Gas cylinder with structural health self-sensing monitoring function and preparation method and gas cylinder system
By using a laminated structure and a few-layer graphene conductive network on the gas cylinder, online self-sensing health monitoring of the pressure vessel is realized, which solves the problems of poor safety performance and difficult detection in traditional technology, and improves the strength and air tightness of the winding layer. sex.
Patent Information
- Application Number
- CN202311113250.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-31
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-08-31
AI Technical Summary
Existing pressure vessels have poor safety performance in terms of health monitoring. Traditional non-destructive testing technology is difficult to detect hidden damage online, and built-in sensors increase structural weight and installation difficulty, affecting performance.
It adopts a laminated structure of carbon fiber winding layer, glass fiber insulation layer, intelligent sensing layer and glass fiber protective layer, uses few layers of graphene and epoxy resin to form a conductive network, and combines the resistance/strain response effect to realize the in-situ and online operation of the gas cylinder. Self-aware structural health monitoring.
The strength and air tightness of the winding layer are improved, real-time structural sensing and damage monitoring of the gas cylinder are realized, the structural safety performance and gas barrier performance are significantly improved, and the preparation process is simplified.
Smart Images

Figure CN117190055B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of pressure vessels and health monitoring, and in particular to a gas cylinder with a structural health self-sensing monitoring function, a preparation method thereof, and a gas cylinder system. Background Art
[0002] In recent years, high-pressure gas cylinders, as the main components of hydrogen supply systems for hydrogen fuel cell vehicles, are developing in the direction of high pressure and light weight, which puts higher requirements on the safety of pressure vessels. Simply relying on traditional design and manufacturing technology can no longer meet the service safety requirements of pressure vessels. The development of health monitoring technology for composite pressure vessels is of great significance to avoid sudden structural damage and ensure service safety throughout its life cycle.
[0003] Some nondestructive testing technologies can detect damage and defects that may occur in composite materials structures, such as X-ray detection and infrared imaging. However, most of the above nondestructive testing methods can only be used for offline detection and it is difficult to detect damage in hidden parts.
[0004] Huang Liang et al. (Huang Liang, Jin Mingzhe, He Qi, et al. Research on X-ray digital imaging detection method for large-volume fiber-wound gas cylinders [J]. Composite Materials Science and Engineering, 2020, (03): 84-89.) For large-volume steel liner fiber-wound gas cylinders, artificial defects such as fiber grooves, fiber holes, liner holes, and liner grooves were made on the cylinders, and an X-ray digital imaging detection method was used to conduct experimental research. Figure 1 As shown in the figure, X-ray imaging is used to detect cylinder defects offline. The experimental results show that digital ray has a certain ability to detect various defects of large-volume fiber-wound cylinders. However, the use of traditional non-destructive testing technology can only perform offline, static, and passive testing, making it difficult to find problems during the use of pressure vessels and difficult to detect damage to hidden parts.
[0005] Xiao Biao et al. (Xiao Biao, Yang Bin, Hu Chaojie, et al. Health monitoring of fiber-wound pressure vessels based on embedded strain gauges [J]. Journal of High Pressure Physics, 2019, 33(04): 56-6) During the preparation of glass fiber wound metal liner composite pressure vessels, strain sensors were embedded between the metal liner and the glass fiber / epoxy resin composite layer to obtain a fiber-wound pressure vessel with in-situ monitoring function.
[0006] QING X (QING X, BEARD S, KUMAR A, et al. Advances in the development of built-in diagnostic system for filament wound composite structures [J]. Composites Science and Technology, 2006, 66 (11-12): 1694-1702.) developed a comprehensive structural health monitoring system based on piezoelectric elements. The system includes a built-in sensor network, supporting diagnostic hardware, and data processing / analysis software, such as Figure 2 Figure 1 shows a piezoelectric smart layer embedded in a composite gas cylinder. Signal acquisition results show that the pressure smart layer can effectively monitor and locate impact damage with a diameter of half an inch.
[0007] CN113776587A discloses a vehicle-mounted hydrogen storage bottle service monitoring device and method based on optical fiber sensing, which senses, demodulates and analyzes the dual deformation signals of the inner liner of the hydrogen storage bottle and the composite material structure deformation of the hydrogen storage bottle by winding an optical fiber grating with a strain sensor on the surface of the inner liner and the winding layer of the hydrogen storage bottle, and uses a hydrogenation gun to connect the optical fiber flange to sense, demodulate and analyze the dual deformation signals of the inner liner of the hydrogen storage bottle and the composite material structure deformation of the hydrogen storage bottle, so as to monitor the stress and strain of the hydrogen storage bottle in real time, such as Figure 3 As shown in the figure: 1 is a fiber grating with a sensor; 2 is the inner liner of a hydrogen storage cylinder; 3 is a composite material on the surface of the inner liner; 4 is a hydrogen storage cylinder; 5 is a characteristic QR code on the body of the hydrogen storage cylinder; 6 is a fiber grating with a sensor outlet at the valve of the hydrogen storage cylinder; 7 is a fiber optic flange interface of a hydrogen filling gun; 8 is a hydrogen filling gun; 9 is a valve of a hydrogen storage cylinder; 10 is a host computer cloud platform.
[0008] Although the above methods all achieve a certain online health monitoring effect by pre-embedding sensors inside the composite material, without exception, during the preparation process of the gas cylinder, the implantation of sensors will form large defects in the winding layer, posing a challenge to the structural safety of the gas cylinder.
[0009] In addition, these built-in sensors are relatively independent of the structure itself. The large number of sensors increases the weight of the structure and the difficulty of installation. There are also problems such as low strain tolerance, sensitivity to the service environment, and difficulty in matching the mechanical properties of the composite materials, resulting in loss of the original performance of the composite structural parts. Summary of the invention
[0010] The purpose of the present invention is to overcome the problem of poor safety performance of existing pressure vessels with online health monitoring functions, and to provide a gas cylinder with structural health self-sensing monitoring function and a preparation method and a gas cylinder system. The gas cylinder can improve the strength and airtightness of the winding layer, and utilize its resistance / strain response effect to achieve in-situ self-sensing structural health monitoring of the gas cylinder.
