained for 5-10min, and a secondary remelting is performed; ⑤ the alloy melt is poured into a preheated stainless steel mold; it is cooled to room temperature to obtain an alloy ingot, high-purity argon gas is filled into the furnace, the furnace door is opened, and the mold and the alloy ingot are taken out;
[0029] 3. Stress relief treatment: placing the alloy ingot obtained in step 2 into a heat treatment furnace, heating it up with the furnace, keeping it at 900-960° C. for 35-50 hours, and then cooling it to room temperature with the furnace to obtain a high niobium TiAl alloy ingot;
[0030] 4. Creep forming: cut a number of cylinders from the high niobium TiAl alloy ingot obtained in step 3, perform surface grinding, ultrasonic cleaning, and obtain cylindrical samples; place the cylindrical sample in the exact center between the upper and lower pressure heads of the electronic creep endurance tester, and fix three K-type thermocouples on the upper pressure head, the lower pressure head, and the vicinity of the cylindrical sample for real-time temperature monitoring and temperature correction; apply a preload to fix the cylindrical sample; close the insulation furnace, heat up at a rate of 17 to 25°C / min, and when the forming temperature reaches 900 to 975°C, keep it warm for 40 to 70 minutes; then, load at a rate of 120 to 200N / s to a forming load of 8000 to 12000N, maintain the load for 2 to 5 hours, control the total compressive strain to be 65% to 85%, then remove the load within 1 to 4 seconds, cool to room temperature with the furnace, and obtain a high niobium TiAl alloy round cake sample;
[0031] 5. Determine the heat treatment temperature: Use differential scanning calorimetry to analyze the high niobium TiAl alloy round cake sample obtained in step 4 and measure the α phase transformation temperature T α ;
[0032] 6. Heat treatment process: The high niobium TiAl alloy round cake sample obtained in step 4 is placed in a heat treatment furnace, and then the temperature is raised in a stepwise manner: the temperature is raised to 560-610°C at a rate of 10-16°C / min and maintained for 1-5 minutes; then the temperature is raised to the target temperature (T at a rate of 8-13°C / min). α -20)~(T α +15)℃ and keep it for 10-40min; then cool it to room temperature to obtain a high niobium TiAl alloy with fine lamellar structure.
[0033] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: the purity of the pure Ti rod in step 1 is >99.9%, the purity of the sponge Ti particles is >99.9%, the purity of the high-purity Al block is >99.9%, the purity of the high-purity Cr particles is >99.9%, the Nb content in the Al-Nb master alloy particles is 53.7wt.%, and the V content in the Al-V master alloy particles is 56.34wt.%. The rest is the same as specific embodiment 1.
[0034] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that: 6% of the mass of Al element is added during weighing in step 1 to compensate for the volatilization of Al element during the smelting process. The rest is the same as specific implementation method 1 or 2.
[0035] Specific implementation method 4: This implementation method is different from specific implementation methods 1 to 3 in that anhydrous ethanol is used for ultrasonic cleaning in step 1. The rest is the same as specific implementation methods 1 to 3.
[0036] Specific implementation mode 5: This implementation mode is different from specific implementation modes 1 to 4 in that the material of the pressure head in step 4 is a nickel-based high-temperature alloy. The rest is the same as specific implementation modes 1 to 4.
[0037] Specific implementation method 6: This implementation method is different from specific implementation methods 1 to 5 in that the cylindrical sample size in step 4 is 6 mm × 9 mm. The rest is the same as specific implementation methods 1 to 5.
[0038] Specific implementation method 7: This implementation method is different from specific implementation methods 1 to 6 in that: in step 4, 200# to 3000# sandpaper is used for surface polishing. The rest is the same as specific implementation methods 1 to 6.
[0039] Specific embodiment 8: This embodiment is different from specific embodiments 1 to 7 in that: in step 4, the temperature fluctuation range of the forming process is controlled to be -1 to 1° C. The rest is the same as specific embodiments 1 to 7.
[0040] Specific embodiment 9: This embodiment is different from specific embodiments 1 to 8 in that the preload applied in step 4 is 300-600 N. The rest is the same as specific embodiments 1 to 8.
