Plasma etching technology
By using a plasma etching process involving fluorine, hydrogen, and nitrogen in semiconductor manufacturing, a nitride passivation layer is formed on the surface of a silicon layer, solving the problem of selective etching of germanium-containing layers. This achieves highly selective etching with good morphology, improving the structure and performance of the device.
Patent Information
- Application Number
- CN202280018961.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-02-09
- Filing Date
- 2022-02-02
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-02-02
AI Technical Summary
Existing technologies make it difficult to selectively etch germanium-containing layers without etching silicon layers in semiconductor manufacturing, especially when the concentration of Ge in the germanium-containing layer is low. Conventional methods result in uncontrollable etching of the silicon layer, affecting device performance and structural integrity.
A plasma etching process containing fluorine, hydrogen, and nitrogen is employed. By forming a nitride passivation layer on the silicon layer surface, the germanium-containing layer is selectively etched to form a recess, while simultaneously suppressing the etching of the silicon layer. The process is carried out using plasma tools under low-pressure and low-power conditions.
Selective etching of germanium-containing layers was achieved, improving the etching profile and silicon layer protection, and enhancing the structural integrity and performance of the device, especially maintaining high selectivity and good etching morphology under low Ge concentration conditions.
Smart Images

Figure CN117203741B_ABST
Abstract
Description
[0001] Cross-reference to related applications
[0002] This application claims the benefit of U.S. non-provisional application No. 17 / 171,742, filed February 9, 2021, which is incorporated herein by reference in its entirety. Technical Field
[0003] This disclosure generally relates to semiconductor manufacturing, and in some embodiments, to plasma etching techniques. Background Technology
[0004] The integrated circuit (IC) manufacturing industry strives to increase device density to improve speed, performance, and cost. To continue shrinking to smaller node sizes, device architectures have evolved from two-dimensional (2D) planar structures to three-dimensional (3D) vertical structures, such as transistors with nanowires or vertical orientation. Insufficient control of the conductive channel by the gate potential has fueled expectations for this change. The short-channel effect (SCE) can become too significant as gate size shrinks and becomes even more pronounced when no voltage is applied to the gate (I0). 关闭 This can increase current conduction. Changes in device architecture can allow for better electrostatic control of the gate, reducing SCE and power loss. Fabricating nanowire devices can present 3D etching challenges, where highly selective isotropic etching processes are beneficial. For example, exposed material layers may need to be etched relative to each other to create indentations in the film stack. Summary of the Invention
[0005] In some embodiments, a method for processing a semiconductor substrate includes receiving a semiconductor substrate comprising a film stack. The film stack includes a first silicon layer, a second silicon layer, and a first germanium-containing layer located between the first silicon layer and the second silicon layer. The method further includes selectively etching the first germanium-containing layer by exposing the film stack to a plasma comprising a fluorine agent, a nitrogen agent, and a hydrogen agent. The plasma etches the first germanium-containing layer, and such that a passivation layer is formed on the exposed surfaces of the first silicon layer and the second silicon layer to inhibit the etching of the first silicon layer and the second silicon layer during the exposure of the film stack to the plasma.
[0006] In some embodiments, the method for processing a semiconductor substrate includes positioning the semiconductor substrate in a plasma chamber of a plasma tool. The semiconductor substrate includes a film stack having silicon layers and germanium-containing layers arranged in an alternating stacked configuration, having at least two silicon layers and at least two germanium-containing layers. The method further includes generating a plasma comprising a fluorine agent, a nitrogen agent, and a hydrogen agent in the plasma chamber of the plasma tool. The plasma is generated by a gas comprising a fluorine-containing gas, a nitrogen-containing gas, a hydrogen-containing gas, and an inert gas. The method further includes exposing the film stack to the plasma in the plasma chamber of the plasma tool. The plasma causes a nitride passivation layer to be formed on the exposed surface of the silicon layers, and selectively etches the opposite exposed ends of the germanium-containing layers to form a recess in the germanium-containing layers relative to the opposite exposed ends of the silicon layers. The nitride passivation layer inhibits the etching of the silicon layers by the plasma.
[0007] In some embodiments, the method for processing a semiconductor substrate includes positioning the semiconductor substrate in a plasma chamber of a plasma tool. The semiconductor substrate includes a film stack having a first layer of a first material and a second layer of a second material arranged in an alternating stacked configuration. The first material is a germanium-containing material comprising a concentration of about 10% to about 50% germanium. The method further includes generating plasma for selectively etching the first layer of the first material. Generating the plasma includes introducing a gas containing fluorine, nitrogen, hydrogen, and an inert gas into the plasma chamber, and maintaining a pressure in the plasma chamber less than about 50 millitors. The method further includes exposing the film stack to plasma in the plasma chamber for a period of time. The plasma selectively etches opposite exposed ends of the first layer of the first material to form recesses in the first layer of the first material relative to opposite exposed ends of the second layer of the second material. Attached Figure Description
[0008] To gain a more complete understanding of this disclosure and its advantages, reference is made to the following description taken in conjunction with the accompanying drawings, in which:
[0009] Figure 1A-1D A cross-sectional view of an example semiconductor substrate during an example process for processing a semiconductor substrate, according to certain embodiments of this disclosure;
[0010] Figure 2 This illustrates example methods for processing a semiconductor substrate according to certain embodiments of this disclosure;
[0011] Figure 3 This illustrates example methods for processing a semiconductor substrate according to certain embodiments of this disclosure;
[0012] Figure 4 Example devices illustrating certain embodiments of this disclosure include substrates comprising alternating film stacks with recesses; and
[0013] Figure 5 A block diagram illustrating an example plasma tool according to certain embodiments of this disclosure. Detailed Implementation
[0014] There are various techniques for selectively etching one material relative to another. In some cases, the two materials are chemically different enough to allow the use of a plasma selectively etching one material without concern for etching the other. In other cases, determining the appropriate etching scheme for selective etching is more difficult because the materials may have similar chemical properties, or the available etching processes may be limited by other factors. Certain materials present more challenging selective etching challenges, where it is desirable to etch one material while barely etching the other. Conventional processes for this type of selective etching may not be able to achieve selective etching of one material relative to another, or may fail to meet process requirements such as selectivity, etching profile (e.g., local uniformity and / or surface roughness), etc.