[0011] In order to achieve the above-mentioned object, the first aspect of the present invention provides a gas cylinder with a structural health self-sensing monitoring function, the gas cylinder comprising an inner liner, and a carbon fiber winding layer, a glass fiber insulation layer, an intelligent sensing layer and a glass fiber protective layer are sequentially stacked on the outer surface of the inner liner; wherein:
[0012] The carbon fiber winding layer contains carbon fibers and a cured resin I;
[0013] The glass fiber insulation layer contains glass fiber I and cured resin II;
[0014] The smart sensing layer contains glass fiber bundles, cured epoxy resin, and few-layer graphene dispersed in the cured epoxy resin;
[0015] The glass fiber protective layer contains glass fiber II and curing resin III.
[0016] The second aspect of the present invention provides a method for preparing the gas cylinder with the structural health self-sensing monitoring function according to the first aspect, the method comprising the following steps:
[0017] (1) Preparation of carbon fiber winding layer: Winding carbon fiber impregnated with resin I and curing agent I on the outer surface of the inner liner to obtain a prefabricated gas cylinder I;
[0018] (2) Preparation of glass fiber insulation layer: Winding glass fiber I impregnated with resin II and curing agent II around the outer surface of the prefabricated gas cylinder I to obtain a prefabricated gas cylinder II;
[0019] (3) Preparation of the smart sensing layer: coating the outer surface of the prefabricated gas cylinder II with a gel mixture containing a few-layer graphene, epoxy resin and curing agent III to form a coating layer, and then winding a glass fiber bundle on the outer surface of the coating layer to form a glass fiber bundle layer, wherein the coating and the winding are performed alternately to obtain a prefabricated gas cylinder III;
[0020] (4) Preparation of glass fiber protective layer: Winding glass fiber II impregnated with resin III and curing agent IV on the outer surface of the prefabricated gas cylinder III to obtain a prefabricated gas cylinder IV;
[0021] (5) The prefabricated gas cylinder IV is subjected to a curing treatment.
[0022] The third aspect of the present invention provides a gas cylinder system with a structural health self-sensing monitoring function, the gas cylinder system comprising a gas cylinder, an electrode sensing unit, an excitation signal control unit, a data acquisition unit and an image reconstruction unit; wherein the gas cylinder is the gas cylinder with a structural health self-sensing monitoring function as described in the first aspect.
[0023] Through the above technical solution, the present invention has the following advantages:
[0024] 1. The gas cylinder provided by the present invention comprises an inner liner, and a carbon fiber winding layer, a glass fiber insulation layer, an intelligent sensing layer and a glass fiber protective layer are sequentially stacked on the outer surface of the inner liner, wherein the intelligent sensing layer contains a glass fiber bundle, a resin matrix and a few-layer graphene dispersed in the resin matrix; while improving the strength and airtightness of the winding layer, it utilizes its resistance / strain response effect and uses the resistance tomography technology to realize in-situ, online and full-life self-sensing structural health monitoring of the gas cylinder without disassembling the gas cylinder, and realizes real-time structural perception, damage monitoring and positioning of the gas cylinder;
[0025] 2. The gas cylinder provided by the present invention has excellent mechanical properties. The two-dimensional few-layer graphene filler has a good aspect ratio, ultra-high specific surface area, rough surface and wrinkles. Adding an appropriate amount of few-layer graphene will not only not damage the original structural strength of the gas cylinder, but also can significantly improve the mechanical properties of the matrix polymer material and improve the structural safety performance of the gas cylinder;
[0026] 3. The gas cylinder provided by the present invention has good gas barrier properties. The defect-free few-layer graphene has a good barrier effect on gas. The few-layer graphene uniformly dispersed in the resin matrix can form a barrier network, increase the diffusion path length, limit the diffusion of molecules in the matrix, improve the barrier properties of the polymer, and further ensure the airtightness of the gas cylinder;
[0027] 4. The conductivity of few-layer graphene / polymer composites has increased by several orders of magnitude. Glass fiber and resin matrix are both insulators, but when the content of few-layer graphene in the polymer reaches its percolation threshold, a conductive network can be formed, causing a sudden change in the conductivity of the composite material. Using two-dimensional few-layer graphene as the conductive network carrier of electrical resistance tomography technology, its conductive network is more uniform and stable, which has more advantages in practical applications.
[0028] 5. The preparation method provided by the present invention is simple and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the double-wall single-shadow vertical transillumination test arrangement of the prior art;
[0030] Figure 2It is a schematic diagram of the embedding position of the smart interlayer in the wrapped gas cylinder of the prior art;
[0031] Figure 3 It is a connection relationship diagram of a monitoring and diagnosis evaluation cloud platform of the prior art;
[0032] Figure 4 is a schematic diagram of a gas cylinder with a structural health self-sensing monitoring function according to a specific embodiment of the present invention;
[0033] Figure 5 is a schematic diagram of a gas cylinder with a structural health self-sensing monitoring function according to a specific embodiment of the present invention;
[0034] Figure 6 It is a schematic diagram of a gas cylinder system with structural health self-sensing monitoring function according to a specific embodiment of the present invention. DETAILED DESCRIPTION
[0035] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0036] In the present invention, unless otherwise specified, the room temperature refers to 25±2°C.
[0037] The first aspect of the present invention provides a gas cylinder with a structural health self-sensing monitoring function, the gas cylinder comprising an inner liner, and a carbon fiber winding layer, a glass fiber insulation layer, an intelligent sensing layer and a glass fiber protective layer are sequentially stacked on the outer surface of the inner liner; wherein:
[0038] The carbon fiber winding layer contains carbon fibers and a cured resin I;
[0039] The glass fiber insulation layer contains glass fiber I and cured resin II;
[0040] The smart sensing layer contains glass fiber bundles, cured epoxy resin, and few-layer graphene dispersed in the cured epoxy resin;
[0041] The glass fiber protective layer contains glass fiber II and curing resin III.