[0041] Specific embodiment 10: This embodiment differs from the first to ninth embodiments in that the microstructure of the high niobium TiAl alloy round cake sample obtained in step 4 is fine equiaxed crystals and has dispersed fine β o Phase, step six β in high niobium TiAl alloy o The other aspects are the same as those of the first to ninth embodiments.
[0042] The content of the present invention is not limited to the content of the above-mentioned embodiments. The combination of one or several specific embodiments can also achieve the purpose of the invention.
[0043] Embodiment 1:
[0044] The chemical composition of the β-solidifying high-niobium TiAl alloy of this embodiment is Ti-43Al-6Nb-1Cr-1.5V (atomic percentage).
[0045] At the same time, the brittle β in β-solidified high niobium TiAl alloy is eliminated. o The method for refining the structure is specifically carried out in the following steps:
[0046] 1. According to the atomic percentage composition: Al is 43%, Nb is 6%, Cr is 1%, V is 1.5% and the balance is Ti, and other inevitable impurity elements, pure Ti rods (purity>99.9%), sponge Ti particles (purity>99.9%), high-purity Al blocks (purity>99.9%), high-purity Cr particles (purity>99.9%), Al-Nb master alloy particles (Nb content is 53.7wt.%) and Al-V master alloy particles (V content is 56.34wt.%) are weighed respectively; the weighed metal raw materials are ultrasonically cleaned for 10 minutes with anhydrous ethanol, and then placed in a drying oven for drying;
[0047] 2. Melting: ① Place the metal raw materials processed in step 1 into a copper crucible in a water-cooled copper crucible vacuum induction shell melting furnace. The order of placing the metal raw materials is: pure Ti rods are evenly erected around the inner wall of the copper crucible, sponge Ti particles are spread on the bottom of the copper crucible, high-purity Cr particles, Al-Nb master alloy particles and Al-V master alloy particles are laid on the sponge Ti particles in turn, and high-purity Al blocks are placed on the top; then close the furnace door; ② Perform vacuum treatment: when the vacuum degree is lower than 5Pa, fill the furnace with high-purity argon gas until the pressure in the furnace is 800Pa, and then perform a second vacuum treatment. When the vacuum degree is lower than 5Pa again, fill the furnace with high-purity argon gas until the pressure in the furnace is 800Pa; ③ Heating and melting: Control The heating power is 30kW. When the high-purity Al block is melted, the heating power is increased to 55kW. When the pure Ti rod is melted and poured to the center, the heating power is further increased to 80kW. When all the metal raw materials are completely melted to form an alloy melt, the heating power is maintained for 12 minutes, and electromagnetic stirring is performed; ④ Stop heating, wait for the alloy melt to solidify and cool to room temperature in the copper crucible, then increase the heating power to 70kW again, maintain for 8 minutes, and perform secondary remelting; ⑤ Pour the alloy melt into the preheated stainless steel mold; cool to room temperature to obtain an alloy ingot, fill the furnace with high-purity argon gas, open the furnace door, take out the mold and the alloy ingot, and the alloy ingot is a β-solidified high-niobium TiAl alloy ingot;
[0048] 3. Stress relief treatment: The alloy ingot obtained in step 2 is placed in a heat treatment furnace, heated with the furnace, kept at 950°C for 36 hours, and then cooled to room temperature with the furnace to obtain a high niobium TiAl alloy ingot. The microstructure of the high niobium TiAl alloy ingot is a coarse lamellar cluster structure, and there are large-sized blocky β o Mutually;
[0049] 4. Creep forming: Cut a number of cylinders with a size of 6mm×9mm from the high niobium TiAl alloy ingot obtained in step 3, grind the upper and lower surfaces of the cylinders with 200#~3000# sandpaper, and use anhydrous ethanol to ultrasonically clean for 10 minutes to obtain cylindrical samples; place the cylindrical samples in the center between the upper and lower pressure heads of the RDL-50 electronic creep endurance testing machine. The pressure head material is a nickel-based high-temperature alloy. Three K-type thermocouples are respectively fixed to the upper pressure head, the lower pressure head and the area near the cylindrical sample for real-time temperature monitoring and temperature correction to control the forming. The temperature