[0015] Selective challenges can arise when forming nanowires or nanosheets to serve as channel regions in the 3D vertical structure of semiconductor devices such as gate-all-around (GAA) devices. Forming such nanowires may involve forming a film stack on a substrate layer comprising alternating layers of Si and Ge or Si-Ge (SiGe) alloys. Part of this process may include etching recesses in the film stack at opposite ends of the Ge or Ge-containing layers while minimizing etching of the silicon (Si) layers to expose the ends of the Si layers for later use as conductive devices. Conventional etching techniques may be unsatisfactory due to various challenges, including native oxide (NOL) layers and / or other residues (e.g., reactive ion etching (RIE) residues) present on the surface of the film stack.
[0016] Etching the Ge-containing layer while minimizing the etching of the Si layer can be particularly challenging when the Ge-containing layer comprises a relatively low concentration of Ge, such as less than or equal to about 30% Ge, and in a specific example, less than or equal to about 15%. This challenge may be at least in part due to the chemical composition of the Ge-containing layer (e.g., a SiGe layer), and the fact that the Si layer becomes more similar when using a Ge-containing layer with a lower Ge concentration.
[0017] Before performing plasma etching to form recesses in the film stack, some conventional techniques use wet or dry processes to remove NOL (non-nitrous oxide) residues. The film stack can be treated with dilute hydrogen fluoride (HF) acid or chemical oxide removal processes that form ammonium fluorosilicate. However, removing NOL from both the Si layer and the Ge-containing layer surface can reduce the selectivity of subsequent recess plasma etching processes (e.g., using conventional fluorine-based etching processes, as described below) in etching the Ge-containing layer with minimal to no etching of the Si layer.
[0018] Some conventional techniques expose the surfaces of both the Si layer and the Ge-containing layer (e.g., along the sidewalls of the film stack) to fluorinated chemicals (e.g., fluorine (F2), chlorine trifluoride (ClF3), bromine trifluoride (BrF3), or iodine pentafluoride (IF5)) or to fluorinated radicals generated by plasma. Such conventional plasmas can be generated by gases including carbon tetrafluoride (CF4) and argon (Ar) or by gases including nitrogen trifluoride (NF3) and nitrogen (N2). Fluorinated etchants (whether in the form of fluorinated chemicals or fluorinated radicals in plasma) can react with the Ge-containing layer faster than with the Si layer, allowing for a degree of selectivity towards Si (etching the Ge-containing layer faster than etching the Si layer). Although the Si layer is less reactive to the fluorinated etchants associated with these conventional techniques, undesirable amounts of Si layer etching still occur. For example, if the etching of the Si layer occurs at a corner of the Si layer, the etching can cause the corner to become rounded. Furthermore, at relatively low Ge concentrations in the Ge-containing layer (e.g., ≤ about 30% and ≤ about 15% in certain examples), the difference in reactivity between the Si layer and the Ge-containing layer to the fluorinated etchant can be significantly reduced, which may result in poor selectivity (e.g., less than about 20:1 (etch rate of the Ge-containing layer: etch rate of the Si layer) for 15% Ge in certain examples).
[0019] The embodiments described below provide various techniques for selective etching. For example, the embodiments can be used to selectively etch portions of a film stack (e.g., comprising Si layers and Ge-containing layers arranged in an alternating stacked configuration) of a substrate. It may be desirable to selectively etch recesses (or possibly completely remove the Ge-containing layer) in the edge portions of the Ge-containing layer to form contact stalks for the Si nanowire layer, and to provide improved selectivity for the Si layer even in cases of low Ge concentrations in the Ge-containing layer (e.g., less than about 50% Ge, less than about 30% Ge, less than about 25% Ge, and less than about 15% Ge in certain embodiments).
[0020] Some embodiments use plasma to form recesses or depressions in a film stack comprising alternating Si layers and Ge-containing layers. The plasma can be generated by a gas comprising a fluorine-containing gas, a hydrogen-containing gas, and a carrier gas (e.g., an inert gas such as Ar and He), and the plasma can include fluorine, hydrogen, and nitrogen agents. The plasma allows for the formation of a passivation layer (e.g., a nitride passivation layer, such as a silicon nitride passivation layer) on the exposed surface of the Si layers, which can serve as an etch stop layer on the exposed surface of the Si layers when an etchant (e.g., a fluorine agent) in the plasma etches the Ge-containing layers. Before exposing the substrate to the plasma, a suitable dry or wet etching process can be used to substantially remove the barrier layer (e.g., NOL) from the exposed surface of the film stack.
[0021] Figure 1A-1D The illustration shows a cross-sectional view of an example substrate 102 during an example process 100 for processing substrate 102 according to certain embodiments of the present disclosure. In some embodiments, process 100 includes plasma used to etch portions of certain layers (e.g., Ge-containing layers) of a film stack of substrate 102, while forming a protective passivation layer on exposed portions of other layers (e.g., Si layers) of the film stack, resulting in substrate 102 having a recessed film stack after performing process 100.
[0022] like Figure 1A As shown, substrate 102 is a semiconductor substrate including a film stack 104 disposed on a base layer 106. Film stack 104 includes Ge-containing layers 108 and Si layers 110 arranged in an alternating stacked configuration. Film stack 104 may have any suitable shape and include any suitable number of layers. As an example, the vertical thickness of a single Ge-containing layer 108 and Si layer 110 may each be from about 5 nm to about 25 nm, and as a specific example, may be about 10 nm or about 20 nm. Furthermore, Ge-containing layers 108 may have the same thickness or may have different thicknesses relative to each other, and Si layers 110 may have the same thickness or may have different thicknesses relative to each other. In a specific example, Ge-containing layers 108 and Si layers 110 both have substantially the same thickness.
[0023] For example, the material containing the Ge layer 108 can be pure Ge or a SiGe alloy. As a specific example, the Ge layer 108 may include an appropriate ratio (e.g., Si) for the desired etching characteristics of a given application or for the desired performance of a semiconductor device formed using process 100. 0.7 Ge 0.3 Si 0.85 Ge 0.15The SiGe alloy (mixture) is described. While this disclosure contemplates the Ge-containing layer 108 comprising any suitable concentration of Ge relative to another material (e.g., Si) (including 100% Ge), in some embodiments, the Ge-containing layer 108 comprises less than or equal to about 50% Ge, less than or equal to about 30% Ge, less than or equal to about 25% Ge, less than or equal to about 15% Ge, or less than or equal to about 10% Ge. By way of a particular example only, the Ge-containing layer 108 may comprise from about 10% to about 50% Ge relative to another material (e.g., Si). In some embodiments, all Ge-containing layers 108 comprise the same material; however, if desired, the Ge-containing layer 108 may comprise different materials.