[0042] According to some embodiments of the present invention, preferably, the material of the liner is metal and / or plastic; wherein the metal is selected from at least one of aluminum alloy, magnesium alloy and titanium alloy, preferably aluminum alloy; the plastic is at least one of nylon, high-density polyethylene and modified polyethylene, preferably nylon.
[0043] According to some embodiments of the present invention, preferably, the wall thickness of the inner liner is 1 mm to 10 mm, and the volume of the inner liner is 3 L to 680 L.
[0044] According to some embodiments of the present invention, the thickness of the carbon fiber winding layer can be determined according to actual needs. Preferably, the thickness of the carbon fiber winding layer is 4-18 mm.
[0045] According to some embodiments of the present invention, preferably, in the carbon fiber winding layer, the carbon fiber is a polyacrylonitrile-based carbon fiber;
[0046] Preferably, the tow size of the polyacrylonitrile-based carbon fiber is 12K to 24K.
[0047] According to some embodiments of the present invention, preferably, in the carbon fiber winding layer, the cured resin I is obtained by curing a mixture containing resin I and curing agent I.
[0048] Preferably, the resin I is selected from epoxy resins and / or vinyl resins.
[0049] Preferably, the curing agent I is selected from at least one of triethylenetetramine, tertiary amine titanate, modified polyetheramine and methyl ethyl ketone peroxide.
[0050] According to some embodiments of the present invention, preferably, the glass fiber insulation layer has a thickness of 4-10 mm.
[0051] According to some embodiments of the present invention, preferably, the glass fiber I is E-glass fiber.
[0052] According to some embodiments of the present invention, preferably, in the glass fiber insulation layer, the cured resin II is obtained by curing a mixture containing a resin II and a curing agent II.
[0053] Preferably, the resin II is selected from epoxy resins and / or vinyl resins.
[0054] Preferably, the curing agent II is selected from at least one of triethylenetetramine, tertiary amine titanate, modified polyetheramine and methyl ethyl ketone peroxide.
[0055] According to some embodiments of the present invention, preferably, the thickness of the smart sensing layer is 6 mm to 12 mm.
[0056] According to some embodiments of the present invention, preferably, the thickness of the few-layer graphene is 2-10 nm and the lateral size is 10-50 μm. Compared with spherical and tubular conductive nanomaterials such as carbon black and carbon nanotubes, sheet-like two-dimensional few-layer graphene is less likely to aggregate and entangle, and is more conducive to forming a uniform and stable conductive network.
[0057] According to some embodiments of the present invention, preferably, in the smart sensing layer, the cured epoxy resin is obtained by curing a mixture containing an epoxy resin and a curing agent III.
[0058] Preferably, the curing agent III is at least one of triethylenetetramine, tertiary amine titanate and modified polyetheramine.
[0059] According to some embodiments of the present invention, preferably, the smart sensing layer further contains a dispersant; the dispersant is selected from cetylpyridinium chloride and / or polyvinylpyrrolidone, preferably polyvinylpyrrolidone. The above preferred embodiment is conducive to further promoting the dispersion of the few-layer graphene in the cured epoxy resin, while further improving the conductivity of the smart sensing layer, and further improving the strength and airtightness of the gas cylinder.
[0060] According to some embodiments of the present invention, preferably, in the smart sensing layer, the content of the dispersant is 2-6.5 wt % of the content of the few-layer graphene.
[0061] According to some embodiments of the present invention, preferably, the glass fiber protective layer has a thickness of 2-5 mm.
[0062] According to some embodiments of the present invention, preferably, the glass fiber II is selected from E-glass fiber and / or S-glass fiber.
[0063] According to some embodiments of the present invention, preferably, in the glass fiber protective layer, the cured resin III is obtained by curing a mixture containing resin III and curing agent IV.
[0064] Preferably, the resin III is selected from epoxy resins and / or vinyl resins.
[0065] Preferably, the curing agent IV is selected from at least one of triethylenetetramine, tertiary amine titanate, modified polyetheramine and methyl ethyl ketone peroxide.
[0066] According to some embodiments of the present invention, the content of each component in the carbon fiber winding layer, the glass fiber insulation layer, the smart sensing layer and the glass fiber protective layer is calculated by the feed amount (dosage) of the raw materials.
[0067] The second aspect of the present invention provides a method for preparing the gas cylinder with the structural health self-sensing monitoring function according to the first aspect, the method comprising the following steps:
[0068] (1) Preparation of carbon fiber winding layer: Winding carbon fiber impregnated with resin I and curing agent I on the outer surface of the inner liner to obtain a prefabricated gas cylinder I;
[0069] (2) Preparation of glass fiber insulation layer: Winding glass fiber I impregnated with resin II and curing agent II around the outer surface of the prefabricated gas cylinder I to obtain a prefabricated gas cylinder II;
[0070] (3) Preparation of the smart sensing layer: coating the outer surface of the prefabricated gas cylinder II with a gel mixture containing a few-layer graphene, epoxy resin and curing agent III to form a coating layer, and then winding a glass fiber bundle on the outer surface of the coating layer to form a glass fiber bundle layer, wherein the coating and the winding are performed alternately to obtain a prefabricated gas cylinder III;
[0071] (4) Preparation of glass fiber protective layer: Winding glass fiber II impregnated with resin III and curing agent IV on the outer surface of the prefabricated gas cylinder III to obtain a prefabricated gas cylinder IV;
[0072] (5) The prefabricated gas cylinder IV is subjected to a curing treatment.
[0073] According to some embodiments of the present invention, preferably, the winding method in step (1) is circumferential winding and / or spiral winding, preferably circumferential winding and spiral winding are performed alternately, that is, circumferential winding first, then spiral winding, and then circumferential winding, and so on alternately. The angle of the circumferential winding is 85°-90°, and the angle of the spiral winding is 9°-60°.