fluctuation range of the process is -1 to 1°C; a preload of 500N is applied to fix the cylindrical sample; the holding furnace is closed, the temperature is increased at a rate of 18°C / min, and when the forming temperature reaches 950°C, the temperature is kept for 60 minutes; then, the forming load is loaded to 9896N at a rate of 150N / s, and the load is maintained for 4.5 hours, and the total compression strain is controlled to be 75%, and then the load is unloaded within 3s, and the sample is cooled to room temperature with the furnace to obtain a high niobium TiAl alloy round cake sample, the microstructure of which is fine equiaxed crystals and dispersed fine β o Mutually;
[0050] 5. Determine the heat treatment temperature: Use differential scanning calorimetry to analyze the high niobium TiAl alloy round cake sample obtained in step 4 and measure the α phase transformation temperature T α 1280℃;
[0051] 6. Heat treatment process: The high niobium TiAl alloy round cake sample obtained in step 4 is placed in a heat treatment furnace, and then the temperature is raised in a stepwise manner: the temperature is raised to 600°C at a rate of 15°C / min and maintained for 4 minutes; then the temperature is raised to the target temperature of 1290°C at a rate of 12°C / min and maintained for 20 minutes; the high niobium TiAl alloy with fine lamellar structure is obtained. o The phase has been completely eliminated, completed.
[0052] Figure 1 This is a microstructure photograph of the high niobium TiAl alloy ingot after stress relief annealing in step 3 of Example 1; Figure 1 (a) is an optical microscope image, Figure 1 (b) is a scanning electron microscope image. Figure 1 (c) Yes Figure 1 (b) A local magnified image of the white box area. The as-cast Ti-43Al-6Nb-1Cr-1.5V alloy exhibits a typical near-lamellar structure, mainly composed of coarse lamellar clusters. The average lamellar cluster size is measured to be about 418.6 μm. In addition, there are a large number of white blocky β o Phase, such as Figure 1(c) Indicated by the arrow.
[0053] Figure 2 This is a microstructure photograph of the high niobium TiAl alloy after creep forming in step 4 of Example 1; Figure 2 (a) is a scanning electron microscope image. Figure 2 (b) Yes Figure 2 (a) is a partial magnified image of the white box area. Obviously, after creep forming, the coarse lamellar clusters in the cast alloy have been transformed into fine equiaxed crystals. The average size of these equiaxed crystals is about 3.25μm. In addition, it can be seen from Figure 2 (b) It was found that the large-sized blocky β o The phases have been broken up and dispersed.
[0054] Figure 3 This is a microstructure photograph of the high niobium TiAl alloy after heat treatment in step 6 of Example 1; Figure 3 (a) is an optical microscope image, Figure 3 (b) is a scanning electron microscope image. Figure 3 (c) Yes Figure 3 (b) A local magnified image of the white box area. Compared with the cast Ti-43Al-6Nb-1Cr-1.5V alloy, the size of the lamellar clusters of the alloy is significantly refined after creep forming and heat treatment. The average lamellar cluster size at this time is measured to be about 180.7μm. At the same time, there is no white blocky β in the alloy after creep forming and heat treatment. o phase, which means β o The phase has been completely eliminated.
[0055] Embodiment 2:
[0056] The present embodiment is different from the first embodiment in that the chemical composition of the β-solidified high niobium TiAl alloy is Ti-46Al-6Nb-1Cr-1.5V (atomic percentage); the total compressive strain in step 4 is controlled to be 67%; the α phase transformation temperature T in step 5 is α Step 6: Stepwise heating to finally reach the target temperature of 1310°C and maintain for 20 minutes. Other steps are the same as those in Example 1.
[0057] Figure 4 This is a microstructure photograph of the high niobium TiAl alloy ingot after stress relief annealing in step 3 of Example 2; Figure 4 (a) is an optical microscope image, Figure 4 (b) is a scanning electron microscope image. Figure 4 (c) Yes Figure 4(b) A local magnified image of the white box area. The as-cast Ti-46Al-6Nb-1Cr-1.5V alloy exhibits a typical near-lamellar structure, mainly composed of coarse lamellar clusters. The average lamellar cluster size is measured to be about 317.6 μm. In addition, there are a large number of large-sized white blocky β o Phase, such as Figure 4 (c) Indicated by the arrow.