[0024] For example, the material of Si layer 110 can be pure Si. In some embodiments, all Si layers 110 comprise the same material; however, if desired, Si layers 110 can comprise different materials. Although Si layer 110 is primarily described as pure Si in this particular example, it should be understood that in some embodiments, the material selective for etching the Ge-containing layer (e.g., Ge-containing layer 108) can comprise another suitable material, such as silicon nitride (SiN).
[0025] The substrate 106 can be any suitable material, and in one example is or includes Si. In a particular example, the film stack 104 is formed by growing alternating heteroepitaxial layers of Ge or SiGe (e.g., Ge-containing layer 108) and Si (e.g., Si layer 110) on top of the substrate 106.
[0026] An optional hard mask 112 may be included on top of the film stack 104. For example, the hard mask 112 may be used in a prior etching process to form the structure of the film stack 104. In some embodiments, the hard mask 112 is SiN (e.g., silicon nitride (Si3N4)), but may include any suitable material.
[0027] A barrier layer 114 is formed on the film stack 104 (including the hard mask 112), and in this example, on the substrate layer 106. The barrier layer 114 may be generated by a previous fabrication step (e.g., RIE) applied to the substrate 102, or by other treatments of the substrate 102 (e.g., exposure to ambient air during transfer between processing tools). As a specific example, the barrier layer 114 may include NOL, RIE residue, or both. NOL may be, for example, a thin layer of SiO2 (or other suitable material) about 1.0 nm to about 2.0 nm thick, formed on the surface of the substrate 102, such as when the substrate 102 is exposed to ambient air containing O2 and H2O. For example, the surfaces of the substrate layer 106, the Ge-containing layer 108, the Si layer 110, and the hard mask 112 may interact with ambient air, which can generate the barrier layer 114 at these surfaces. As another example, the surfaces of the substrate 106, the Ge-containing layer 108, the Si layer 110, and the hard mask 112 may include residues produced by the previous RIE steps.
[0028] The barrier layer 114 may have different etch characteristics than the layers located beneath it. Although shown as having a substantially uniform coverage over the film stack 104 (including the hard mask 112) and the substrate layer 106, the barrier layer 114 may or may not have uniform coverage.
[0029] As shown, when viewed from a cross-sectional perspective, each layer in the film stack 104 has a pair of exposed surfaces at opposite ends. That is, each Ge-containing layer 108 has an (opposite) exposed surface 116, and each Si layer 110 has an (opposite) exposed surface 118. Furthermore, in Figure 1A In the state shown, because the substrate 102 includes a barrier layer 114, the exposed surface 116 containing the Ge layer 108 and the exposed surface 118 containing the Si layer 110 also include the barrier layer 114.
[0030] like Figure 1BAs shown, barrier layer 114 is etched to remove some or all of barrier layer 114 from the exposed surface 116 containing Ge layer 108, the exposed surface 118 of Si layer 110, and the exposed surfaces of substrate layer 106 and hard mask 112. Barrier layer 114 can be removed using any suitable process, including any suitable wet or dry etching process. In some embodiments, substrate 102 is treated with dilute HF acid or chemical oxide removal processes to remove some or all of barrier layer 114. The process used to etch barrier layer 114 may or may not remove some or all of hard mask 112, but for the purposes of this example, hard mask 112 is shown as not being removed or otherwise etched. However, removing barrier layer 114 from the exposed surface 116 containing Ge layer 108 and the exposed surface 118 of Si layer 110 can reduce the selectivity of subsequent conventional fluorine-based recessed plasma etching processes that attempt to etch Ge layer 108 with minimal to no etching of Si layer 110.
[0031] like Figure 1C As shown, in the plasma step 120 of process 100, substrate 102 is exposed to plasma 122 to selectively etch the Ge-containing layer 108. For example, substrate 102 may be exposed to plasma 122 to selectively etch the exposed surface 116 of the Ge-containing layer 108 to form a recess 136 in the film stack 104, wherein opposite ends of the Ge-containing layer 108 are in an intermediate state of removal / etching relative to the adjacent Si layer 110. In some embodiments, plasma step 120 is an isotropic etching process.
[0032] Plasma step 120 can be performed in the plasma chamber 123 of the plasma tool. The plasma tool can be any suitable type, including inductively coupled plasma (ICP) tools, capacitively coupled plasma (CCP) tools, surface wave plasma (SWP) tools, etc. See below for reference. Figure 5 Describe an example plasma tool.
[0033] During the exposure of substrate 102 to plasma 122 and to facilitate selective etching of the Ge-containing layer 108, plasma 122 may cause a passivation layer 124 to be formed on the exposed surface 118 of the Si layer 110. Plasma 122 may cause the passivation layer 124 to be formed on the exposed surface 118 of the Si layer 110 by removing and replacing or otherwise modifying portions of the exposed surface 118 of the Si layer 110. In some embodiments, the passivation layer 124 may also be formed on the exposed surface of the substrate layer 106, such as when the substrate layer 106 is pure Si or silicon nitride.
[0034] During exposure of substrate 102 to plasma 122, a passivation layer 124 on the exposed surface 118 of Si layer 110 (and, in the illustrated example, on the exposed surface of base layer 106) inhibits etching of Si layer 110 (and, in the illustrated example, base layer 106). In other words, plasma 122 selectively etches the Ge-containing layer 108 at least in part due to the formation and presence of passivation layer 124 on the exposed surface 118 of Si layer 110 (and on the exposed surface of base layer 106), with passivation layer 124 acting as an etch-stopping layer on the exposed surface 118 of Si layer 110 (and on the exposed surface of base layer 106). In some embodiments, the passivation layer 124 that inhibits etching of Si layer 110 (and, in the illustrated example, base layer 106) includes passivation layers 124 that prevent some or all of the etching of Si layer 110, reduce some or all of the etching of Si layer 110, slow down some or all of the etching of Si layer 110, etc.
[0035] While the passivation layer 124 can have any suitable thickness, in some embodiments, the passivation layer 124 is relatively thin, such as 2 nm or less. The passivation layer 124 can be, for example, a single layer. In some embodiments, the passivation layer 124 is a nitride, such as silicon nitride (e.g., Si3N4).