[0074] According to some embodiments of the present invention, preferably, the number of layers of winding in step (1) is 6-30 layers.
[0075] According to some embodiments of the present invention, preferably, in step (1), the weight ratio of the carbon fiber to the resin I is 1.81-2.47:1.
[0076] According to some embodiments of the present invention, preferably, in step (1), the weight ratio of the curing agent I to the resin I is 0.03-0.2:1.
[0077] According to some embodiments of the present invention, preferably, the winding method in step (2) is spiral winding, and the angle of the spiral winding is 12°-40°.
[0078] According to some embodiments of the present invention, preferably, the number of layers of winding in step (2) is 8-20 layers.
[0079] According to some embodiments of the present invention, preferably, in step (2), the weight ratio of the glass fiber I to the resin II is 1.81-2.36:1.
[0080] According to some embodiments of the present invention, preferably, in step (2), the weight ratio of the curing agent II to the resin II is 0.03-0.2:1.
[0081] According to some embodiments of the present invention, preferably, the winding method in step (3) is spiral winding, and the angle of the spiral winding is 25°-50°.
[0082] According to some embodiments of the present invention, preferably, the diameter of the spirally wound polar hole in step (3) is larger than the diameter of the mouth of the gas cylinder.
[0083] According to some embodiments of the present invention, preferably, the glass fiber bundle layers in step (3) are 10-20 layers.
[0084] According to some embodiments of the present invention, preferably, the boundary of the coating in step (3) coincides with the position of the wound pole hole.
[0085] According to some embodiments of the present invention, preferably, in step (3), the amount of the few-layer graphene is 0.2-6wt% of the amount of the epoxy resin. The above preferred embodiment is conducive to further improving the conductivity of the smart sensing layer, and further improving the strength and airtightness of the gas cylinder.
[0086] According to some embodiments of the present invention, preferably, in step (3), the amount of the curing agent III is 10-30 wt % of the amount of the epoxy resin.
[0087] According to some embodiments of the present invention, preferably, in step (3), the method for preparing the gel mixture comprises: dispersing the few-layer graphene in the epoxy resin, and then mixing the obtained resin mixture with the curing agent III.
[0088] According to some embodiments of the present invention, preferably, in step (3), the dispersing step comprises: in the presence of an organic solvent, contacting the few-layer graphene with a dispersant for a primary ultrasonic treatment to obtain a mixture; drying the epoxy resin to remove moisture in the epoxy resin, contacting the mixture with the epoxy resin for a secondary ultrasonic treatment, and then vacuum drying the obtained dispersion to remove the organic solvent.
[0089] Preferably, the organic solvent is ethanol and / or propanol.
[0090] Preferably, the amount of the dispersant used is 2-6.5 wt % of the amount of the few-layer graphene used.
[0091] Preferably, the time of the primary ultrasonic treatment is 10-100 min.
[0092] Preferably, the drying conditions include: a drying time of 20-60 minutes and a drying temperature of 80-125°C.
[0093] Preferably, the secondary ultrasonic treatment lasts for 30 min-1.5 h.
[0094] Preferably, the vacuum drying conditions include: temperature of 60-80° C. and time of 10-120 min.
[0095] According to some embodiments of the present invention, preferably, after the coating and winding of step (3) are completed, step (3) further includes the step of extracting the electrode, including:
[0096] The obtained product is cured at room temperature for 8-36 hours. After the surface becomes sticky, the electrode group and multiple electrodes in the opposite electrode group are respectively compounded on the boundaries of the smart sensing layer at both ends of the gas cylinder through conductive silver paste to collect the boundary voltage of the smart sensing layer; preferably, the electrode is copper foil.
[0097] According to some embodiments of the present invention, preferably, in step (4), the winding method is circumferential winding and / or spiral winding, preferably circumferential winding and spiral winding are performed alternately, that is, circumferential winding first, then spiral winding, and then circumferential winding, and so on alternately. The angle of the circumferential winding is 85-90°, and the angle of the spiral winding is 12°-40°.
[0098] According to some embodiments of the present invention, preferably, the number of layers of winding in step (4) is 4-10 layers.
[0099] According to some embodiments of the present invention, preferably, the diameter of the polar hole of the spiral winding in step (4) is smaller than the diameter of the polar hole of the spiral winding in step (3). The above preferred embodiment is conducive to achieving comprehensive protection of the intelligent sensing layer by the glass fiber protective layer.
[0100] According to some embodiments of the present invention, preferably, the angle of the spiral winding in step (4) is smaller than the angle of the spiral winding in step (3). The use of the above preferred embodiment is conducive to achieving the required polar hole diameter in step (4).
[0101] According to some embodiments of the present invention, preferably, in step (4), the weight ratio of the glass fiber II to the resin III is 1.67-2.36:1.
[0102] According to some embodiments of the present invention, preferably, in step (4), the weight ratio of the curing agent IV to the resin III is 0.03-0.2:1.
[0103] According to some embodiments of the present invention, preferably, in step (5), the curing treatment conditions include: a curing temperature of 70-180° C. and a curing time of 2-10 h.
[0104] The third aspect of the present invention provides a gas cylinder system with a structural health self-sensing monitoring function, the gas cylinder system comprising a gas cylinder, an electrode sensing unit, an excitation signal control unit, a data acquisition unit and an image reconstruction unit; wherein the gas cylinder is the gas cylinder with a structural health self-sensing monitoring function as described in the first aspect.
[0105] According to some embodiments of the present invention, preferably, the electrode sensing unit comprises an electrode group and a contralateral electrode group respectively arranged at both ends of the gas cylinder;
[0106] The electrodes in the electrode group and the opposite electrode group are connected to the boundary of the smart sensing layer in the gas cylinder through conductive silver paste to collect the boundary voltage of the smart sensing layer.