[0058] Figure 5 This is a microstructure photograph of the high niobium TiAl alloy after creep forming in step 4 of Example 2; Figure 5 (a) is a scanning electron microscope image. Figure 5 (b) Yes Figure 5 (a) is a partial magnified image of the white box area. Obviously, after creep forming, the coarse lamellar clusters in the cast alloy have been transformed into fine equiaxed crystals, but there are also a small number of residual lamellar clusters. The average size of these equiaxed crystals is about 4.01μm. In addition, it can be seen from Figure 5 (b) It was found that the large-sized blocky β o The phase has been broken and dispersed, and the β o The phase has been significantly reduced.
[0059] Figure 6 This is a microstructure photograph of the high niobium TiAl alloy after heat treatment in step 6 of Example 2; Figure 6 (a) is an optical microscope image, Figure 6 (b) is a scanning electron microscope image. Figure 6 (c) Yes Figure 6 (b) A local magnified image of the white box area. Compared with the cast Ti-46Al-6Nb-1Cr-1.5V alloy, the size of the lamellar clusters of the alloy is significantly refined after creep forming and heat treatment. The average lamellar cluster size at this time is measured to be about 125.5μm. At the same time, there is no white blocky β in the alloy after creep forming and heat treatment. o phase, which means β o The phase has been completely eliminated.
[0060] According to the above two embodiments, the present invention successfully and completely eliminates the brittle β in the β-solidified high niobium TiAl alloy by using a composite method of creep forming combined with a single-step heat treatment. o phase, and effectively refines the size of the alloy lamellar clusters. At the same time, it is found through two examples that this composite method is suitable for both high Al content and low Al content β-solidifying high niobium TiAl alloys.
Claims
1. Simultaneously eliminate the brittle β in β-solidified high niobium TiAl alloy o A method for refining a phase structure, characterized in that The method is specifically carried out in the following steps:
1. According to the atomic percentage composition: Al is 42% to 48%, Nb is 5% to 10%, Cr is 0.5% to 2%, V is 0.5% to 2.5% and the balance is Ti, pure Ti rods, sponge Ti particles, high-purity Al blocks, high-purity Cr particles, Al-Nb master alloy particles and Al-V master alloy particles are weighed respectively; the weighed metal raw materials are ultrasonically cleaned and then placed in a drying oven for drying; 2. Melting: ① Place the metal raw materials processed in step 1 into the copper crucible in the water-cooled copper crucible vacuum induction shell melting furnace. The order of placing the metal raw materials is: pure Ti rods are evenly erected around the inner wall of the copper crucible, sponge Ti particles are spread on the bottom of the copper crucible, high-purity Cr particles, Al-Nb master alloy particles and Al-V master alloy particles are laid on the sponge Ti particles in turn, and high-purity Al blocks are placed on the top; then close the furnace door; ② Perform vacuum treatment: when the vacuum degree is lower than 5Pa, fill the furnace with high-purity argon gas until the pressure in the furnace is 800Pa, and then perform a second vacuum treatment. When the vacuum degree is lower than 5Pa again, fill the furnace with high-purity argon gas until the pressure in the furnace is 800Pa; ③ Heating and melting: control the heating power to 10~35 kW. When the high-purity Al block is melted, increase the heating power to 40~60 kW, when the pure Ti rod melts and pours toward the center, continue to increase the heating power to 80~90kW. When all the metal raw materials are completely melted to form an alloy melt, maintain the heating power for 10~15 min and perform electromagnetic stirring; ④ Stop heating, wait for the alloy melt to solidify and cool to room temperature in the copper crucible, then increase the heating power to 60~80 kW again, maintain for 5~10 min, and perform secondary remelting; ⑤ Pour the alloy melt into the preheated stainless steel mold; cool to room temperature to obtain an alloy ingot, fill the furnace with high-purity argon gas, open the furnace door, and take out the mold and the alloy ingot; 3. Stress relief treatment: placing the alloy ingot obtained in step 2 into a heat treatment furnace, heating it up with the furnace, keeping it at 900-960°C for 35-50h, and then cooling it to room temperature with