[0036] As plasma 122 etches the Ge-containing layer 108, an additional surface 138 of the Si layer 110 is exposed. That is, due to the selective etching of the Ge-containing layer 108, an additional surface 138 of the Si layer 110 is exposed as a recess 136 or depression is formed in the film stack 104. Plasma 122 may continue to form a passivation layer 124 on the additional surface 138. The passivation layer 124 formed on the additional surface 138 may also be a nitride, such as silicon nitride (e.g., Si3N4). In other words, as the Ge-containing layer 108 is etched above, below, and / or between the Si layer 110, the passivation layer 124 is further formed on the newly exposed surface of the Si layer 110 (e.g., the additional surface 138). The passivation layer 124 on the additional surface 138 inhibits etching of the Si layer 110 at the additional surface 138, while the passivation layer 124 at the exposed surface 118 of the Si layer 110 inhibits etching of the Si layer 110 at the exposed surface 118.
[0037] Plasma 122 may include a fluorine agent 126, a hydrogen agent 128, and a nitrogen agent 130. Fluorine agent 126 may primarily act as an etchant for etching the Ge-containing layer 108 at the exposed surface 116 of the Ge-containing layer 108. Hydrogen agent 128 may act as a reducing agent, promoting the etching of the Ge-containing layer 108 at the exposed surface 116 of the Ge-containing layer 108 in the presence of fluorine agent 126. Furthermore, if applicable, depending on the gas used to generate plasma 122, hydrogen agent 128 may further decompose certain compounds of fluorine and nitrogen to produce fluorine agent 126 and nitrogen agent 130, and promote the formation of a passivation layer 124 (e.g., a nitride, such as silicon nitride) on the surface 118 of the Si layer 110 and / or the etching of the Ge-containing layer 108. Nitrogen agent 130 reacts with Si at the exposed surface 118 of the Si layer 110 to form a nitride layer (e.g., a silicon nitride layer, such as Si3N4) at the exposed surface 118. For example, atomic nitrogen (N) generated in plasma 122 can react with Si molecules at the exposed surface 118 of Si layer 110 (and the exposed surface of substrate 106) to form a passivation layer 124 (e.g., a nitride layer) on the exposed surface 118 of Si layer 110 (and on the exposed surface of substrate 106).
[0038] Although fluorine agent 126, hydrogen agent 128, and nitrogen agent 130 are primarily shown and described as separate elements, this disclosure contemplates that fluorine agent 126, hydrogen agent 128, and nitrogen agent 130 are either separate or that some or all of fluorine agent 126, hydrogen agent 128, and nitrogen agent 130 are part of one or more compounds within plasma 122. For example, plasma 122 may include one or more of NH species, HF species, NF species, or other suitable species. It should be understood that references to fluorine agent 126, hydrogen agent 128, and nitrogen agent 130 throughout this disclosure contemplate that these agents are separate elements and that they are part of one or more compounds within plasma 122.
[0039] In some embodiments, plasma 122 may be generated by a gas comprising fluorine-containing gas, hydrogen-containing gas, nitrogen-containing gas, and inert gas. The fluorine-containing gas may act as an etchant, the hydrogen-containing gas as a reducing gas, and the inert gas as a carrier gas. As several examples, the fluorine-containing gas used to generate plasma 122 may include NF3, sulfur hexafluoride (SF6), or carbon tetrafluoride (CF4). In some embodiments, such as some examples where a fluorine-containing gas excluding nitrogen is used (or even some examples where a fluorine-containing gas including nitrogen is used), nitrogen may be suitably provided in another appropriate manner, such as by introducing ammonia (NH3) (which can also be used as a hydrogen-containing gas as described below) or nitrogen (N2). Regarding hydrogen-containing gas, as several examples, the hydrogen-containing gas used to generate plasma 122 may include H2 or ammonia (NH3). As described above, hydrogen may facilitate the formation of a passivation layer 124 (e.g., a nitride, such as silicon nitride) on the surface 118 of the Si layer 110 and / or the etching of the Ge-containing layer 108.
[0040] Although shown separately, the nitrogen-containing gas can be provided alone (e.g., as nitrogen (N2)) and / or as part of a mixture with one or more other gases used to generate plasma 122 (e.g., as part of a mixture with a fluorine-containing gas and / or as part of a mixture with a hydrogen-containing gas). For example, nitrogen carrier gas (N2) and / or nitrogen agent 130 for forming passivation layer 124 (e.g., in embodiments where passivation layer 124 is a nitride layer) can be provided by other gases such as nitrogen-containing compounds for fluorine-containing gases or nitrogen-containing compounds for hydrogen-containing gases. In other words, the source of nitrogen agent 130 in plasma 122 can be an etchant gas (e.g., a fluorine-containing gas) including nitrogen (e.g., NF3), a reducing gas (e.g., a hydrogen-containing gas) including nitrogen (e.g., NH3), a carrier gas including nitrogen (e.g., N2 carrier gas), or another suitable nitrogen-containing source gas, and nitrogen agent 130 can be atomic nitrogen dissociated from the source gas.
[0041] As a specific example, the gas used to generate plasma 122 may include a suitable combination of NF3, Ar, and H2. In some embodiments, Ar may be replaced by another inert gas such as helium (He) or krypton (Kr). As a specific example, the gas / gas combination used to generate plasma 122 may include NF3 / NH3 / Ar, NF3 / NH3 / N2 / Ar, NF3 / H2 / Ar, or NF3 / H2 / Ar / N2.
[0042] Various process parameters of plasma step 120 can be optimized to promote the formation of fluorine agent 126 for efficient etching of the Ge-containing layer 108, while generating sufficient hydrogen agent 128 and nitrogen agent 130 for forming passivation layers 124 (e.g., nitride passivation layers, such as silicon nitride) at the exposed surface 118 and additional surface 138 of the Si layer 110. In an example where the gases used to generate plasma 122 include NF3 and H2, the ratio of NF3 to H2 can be a suitable consideration. The ratio of one gas to another can be measured based on their respective flow rates, such as standard cubic centimeters per minute (sccm). In some embodiments, plasma 122 includes more fluorine agent 126 than hydrogen agent 128 to ensure that the Ge-containing layer 108 is still etched and that a passivation layer similar to passivation layer 124 is unlikely to form on the exposed surface 116 of the Ge-containing layer 108 (especially in the case of low Ge concentration in the Ge-containing layer 108), and also includes sufficient nitrogen agent 130 and hydrogen agent 128 to promote the formation of passivation layer 124 quickly enough to reduce or eliminate the etching of Si layer 110 by the generally more reactive fluorine agent 126.