[0107] According to some embodiments of the present invention, preferably, the number of electrodes in the electrode group is ≥ 8, and the electrodes are equidistantly distributed.
[0108] According to some embodiments of the present invention, preferably, the number of electrodes in the contralateral electrode group is ≥ 8, and the electrodes are equidistantly distributed.
[0109] Figure 4 It is a schematic diagram of a gas cylinder with a structural health self-sensing monitoring function according to a specific embodiment of the present invention. As can be seen from the figure, the gas cylinder includes an inner liner, and a carbon fiber winding layer, a glass fiber insulation layer, an intelligent sensing layer and a glass fiber protective layer are sequentially stacked on the outer surface of the inner liner.
[0110] In addition, an electrode group and an opposite electrode group are provided at both ends of the gas cylinder. The electrodes in the electrode group and the opposite electrode group are connected to the boundary of the smart sensing layer in the gas cylinder through conductive silver paste to collect the boundary voltage of the smart sensing layer.
[0111] The present invention will be described in detail below through examples.
[0112] In the following examples and comparative examples, unless otherwise specified, the raw materials used are commercially available.
[0113] in:
[0114] Polyacrylonitrile-based carbon fibers were purchased from Zhongfu Shenying Carbon Fiber Co., Ltd., with the models / brands being TG800-24K and TG800-12K;
[0115] Triethylenetetramine was purchased from Tianjin Dingshengxin Chemical Co., Ltd.;
[0116] Polyvinyl pyrrolidone was purchased from Chengdu Kelong Chemical Reagent Factory;
[0117] Hexadecylpyridinium chloride was purchased from Tianjin Xingfu Fine Chemical Research Institute;
[0118] Bisphenol A epoxy resin E-51 was purchased from Shanghai Xinhua Resin Factory;
[0119] The vinyl resin was 430LV vinyl resin purchased from Nanjing Jinling DSM Resins Co., Ltd.;
[0120] The methyl ethyl ketone peroxide was Butanox M50 from AkzoNobel.
[0121] In the following examples and comparative examples, the relevant parameters were measured by the following methods, wherein:
[0122] The thickness of each layer was measured by optical metallographic microscope.
[0123] Example 1
[0124] (1) Preparation of carbon fiber winding layer: Winding carbon fiber impregnated with resin I and curing agent I on the outer surface of the inner liner to obtain a prefabricated gas cylinder I; wherein:
[0125] The material of the liner is nylon; the wall thickness of the liner is 5mm and the volume is 210L;
[0126] The carbon fiber is polyacrylonitrile-based carbon fiber, and its tow size is 24K;
[0127] Resin I is bisphenol A epoxy resin E-51; curing agent I is triethylenetetramine;
[0128] The weight ratio of carbon fiber to resin I is 1.93:1;
[0129] The weight ratio of curing agent I to resin I is 0.12:1;
[0130] The winding method is to wind the circumferential winding and the spiral winding alternately, first the circumferential winding, the angle is 87° (7 layers); then the spiral winding, the angles are 10° (4 layers), 18° (4 layers), 33° (6 layers), 45° (6 layers); the total number of winding layers is 27;
[0131] (2) Preparation of glass fiber insulation layer: Winding glass fiber I impregnated with resin II and curing agent II on the outer surface of prefabricated gas cylinder I to obtain prefabricated gas cylinder II; wherein:
[0132] Glass fiber I is E-glass fiber; resin II is bisphenol A type epoxy resin E-51; curing agent II is triethylenetetramine;
[0133] The weight ratio of glass fiber I and resin II is 1.9:1;
[0134] The weight ratio of curing agent II to resin II is 0.13:1;
[0135] The winding method is spiral winding, and the spiral winding angles are 13° (3 layers), 20° (3 layers), and 35° (5 layers) respectively; the total number of winding layers is 11;
[0136] (3) Preparation of the intelligent sensing layer: a few-layer graphene is dispersed in a resin matrix, and then the obtained resin mixture is mixed with a curing agent III to obtain a gel mixture, and then the gel mixture is coated on the outer surface of the prefabricated gas cylinder II to form a coating layer, and then a glass fiber bundle is wound on the outer surface of the coating layer to form a glass fiber bundle layer, and the coating and winding are alternately performed to obtain a prefabricated gas cylinder III; wherein:
[0137] The resin matrix is bisphenol A epoxy resin E-51; the thickness of the few-layer graphene is 4nm and the lateral size is 35μm;
[0138] The amount of the few-layer graphene is 0.85wt% of the amount of the resin matrix;
[0139] The curing agent III is triethylenetetramine; the amount of curing agent III is 11wt% of the amount of the resin matrix;
[0140] The dispersing step is specifically as follows: in the presence of an organic solvent, the few-layer graphene is contacted with a dispersant for a primary ultrasonic treatment to obtain a mixture; the resin matrix is dried, the mixture is contacted with the resin matrix for a secondary ultrasonic treatment, and the obtained dispersion is vacuum dried to remove the organic solvent; wherein: the organic solvent is ethanol; the dispersant is polyvinyl pyrrolidone; the amount of the dispersant is 2.3wt% of the amount of the few-layer graphene; the time of the primary ultrasonic treatment is 30min; the drying time is 30min, and the drying temperature is 110°C; the time of the secondary ultrasonic treatment is 70min; the vacuum drying conditions are: the temperature is 80°C, and the time is 60min;
[0141] The winding method is spiral winding, and the spiral winding angle is 30 degrees; the glass fiber bundle layer is 15 layers; the diameter of the spirally wound pole hole is larger than the diameter of the bottle mouth of the gas cylinder; the coating boundary coincides with the position of the wound pole hole;
[0142] (4) Preparation of glass fiber protective layer: Winding glass fiber II impregnated with resin III and curing agent IV on the outer surface of prefabricated gas cylinder III to obtain prefabricated gas cylinder IV; wherein:
[0143] Glass fiber II is S-glass fiber; resin III is bisphenol A type epoxy resin E-51; curing agent IV is triethylenetetramine;
[0144] The weight ratio of glass fiber II to resin III is 1.82:1;
[0145] The weight ratio of curing agent IV to resin III is 0.13:1;
[0146] The winding method is to alternately perform hoop winding and spiral winding, first hoop winding at an angle of 87° (2 layers), then spiral winding at angles of 12° (2 layers) and 18° (1 layer), respectively; the total number of winding layers is 5;
[0147] The diameter of the polar hole of the spiral winding is smaller than the diameter of the polar hole of the spiral winding in step (3);
[0148] (5) curing the prefabricated gas cylinder IV to obtain a gas cylinder; wherein:
[0149] The curing conditions are as follows: curing temperature is 80°C and curing time is 8h.