the furnace to obtain a high niobium TiAl alloy ingot; 4. Creep forming: cut several cylinders from the high niobium TiAl alloy ingot obtained in step 3, perform surface grinding, ultrasonic cleaning, and obtain cylindrical samples; place the cylindrical sample in the exact center between the upper and lower pressure heads of the electronic creep endurance testing machine, and fix three K-type thermocouples on the upper pressure head, the lower pressure head, and the area near the cylindrical sample for real-time temperature monitoring and temperature correction; apply a preload to fix the cylindrical sample; turn off the insulation furnace, heat up at a rate of 17-25℃ / min, and when the forming temperature reaches 900-975℃, keep it warm for 40-70min; then, load at a rate of 120-200 N / s to a forming load of 8000-12000N, maintain the load for 2-5h, control the total compressive strain to 65%-85%, then remove the load within 1-4s, cool to room temperature with the furnace, and obtain a high niobium TiAl alloy round cake sample; 5. Determine the heat treatment temperature: Use differential scanning calorimetry to analyze the high niobium TiAl alloy round cake sample obtained in step 4 and measure the α phase transformation temperature T α ; 6. Heat treatment process: The high niobium TiAl alloy round cake sample obtained in step 4 is placed in a heat treatment furnace, and then the temperature is raised in a stepwise manner: the temperature is raised uniformly at a rate of 10-16 °C / min to 560-610 °C and maintained for 1-5 min; then the temperature is raised uniformly at a rate of 8-13 °C / min to the target temperature (T α -20℃)~(T α +15℃) and keep it for 20 min; then cool it to room temperature in the furnace to obtain a high niobium TiAl alloy with fine lamellar structure.
2. The method for simultaneously eliminating brittle β in β-solidified high niobium TiAl alloy according to claim 1. o A method for refining a phase structure, characterized in that The purity of the pure Ti rod in step 1 is >99.9%, the purity of the sponge Ti particles is >99.9%, the purity of the high-purity Al block is >99.9%, the purity of the high-purity Cr particles is >99.9%, the Nb content in the Al-Nb master alloy particles is 53.7 wt.%, and the V content in the Al-V master alloy particles is 56.34 wt.%.
3. The method for simultaneously eliminating brittle β in β-solidified high niobium TiAl alloy according to claim 1. o A method for refining a phase structure, characterized in that In step 1, 6% of the Al element mass is added during weighing to compensate for the volatilization of the Al element during the smelting process.
4. The method for simultaneously eliminating brittle β in β-solidified high niobium TiAl alloy according to claim 1. o A method for refining a phase structure, characterized in that Step 1: Ultrasonic cleaning using anhydrous ethanol.
5. The method for simultaneously eliminating brittle β in β-solidified high niobium TiAl alloy according to claim 1. o A method for refining a phase structure, characterized in that The material of the pressure head in step 4 is a nickel-based high-temperature alloy.
6. The method for simultaneously eliminating brittle β in β-solidified high niobium TiAl alloy according to claim 1. o A method for refining a phase structure, characterized in that Step 4: The size of the cylindrical sample is Ф6 mm × 9 mm.
7. The method for simultaneously eliminating brittle β in β-solidified high niobium TiAl alloy according to claim 1. o A method for refining a phase structure, characterized in that Step 4: Use 200#~3000# sandpaper to polish the surface.
8. The method for simultaneously eliminating brittle β in β-solidifying high niobium TiAl alloy according to claim 1. o A method for refining a phase structure, characterized in that Step 4: Control the temperature fluctuation range during the forming process to -1~1°C.
9. The method for simultaneously eliminating brittle β in β-solidified high niobium TiAl alloy according to claim 1. o A method for refining a phase structure, characterized in that Step 4: Apply a preload of 300~600N.
10. The method for simultaneously eliminating brittle β in β-solidified high niobium TiAl alloy according to claim 1. o A method for refining a phase structure, characterized in that The microstructure of the high niobium TiAl alloy round cake sample obtained in step 4 is fine equiaxed crystals with dispersed fine β o Phase, step six β in high niobium TiAl alloy o Phase completely eliminated.