[0043] An appropriate ratio (or range of ratios) can depend on various factors, including other process parameters and the Ge concentration in the Si layer 110. Hydrogen (H2) can help drive the reactions occurring in the plasma chamber 123, including etching the Ge-containing layer 108 and forming a passivation layer 124 on the exposed surface 118 and additional surface 138 of the Si layer 110. Example ranges for the NF3:H2 ratio can include from NF3:H2 = about 4:about 1 to NF3:H2 = about 10:about 1, and in a particular example it can be NF3:H2 = about 5:about 1. In some embodiments, the etching rate of the Ge-containing layer 108 by the fluorine agent 126 can be reduced when the H2 low value is above about 30 sccm and the Ge concentration in the Ge-containing layer 108 is less than or equal to about 15%. It should be understood that this may or may not be the case for some embodiments, as a particular etching rate can depend on a variety of factors. For inert gases, the example range for the ratio of NF3 to Ar can include from NF3:Ar = about 1: about 2.5 to NF3:Ar = about 1: about 10.
[0044] Other process parameters used to generate plasma 122 include gas flow rate, pressure, plasma source power, plasma bias power, time, and temperature. The gas used to form plasma 122 can be provided at any suitable flow rate. In some embodiments, the etchant source gas flow rates are fluorine-containing gas (e.g., NF3) = 20-80 sccm (and 50 sccm in a specific example), H2 = 5-15 sccm (and 10 sccm in a specific example), and Ar = 500-1500 sccm (and 1000 sccm in a specific example). In these examples, the flow rates of the fluorine-containing gas are relatively moderate, the flow rates of the hydrogen-containing gas are relatively low, and the flow rates of the inert gas are relatively high.
[0045] In some embodiments, plasma step 120 may be performed at relatively low pressures (e.g., less than about 100 mTorr, less than about 50 mTorr, and in one example, about 15 mTorr to about 25 mTorr) and relatively low source power (e.g., less than about 400 W, less than about 100 W, and in one example, about 100 W of high-frequency source power and about 0 W of low-frequency bias power). The exposure time of plasma step 120 may be any suitable time. In some embodiments, the exposure time may be as short as about five seconds or less, fifteen seconds or less, twenty-five seconds or less, thirty seconds or less, or 45 seconds or less. The appropriate exposure time may depend on other parameters, such that the optimal combination of parameters is determined to achieve the desired level of selectivity (or other suitable objective). In some embodiments, plasma step 120 is performed at a temperature from about -40°C to about 20°C, and in one example, at about 0°C.
[0046] An example formulation for plasma step 120 includes the following: a pressure of about 15 mTorr to about 25 mTorr; a source power (inductively coupled plasma) of 100 W; a bias power of 0 W; a wafer processing temperature of 0 °C; and flow rates of NF3, H2 and Ar of 50 sccm, 10 sccm and 1000 sccm, respectively.
[0047] It should be understood that the specific values and ranges for all parameters described in this article are provided for illustrative purposes only.
[0048] In some embodiments, plasma step 120 is an oxygen-free plasma etching step to etch portions of certain layers of the film stack of substrate 102, resulting in a recessed or dented film stack on substrate 102 after performing process 100. It should be understood that oxygen-free does not necessarily mean the removal of all oxygen from plasma step 120, but rather reflects that oxygen-containing gas is not intentionally introduced as part of plasma step 120. Removing all oxygen from plasma chamber 123 may be difficult or impossible, and therefore some oxygen may still remain in plasma chamber 123 during plasma step 120.
[0049] Figure 1D Substrate 102 is shown after plasma step 120. Figure 1D In the illustrated state, the film stack 104 includes recesses 136 (two examples are labeled). Furthermore, due to the formation of the recesses 136, exposed ends 141 of the Si layer 110 can be formed (one example is labeled).
[0050] Figure 1D Some measurements of the resulting substrate 102 are shown, such as the exposed end spacing 142 and the etch width 144. For example, the exposed end spacing 142 indicates the remaining width of the Ge-containing layer 108 (each of these sections) by measuring each Ge-containing layer 108 from a first exposed surface 116 on a first side of the film stack 104 to an opposite second exposed surface 116 on a second side of the film stack 104. In some embodiments, the exposed end spacing 142 may be less than about 20 nm, and in one embodiment it is between about 2 nm and about 20 nm. The exposed end spacing may also refer to the spacing of the exposed ends before etching. The etch width 144 can measure how much of a particular Ge-containing layer 108 is removed from a particular end of a particular Ge-containing layer 108. In other words, the etch width 144 can measure the amount of recess 136 in the Ge-containing layer 108. In some embodiments, the etch width 144 is from about 5 nm to about 50 nm. However, depending on the given application, the exposed end spacing 142 and the etch width 144 may be outside these ranges.
[0051] Subsequent processing can then be performed on substrate 102. For example, plasma step 120 can be integrated into a process for forming the Si layer 110 into a corresponding nanowire for a channel region of a semiconductor device such as a GAA or other 3D device. In such devices, subsequent processing may include filling the recess 136 with an insulator, removing the remaining portion of the Ge-containing layer 108, providing a gate oxide around the Si layer 110, and other associated steps, all of which are provided merely for illustrative purposes. In such devices, the exposed end 141 of the Si layer 110 can be used as a conductive contact to a channel region formed in the region of the film stack 104.
[0052] Process 100 can provide one or more technical advantages. Some conventional techniques for attempting selective etching of the Ge-containing layer 108 from the Si layer 110 expose the surfaces of the Si layer 110 (e.g., exposed surface 118 and additional surface 138) and the surfaces of the Ge-containing layer 108 (e.g., exposed surface 116) (e.g., along the sidewalls of the film stack 104) to fluorinated chemicals (e.g., F2, ClF3, BrF3, or IF5) or to fluorinated radicals generated by plasma. For example, such conventional plasmas can be generated by gases including CF4 and Ar or by gases including NF3 and N2. The fluorinated etchant (whether in the form of fluorinated chemicals or fluorinated radicals in plasma) can react with the Ge-containing layer 108 faster than with the Si layer 110, which can achieve a degree of selectivity for Si (etching the Ge-containing layer 108 faster than etching the Si layer 110); however, an undesirable amount of Si layer 110 is still etched.