[0150] In this gas cylinder, the thickness of the carbon fiber winding layer is 16.2mm; the thickness of the glass fiber insulation layer is 5.5mm; the thickness of the intelligent sensing layer is 9mm; and the thickness of the glass fiber protective layer is 2.5mm.
[0151] Example 2
[0152] The method of Example 1 is different from that of Example 1:
[0153] In step (1), the material of the inner liner is high-density polyethylene; the wall thickness of the inner liner is 7 mm, and the volume is 350 L;
[0154] The carbon fiber is polyacrylonitrile-based carbon fiber, and its tow size is 12K;
[0155] Resin I is vinyl resin; curing agent I is methyl ethyl ketone peroxide;
[0156] The weight ratio of carbon fiber to resin I is 1.81:1;
[0157] The weight ratio of curing agent I to resin I is 0.04:1;
[0158] The winding method is to wind the circumferential winding and the spiral winding alternately, first the circumferential winding, the angle is 87° (5 layers); then the spiral winding, the angles are 10° (5 layers), 16° (5 layers), 28° (5 layers), 41° (5 layers), 60° (5 layers); the total number of winding layers is 30;
[0159] In step (2): glass fiber I is E-glass fiber;
[0160] Resin II is vinyl resin; curing agent II is methyl ethyl ketone peroxide;
[0161] The weight ratio of glass fiber I and resin II is 1.9:1;
[0162] The weight ratio of curing agent II to resin II is 0.05:1;
[0163] The winding method is spiral winding, and the spiral winding angles are 12° (5 layers), 20° (5 layers), and 40° (5 layers) respectively; the total number of winding layers is 15 layers;
[0164] In step (3): the resin matrix is bisphenol A epoxy resin E-51; the thickness of the few-layer graphene is 6 nm and the lateral size is 50 μm; the amount of the few-layer graphene is 3 wt% of the amount of the resin matrix;
[0165] The curing agent III is triethylenetetramine; the amount of the curing agent III is 15wt% of the amount of the resin matrix;
[0166] The dispersing step is specifically as follows: in the presence of an organic solvent, the few-layer graphene is contacted with a dispersant for a primary ultrasonic treatment to obtain a mixture; the resin matrix is dried, the mixture is contacted with the resin matrix for a secondary ultrasonic treatment, and the obtained dispersion is vacuum dried to remove the organic solvent; wherein: the organic solvent is ethanol; the dispersant is polyvinyl pyrrolidone; the amount of the dispersant is 3wt% of the amount of the few-layer graphene; the time of the primary ultrasonic treatment is 60min; the drying time is 60min, and the drying temperature is 80°C; the time of the secondary ultrasonic treatment is 90min; the vacuum drying conditions are: the temperature is 60°C, and the time is 120min;
[0167] The winding method is spiral winding, and the spiral winding angle is 40 degrees; the glass fiber bundle layer is 17 layers; the diameter of the spirally wound pole hole is larger than the diameter of the bottle mouth of the gas cylinder; the coating boundary coincides with the position of the wound pole hole;
[0168] In step (4): glass fiber II is S-glass fiber;
[0169] Resin III is vinyl resin; curing agent IV is methyl ethyl ketone peroxide;
[0170] The weight ratio of glass fiber II and resin III is 2.3:1;
[0171] The weight ratio of curing agent IV to resin III is 0.05:1;
[0172] The winding method is to wind the circumferential winding and the spiral winding alternately, first the circumferential winding, the angle is 88° (2 layers), then the spiral winding, the angles are 17° (2 layers), 30° (2 layers) in turn; the total number of winding layers is 6;
[0173] The diameter of the polar hole of the spiral winding is smaller than the diameter of the polar hole of the spiral winding in step (3);
[0174] In step (5), the curing conditions are: curing temperature is 150°C and curing time is 5h;
[0175] The rest are the same, and a gas cylinder is obtained. In the gas cylinder, the thickness of the carbon fiber winding layer is 18 mm; the thickness of the glass fiber insulation layer is 7.5 mm; the thickness of the intelligent sensing layer is 11 mm; and the thickness of the glass fiber protective layer is 3 mm.
[0176] Example 3
[0177] The method of Example 1 is followed, except that in step (3), the amount of the few-layer graphene used is 7wt% of the amount of the resin matrix used; the rest is the same, to obtain a gas cylinder.
[0178] Example 4
[0179] The method of Example 1 is followed, except that in step (3), hexadecylpyridinium chloride is used as the dispersant; the rest is the same, to obtain a gas cylinder.
[0180] Comparative Example 1
[0181] The method of Example 1 is different in that step (3) is not performed, and in step (4), glass fiber II impregnated with resin III and curing agent IV is wound around the outer surface of prefabricated gas cylinder II, and the rest is the same, and the obtained gas cylinder does not have an intelligent sensing layer. Since the gas cylinder does not have an intelligent sensing layer, it is impossible to use electrical resistance tomography technology to achieve real-time structural perception, damage monitoring and positioning of the gas cylinder.
[0182] Comparative Example 2
[0183] The method of Example 1 is followed, except that in step (3), the few-layer graphene is replaced by carbon nanotubes; the rest is the same, to obtain a gas cylinder.
[0184] Test Example 1
[0185] The gas cylinders were prepared according to the methods of the embodiment and the comparative example. After the coating and winding of step (3) were completed, step (3) also included the step of leading out the electrodes, specifically:
[0186] The obtained product was cured at room temperature for 16 hours. After the surface became sticky, the multiple copper foil electrodes in the electrode group and the opposite electrode group were respectively compounded on the boundaries of the smart sensing layer at both ends of the gas cylinder through conductive silver paste to collect the boundary voltage of the smart sensing layer; wherein the multiple copper foil electrodes in the electrode group and the opposite electrode group were equidistantly distributed, such as Figure 5 and Figure 6 As shown; the number of electrodes in the electrode group is 8; the number of electrodes in the contralateral electrode group is 8.
[0187] The electrode sensing unit, excitation signal control unit, data acquisition unit and image reconstruction unit of the gas cylinder are connected through a computer to perform data acquisition, such as Figure 6 A set of copper foil electrodes at opposite ends of the gas cylinder is used as the injection point and output point of the excitation current signal, and a DC power supply is injected. At the same time, a precision current and voltage signal acquisition instrument is used to measure the voltage difference of each group of remaining adjacent electrode pairs, as shown in FIG. Figure 5 As shown, this process is repeated when each set of relative electrode pairs is excited in turn. The excitation current is a small current that does not damage the material itself. The voltage value changes between the electrodes caused by the structural changes of the intelligent sensing layer of the gas cylinder are measured. The collected boundary voltage value is combined with a suitable image reconstruction algorithm to reconstruct the conductivity distribution inside the gas cylinder, thereby realizing the visual monitoring of the internal structure of the gas cylinder. The specific calculation method refers to the calculation method proposed by Qu Shuxuan et al. (Qu Shuxuan, Gong Wenbin, Sun Xiaozhu, et al. Online damage monitoring of composite materials based on carbon nanotube films [J]. Acta Aeronautica Sinica, 2022, 43(01): 586-598.)
[0188] Among them, the test results of the average resistivity and average conductivity of adjacent electrode pairs (i.e., the intelligent sensing layer) are shown in Table 1:
[0189] Table 1
[0190] Test items Average resistivity Average conductivity unit KΩ·cm S / cm Example 1 0.11 <![CDATA[9.09×10 -3 ]]> Example 2 0.27 <![CDATA[3.7×10 -3 ]]> Example 3 0.41 <![CDATA[2.44×10 -3 <!-- 10 -->]]> Example 4 0.65 <![CDATA[1.54×10 -3 ]]> Comparative Example 1 - - Comparative Example 2 1.35 <![CDATA[0.74×10 -3 ]]>
[0191] Test Example 2
[0192] The gas cylinders prepared in the embodiment and the comparative example were respectively subjected to mechanical property and air tightness tests, and the results are shown in Table 2. Among them:
[0193] The test method for hydraulic bursting pressure is to conduct hydraulic bursting test at room temperature (25±2℃) according to the test method specified in GB / T 15385;
[0194] The test method for hydrogen leakage rate is as follows: Perform an airtightness test at 15±5℃ according to the vacuum chamber method specified in Appendix F of T / CATSI 02 007-2020.
[0195] Table 2
[0196]
[0197]
[0198] It can be seen from the above results that in the gas cylinder provided by the present invention, the electrical conductivity of the intelligent sensing layer is relatively high. While improving the strength and airtightness of the winding layer, it utilizes its resistance / strain response effect and, with the help of resistance tomography technology, can realize in-situ, online, and full-life self-sensing structural health monitoring of the gas cylinder without disassembling the gas cylinder, realize real-time structural perception, damage monitoring and positioning of the gas cylinder, and cooperate with the setting of other layers in the gas cylinder, so that the gas cylinder has excellent mechanical properties and good gas barrier properties.
[0199] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A gas cylinder with structural health self-sensing monitoring function, characterized in that: The gas cylinder comprises an inner liner, and a carbon fiber winding layer, a glass fiber insulation layer, an intelligent sensing layer and a glass fiber protective layer are sequentially stacked on the outer surface of the inner liner; wherein: The carbon fiber winding layer contains carbon fibers and a cured resin I; The glass fiber insulation layer contains glass fiber I and cured resin II; The smart sensing layer contains glass fiber bundles, cured epoxy resin and few-layer graphene dispersed in the cured epoxy resin; in the smart sensing layer, the cured epoxy resin is obtained by curing a mixture containing epoxy resin and curing agent III; The glass fiber protective layer contains glass fiber II and cured resin III; The amount of the few-layer graphene is 0.2-6wt% of the amount of the epoxy resin; The smart sensing layer also contains a dispersant, which is polyvinyl pyrrolidone.
2. The gas cylinder according to claim 1, wherein: The material of the liner is metal and / or plastic; the metal is selected from at least one of aluminum alloy, magnesium alloy and titanium alloy; the plastic is at least one of nylon, high-density polyethylene and modified polyethylene; And / or, the wall thickness of the inner liner is 1 mm to 10 mm, and the volume of the inner liner is 3 L to 680 L.
3. The gas cylinder according to claim 1, wherein: The thickness of the carbon fiber winding layer is 4-18 mm; And / or, in the carbon fiber winding layer, the carbon fiber is polyacrylonitrile-based carbon fiber; and the tow size of the polyacrylonitrile-based carbon fiber is 12K to 24K.
4. The gas cylinder according to any one of claims 1 to 3, wherein: In the carbon fiber winding layer, the cured resin I is obtained by curing a mixture containing resin I and curing agent I; the resin I is selected from epoxy resin and / or vinyl resin; the curing agent I is selected from at least one of triethylenetetramine, tertiary amine titanate, modified polyether amine and methyl ethyl ketone peroxide.