[0053] For example, if the etching of Si layer 110 occurs at a corner of Si layer 110, the etching of Si layer 110 can cause the corner to become rounded. Furthermore, the vertical thickness of Si layer 110 can reduce undesirable amounts, particularly towards the exposed surface 118, which is exposed to the etchant for the longest time when the exposed surface 116 of Ge layer 108 is etched inward to form a recess 136. Moreover, at relatively low Ge concentrations in Ge layer 108 (e.g., ≤ about 30% and ≤ about 15% in certain examples), the difference in reactivity between Si layer 110 and Ge layer 108 to the fluorinated etchant can be significantly reduced, which could result in poor selectivity (e.g., less than about 20:1 (etch rate of Ge layer: etch rate of Si layer)).
[0054] Furthermore, conventional fluorine-based plasmas can etch other materials on semiconductor substrates, such as silicon dioxide (SiO2), silicon nitride (Si3N4), oxides, and low-k dielectric materials, which can be undesirable. In other words, such conventional fluorine-based plasmas are not selective for SiO2, Si3N4, oxides, and low-k dielectric materials (e.g., silicon oxycarbonitride (SiOCN), silicon boron carbonitride (SiBCN), etc.).
[0055] According to an embodiment of process 100, plasma step 120 may include forming a passivation layer 124 (e.g., a nitride, such as silicon nitride) on the Si layer 110. Passivation layer 124 inhibits etching of the Si layer 110 (e.g., exposed surface 118 and additional surface 138) while the etchant of plasma 122 (e.g., fluorine agent 126) etches the Ge-containing layer 108 to form a recess 136 in the film stack 104. In some embodiments, although the concentration of Ge in the Ge-containing layer 108 may be low (e.g., less than about 50%, less than about 30%, less than about 25%, and less than about 15% in certain examples), and depending in part on the concentration of Ge in the Ge-containing layer 108, the selectivity of the Ge-containing layer 108:Si layer 110 (as measured by their respective etch rates) is greater than or equal to about 50:about 1, greater than or equal to about 70:about 1, or greater than or equal to about 100:about 1. It should be understood that the respective etch rates can be determined in any suitable manner.
[0056] Furthermore, at least in part due to the high selectivity of the plasma 122 for the Si layer 110, the film stack 104 can have an improved etch profile, which itself can be attributed at least in part to the rapid formation of the passivation layer 124 on the exposed surface 118 and the additional surface 138 of the Si layer 110. The improved etch profile can include a reduction in surface roughness along the surface 116 containing the Ge layer 108 (to the extent that the Ge layer 108 is not completely removed) after the plasma step 120, and particularly along the exposed surface 118 and the remaining surface 138 of the Si layer 110. Additionally or alternatively, the improved etch profile can include improved sharper edges and a relatively square profile at the exposed end 141 of the Si layer 110 after the plasma step 120, compared to what is possible with conventional techniques. In some embodiments, a plasma step 120, including the use of plasma 122, provides a relatively straight etch front along the surface 116 of the Ge-containing layer 108 (to the extent that the Ge-containing layer 108 is not completely removed) and good local uniformity regarding the amount of material removed from each Ge-containing layer 108 of the film stack 104.
[0057] The nitride (e.g., silicon nitride) passivation layer 124 may be insoluble in water, allowing it to act as a diffusion barrier for O2 and H2O, and thus improving the stability of the nanowires formed from the Si layer 110. In addition to its selectivity for Ge and SiGe, the plasma 122 (e.g., a plasma containing fluorine, hydrogen, and nitrogen) may also be selective for SiO2, Si3N4, oxides, and low-k dielectric materials (e.g., SiOCN, SiBCN, etc.) because, in some embodiments, oxygen is absent in the chemicals typically present for removing carbon and nitrogen bonds in these compounds (e.g., SiO2, Si3N4, oxides, and low-k dielectric materials (e.g., SiOCN, SiBCN, etc.)).
[0058] In addition, some embodiments may provide improved structures that can be used in 3D devices, such as those applicable to GAA devices, 3D NAND or other memory devices, logic devices or any other suitable type of semiconductor device.
[0059] Figure 2 An example method 200 for processing a substrate 102 according to certain embodiments of this disclosure is illustrated. Method 200 begins at step 202. At step 204, the substrate 102 is received. The substrate 102 has a film stack 104 comprising alternating Ge-containing layers 108 and Si layers 110. That is, the film stack 104 may include alternating Ge-containing layers 108 and Si layers 110 (e.g., as shown in the diagram). Figure 1A (As shown). The barrier layer 114 (e.g., NOL) may be present on the surface of the film stack 104, such as on the exposed surface 116 containing the Ge layer 108, the exposed surface 118 of the Si layer 110, and the exposed surfaces of the substrate layer 106 and the hard mask 112.
[0060] In step 206, the barrier layer 114 on the surface of the film stack 104 is etched to remove the barrier layer 114 from, for example, the exposed surface 116 containing the Ge layer 108, the exposed surface 118 of the Si layer 110, and the exposed surfaces of the substrate layer 106 and the hard mask 112. Any suitable process (e.g., wet etching or dry etching) can be used to remove the barrier layer 114.
[0061] In step 208, the Ge-containing layer 108 is selectively etched by exposing the substrate 102 (including the film stack 104) to plasma 122. Plasma 122 may include a fluorine agent 126, a hydrogen agent 128, and a nitrogen agent 130. Plasma 122 etches the Ge-containing layer 108, and such that a passivation layer 124 is formed on the exposed surface 118 of the Si layer 110 to suppress etching of the Si layer 110 during exposure of the semiconductor device 102 (including the film stack 104) to plasma 122. In some embodiments, step 208 is an isotropic etching process.
[0062] In some embodiments, plasma 122 is generated by a gas comprising NF3 gas, and fluorinating agent 126 comprises fluorine dissociated from NF3 gas. In one example, nitrogenizing agent 130 comprises nitrogen dissociated from NF3 gas. In some embodiments, plasma 122 is generated by a gas comprising H2 gas, and hydrogenating agent 128 comprises hydrogen. In some embodiments, plasma 122 is generated by a gas comprising at least one inert gas such as Ar, He, or Kr. As a specific example, plasma 122 may be generated by a combination of gases comprising: NF3, NH3, and Ar; NF3, NH3, N2, and Ar; NF3, H2, and Ar; or NF3, H2, Ar, and N2. In some embodiments, passivation layer 124 formed on exposed surface 118 of Si layer 110 comprises silicon nitride (e.g., Si3N4).
[0063] Selectively etching the Ge-containing layer 108 may include selectively etching the ends of the Ge-containing layer 108 to form a recess 136 above, below, or between the Si layer 110 in the film stack 104. As the Ge-containing layer 108 is selectively etched, additional surfaces 138 of the Si layer 110 are exposed, and plasma 122 forms a passivation layer 124 on the additional surfaces 138. In some embodiments, selectively etching the Ge-containing layer 108 includes selectively removing substantially all of the Ge-containing layer 108, thereby releasing the Si layer 110.
[0064] In some embodiments, one or more of the Ge-containing layers 108 are SiGe layers comprising about fifty percent or less of Ge. In more specific embodiments, one or more of the Ge-containing layers 108 comprise less than or equal to about fifteen percent of Ge, and the selectivity of one or more layers 108 containing fifteen percent of Ge to Si layer 110 (as measured by their respective etch rates) is greater than or equal to about 70:1.
[0065] In step 210, additional manufacturing steps are performed. (See above for reference.) Figure 1D The description of potential additional processing steps is incorporated herein by reference. For example, in some embodiments, step 208 is integrated into a process for forming the Si layer 110 into corresponding nanowires for the channel region of a semiconductor device such as a GAA device. At step 212, the method ends.
[0066] Figure 3 An example method 300 for processing a substrate 102 according to certain embodiments of this disclosure is illustrated. Method 300 begins at step 302. At step 304, the substrate 102 is positioned in the plasma chamber 123 of a plasma tool. The substrate 102 has a film stack 104 comprising alternating Ge-containing layers 108 and Si layers 110 (e.g., as shown in the image). Figure 1A (As shown).
[0067] In step 306, plasma 122 is generated in plasma chamber 123 of the plasma tool. Plasma 122 includes a fluorine agent 126, a hydrogen agent 128, and a nitrogen agent 130. Plasma 122 may be generated by a gas including a fluorine-containing gas such as NF3, SF6, or CF4. Fluorine agent 126 may include fluorine dissociated from a fluorine-containing gas. In some embodiments, nitrogen agent 130 includes nitrogen dissociated from NF3 or another suitable nitrogen-containing gas, which may or may not be part of a compound (e.g., fluorine) used to introduce the etchant. In some embodiments, plasma 122 is generated by a gas including a hydrogen-containing gas (e.g., H2 or NH3), and hydrogen agent 128 includes hydrogen dissociated from a hydrogen-containing gas.
[0068] In some embodiments, plasma 122 is generated by a gas comprising at least one inert gas such as Ar, He, or Kr. As a specific example, plasma 122 may be generated by a combination of gases including: NF3, NH3, and Ar; NF3, NH3, N2, and Ar; NF3, H2, and Ar; or NF3, H2, Ar, and N2. In some embodiments, the passivation layer 124 formed on the exposed surface 118 of the Si layer 110 comprises silicon nitride (e.g., Si3N4).
[0069] In step 308, substrate 102 (including film stack 104) is exposed to plasma 122 in plasma chamber 123. Plasma 122 causes a passivation layer 124, which may be a nitride layer, to be formed on the exposed surface 118 and additional surface 138 of Si layer 110. In some embodiments, passivation layer 124 comprises silicon nitride (Si3N4). Plasma 122 also selectively etches the exposed surface 116 (e.g., the opposite exposed end) of Ge layer 108 to form a recess 136 in Ge layer 108 relative to the exposed surface 118 (e.g., the opposite exposed end) of Si layer 110. Passivation layer 124 inhibits etching of Si layer 110 by plasma 122. In some embodiments, step 308 is an isotropic etching process.
[0070] In step 310, additional manufacturing steps are performed. (See above for reference.) Figure 2 The discussion of the potential additional processing steps described in step 210 is incorporated by reference. In step 312, the method ends.
[0071] Figure 4 Example device 400, comprising a substrate with alternating film stacks having recesses, is shown according to certain embodiments of this disclosure. At least a portion of device 400 may be formed using any of the processes and methods described herein.
[0072] Device 400 includes a substrate 402 comprising a channel material 404 (e.g., Si or SiGe) and a gate material 406 (e.g., Ge or SiGe). At some point after process 100, the channel material 404 may correspond to a Si layer 110 of the substrate 102. Device 400 may be a GAA device as shown herein, or any other device such as a FinFET. Device 400 may also include an isolation region 408. In some embodiments, the isolation region 408 is shallow trench isolation (STI).
[0073] Device 400 can be fabricated by first forming a recessed alternating film stack 410 (which may correspond to film stack 104 after process 100 and may have additional subsequent processes) and then depositing additional gate material 406 on the recessed alternating film stack 410. Specifically, device 400 can be formed by heteroepitaxial growth of alternating Si and Ge or SiGe layers, then patterned and vertically recessed to laterally expose the Si layers.
[0074] The embodiments described herein are advantageously suited as optimal solutions for 5nm, 3nm, or lower nodes. For example, the GAA device architecture is suitable for scaling beyond 7nm nodes. The GAA device architecture addresses the short-channel effect found in some FinFET architectures by wrapping the gate around the entire channel instead of just three sides. This reduces or eliminates current leakage under the gate of the FinFET, thereby reducing non-active power losses.
[0075] Figure 5 A block diagram illustrating an example plasma tool 500 according to certain embodiments of this disclosure is provided. While a particular plasma tool 500 is shown and described, any suitable type of plasma tool can be used. The plasma tool 500 can be used to perform the reference... Figure 1A-1D and Figure 2-4 Plasma step 120 is described.
[0076] Plasma tool 500 includes a plasma chamber 123 in which a semiconductor substrate (e.g., substrate 102) is treated using plasma (e.g., plasma 122). Plasma chamber 123 includes a substrate stage 502 configured to support substrate 102 during processing. In some embodiments, substrate 102 is... Figure 1B In the indicated state, for example after removing the barrier layer 114, the substrate is positioned on the substrate stage 502 for performing plasma step 120 using plasma 122. Plasma (e.g., plasma 122) is injected through the nozzle 504 of the plasma tool 500, selectively etching the material of the Ge-containing layer 108 of the film stack 104 of the substrate 102 within the plasma chamber 123 (e.g., as shown above in the reference). Figure 1A-1D (Described). Nozzle 504 may include a single mixing reaction chamber filled with a precursor gas, a mixed gas, and a carrier gas mixed to form plasma 122, and a set of outlet orifices for distributing plasma 122 toward substrate 102.