5. The gas cylinder according to any one of claims 1 to 3, wherein: The thickness of the glass fiber insulation layer is 4-10 mm; and / or, the glass fiber I is E-glass fiber; In the glass fiber insulation layer, the cured resin II is obtained by curing a mixture containing resin II and curing agent II; the resin II is selected from epoxy resin and / or vinyl resin; the curing agent II is selected from at least one of triethylenetetramine, tertiary amine titanate, modified polyether amine and methyl ethyl ketone peroxide.
6. The gas cylinder according to any one of claims 1 to 3, wherein: The thickness of the intelligent sensing layer is 6 mm to 12 mm; And / or, the few-layer graphene has a thickness of 2-10 nm and a lateral size of 10-50 μm.
7. The gas cylinder according to any one of claims 1 to 3, wherein: The curing agent III is at least one of triethylenetetramine, tertiary amine titanate and modified polyetheramine.
8. The gas cylinder according to any one of claims 1 to 3, wherein: The content of the dispersant is 2-6.5 wt % of the content of the few-layer graphene.
9. The gas cylinder according to any one of claims 1 to 3, wherein: The thickness of the glass fiber protective layer is 2-5 mm; and / or, the glass fiber II is selected from E-glass fiber and / or S-glass fiber; In the glass fiber protective layer, the cured resin III is obtained by curing a mixture containing resin III and curing agent IV; the resin III is selected from epoxy resin and / or vinyl resin; the curing agent IV is selected from at least one of triethylenetetramine, tertiary amine titanate, modified polyether amine and methyl ethyl ketone peroxide.
10. A method for preparing a gas cylinder with a structural health self-sensing monitoring function as claimed in any one of claims 1 to 9, characterized in that: The method comprises the following steps: (1) Preparation of carbon fiber winding layer: Winding carbon fiber impregnated with resin I and curing agent I on the outer surface of the inner liner to obtain a prefabricated gas cylinder I; (2) Preparation of glass fiber insulation layer: Winding glass fiber I impregnated with resin II and curing agent II around the outer surface of the prefabricated gas cylinder I to obtain a prefabricated gas cylinder II; (3) Preparation of the smart sensing layer: coating the outer surface of the prefabricated gas cylinder II with a gel mixture containing a few-layer graphene, epoxy resin and curing agent III to form a coating layer, and then winding a glass fiber bundle on the outer surface of the coating layer to form a glass fiber bundle layer, wherein the coating and the winding of the glass fiber bundle are performed alternately to obtain a prefabricated gas cylinder III; (4) Preparation of glass fiber protective layer: Winding glass fiber II impregnated with resin III and curing agent IV on the outer surface of the prefabricated gas cylinder III to obtain a prefabricated gas cylinder IV; (5) The prefabricated gas cylinder IV is subjected to a curing treatment.
11. The method according to claim 10, wherein: The winding method in step (1) is circumferential winding and / or spiral winding, wherein the circumferential winding angle is 85°-90°, and the spiral winding angle is 9°-60°; And / or, the number of layers of winding in step (1) is 6-30 layers; The weight ratio of the carbon fiber to the resin I is 1.81-2.47:1; The weight ratio of the curing agent I to the resin I is 0.03-0.2:
1.
12. The method according to claim 10, wherein: The winding method in step (2) is spiral winding, and the angle of the spiral winding is 12°-40°; And / or, the number of layers of winding in step (2) is 8-20 layers; The weight ratio of the glass fiber I to the resin II is 1.81-2.36:1; The weight ratio of the curing agent II to the resin II is 0.03-0.2:
1.
13. The method according to any one of claims 10 to 12, wherein: The glass fiber bundle is wound in step (3) by spiral winding, and the angle of the spiral winding is 25°-50°; the diameter of the polar hole of the spiral winding is larger than the diameter of the mouth of the gas cylinder; And / or, the glass fiber bundle layer in step (3) is 10-20 layers; And / or, the coating boundary in step (3) coincides with the position of the pole hole of the wound glass fiber bundle.
14. The method according to any one of claims 10 to 12, wherein: In step (3), the amount of the few-layer graphene is 0.2-6wt% of the amount of the epoxy resin; The amount of the curing agent III is 10-30wt% of the amount of the epoxy resin; The preparation method of the gel mixture comprises: dispersing the few-layer graphene in the epoxy resin, and then mixing the obtained resin mixture with the curing agent III.
15. The method according to any one of claims 10 to 12, wherein: In step (4), the winding method is circumferential winding and / or spiral winding, wherein the circumferential winding angle is 85°-90°, and the spiral winding angle is 12°-40°; And / or, the number of layers of winding in step (4) is 4-10 layers; The polar hole diameter of the spiral winding in step (4) is smaller than the polar hole diameter of the spiral winding in step (3); the angle of the spiral winding in step (4) is smaller than the angle of the spiral winding in step (3).
16. The method according to any one of claims 10 to 12, wherein: In step (4), the weight ratio of the glass fiber II to the resin III is 1.67-2.36:1; The weight ratio of the curing agent IV to the resin III is 0.03-0.2:1; In step (5), the curing conditions include: curing temperature of 70-180° C. and curing time of 2-10 h.
17. A gas cylinder system with structural health self-sensing monitoring function, characterized in that: The gas cylinder system includes a gas cylinder, an electrode sensing unit, an excitation signal control unit, a data acquisition unit and an image reconstruction unit; wherein the gas cylinder is a gas cylinder with a structural health self-sensing monitoring function as described in any one of claims 1-9.
18. The gas cylinder system according to claim 17, wherein: The electrode sensing unit comprises an electrode group and an opposite electrode group respectively arranged at two ends of the gas cylinder; The electrodes in the electrode group and the opposite electrode group are connected to the boundary of the smart sensing layer in the gas cylinder through conductive silver paste to collect the boundary voltage of the smart sensing layer.
19. The gas cylinder system according to claim 18, wherein: The number of electrodes in the electrode group is ≥ 8, and the electrodes are equidistantly distributed; The number of electrodes in the contralateral electrode group is ≥8, and the electrodes are equidistantly distributed.