[0077] Plasma chamber 123 includes and / or is otherwise coupled to a vacuum pump 506, which is coupled to a vacuum line 508 to remove residual precursor gas from plasma chamber 123, and in some embodiments may also include and / or be otherwise coupled to a pressure system to maintain a target pressure. Plasma chamber 123 may further include mechanical tools, such as a heater 510 and a temperature sensor 512, for heating substrate 102 and controlling the temperature within plasma chamber 123 and / or substrate 102.
[0078] The plasma tool 500 includes a precursor gas line 514, a mixed gas line 516, and a carrier gas line 518 coupled to a nozzle 504. In some embodiments, the precursor gas supplied through the precursor gas line 514 may include fluorine-based precursors such as NF3 and / or SF6, the mixed gas supplied through the mixed gas line 516 may include hydrogen (e.g., H2 or NH3), and the carrier gas supplied through the carrier gas line 518 may include an inert gas such as Ar, He, or Kr.
[0079] In some embodiments, the plasma tool 500 may include a mass flow controller and sensor system for controlling gas flow rates (e.g., mass flow rates). Therefore, the plasma tool 500 may include a first flow controller 520, a second flow controller 522, a third flow controller 524, a vacuum pump 506, a heater 510, a temperature sensor 512, a voltage-current (VI) sensor 526, and substrate sensors 528, 530, 532, and 534 (528-534). A precursor gas line 514, a mixed gas line 516, and a carrier gas line 518 are coupled to and controlled by the first flow controller 520, the second flow controller 522, and the third flow controller 524, respectively.
[0080] Plasma tool 500 may include controller 536 to control aspects of plasma step 120. Controller 536 may be implemented in any suitable manner. For example, controller 536 may be a computer. As another example, controller 536 may include one or more programmable ICs programmed to provide the functions described herein. In a particular example, one or more processors (e.g., microprocessors, microcontrollers, central processing units, etc.), programmable logic devices (e.g., complex programmable logic devices, field-programmable gate arrays, etc.), and / or other programmable ICs are programmed using software or other programming instructions to implement the functions described herein with respect to controller 536. The software or other programming instructions may be stored in one or more non-transitory computer-readable media (e.g., memory storage devices, flash memory, dynamic random access memory, reprogrammable storage devices, hard disk drives, floppy disks, DVDs, CD-ROMs, etc.), and the software or other programming instructions, when executed by the programmable IC, cause the programmable IC to perform the operations described herein.
[0081] Machine components such as heater 510 and temperature sensor 512 of plasma chamber 123, as well as flow controllers 520, 522 and 524, vacuum pump 506 and other components outside plasma chamber 123 are coupled to and controlled by controller 536.
[0082] Equipment sensors measure equipment parameters, such as the temperature of the substrate stage 502, heater current, vacuum pump speed and temperature, and provide signals to ensure proper equipment operation. Various process sensors measure process parameters, such as process temperature, process pressure, plasma density, gas flow rate, and gas composition, and provide signals to ensure proper process operation. Data from the equipment and process sensors continuously provides feedback to the controller 536 throughout the plasma step 120. The controller 536 can adjust in real time to keep the equipment and process close to specifications.
[0083] The controller 536 receives data from sensors and controls the process parameters of the plasma chamber 123 based on the sensor data. The controller 536 can analyze the data collected by the sensors to determine when to modify or terminate one or more steps of the plasma step 120, and provide feedback to control the process parameters of the components of the plasma chamber 123.
[0084] The controller 536 can be connected to the VI sensor 526 and the substrate sensors 528-534 to monitor the plasma 122 when the substrate 102 is exposed to the plasma 122, thereby providing real-time status of the plasma 122 and optional composition and thickness data. This feedback data can be used by the controller 536 to continuously adjust the plasma step 120 when selectively etching the substrate 102 using the plasma 122, and, for example, to shut down the plasma step 120 when a target recess (e.g., etch width 144) is reached.
[0085] Specifically, the measurement data from the substrate sensors 528-534 and the temperature sensor 512 can be received by the controller 536, and the controller 536 generates control signals that are sent to the first flow controller 520, the second flow controller 522, the third flow controller 524, the vacuum pump 506, and the heater 510.
[0086] Controller 536 can receive measurement or metrological data acquired at multiple points on substrate 102 from substrate sensors 528-534 to measure, in situ and in real time, the thickness and composition of passivation layer 124 (formed by exposing substrate 102 to plasma 122), the exposed end spacing 142, and / or the target recess (e.g., etch width 144). For example, multiple trans-substrate sensors in a multi-substrate plasma tool can be used to monitor and adjust the thickness and composition of passivation layer 124 (formed by exposing substrate 102 to plasma 122), the exposed end spacing 142, and / or the target recess from top to bottom of substrate 102 (e.g., etch width 144). Multiple trans-substrate sensors in a single-substrate plasma tool can be used to monitor and adjust the thickness and composition of passivation layer 124 (formed by exposing substrate 102 to plasma 122), the exposed end spacing 142, and / or the target recess from the center to the edge of substrate 102 (e.g., etch width 144).
[0087] Substrate sensors 528-534 may be coupled to and / or located within plasma chamber 123 for monitoring various parameters of substrate 102, plasma tool 500, and / or plasma step 120. Substrate sensors 528-534 may include various types of sensors, including but not limited to optical sensors (such as cameras, lasers, light, reflectometers, spectrometers, ellipsometers, etc.), capacitive sensors, ultrasonic sensors, gas sensors, or other sensors capable of monitoring the state of substrate 102, plasma 122, and / or plasma tool 500. In some embodiments, one or more optical sensors may be used to measure in real time (during plasma step 120) the thickness and refractive index of the material at the surface 118 of Si layer 110 and the surface of substrate layer 106 (e.g., where passivation layer 124 is being formed), the exposed end spacing 142, and / or the etch width 144a (or another suitable measurement) of the material at these surfaces. As another example, a spectrometer can be used to measure in real time (during plasma step 120) the film thickness, exposed end spacing 142, and / or etch width 144a (or another suitable measurement) of the material at the surface 118 of the Si layer 110 and the surface of the substrate layer 106 (e.g., where the passivation layer 124 is being formed). In yet another embodiment, a residual gas analyzer (RGA) can be used to detect precursor decomposition in real time (during plasma step 120) for real-time detection of chemical reaction completion.
[0088] The controller 536 can receive user-inputted process parameters, including, for example, etch rate, conformality, profile, and deposition rate based on standard plasma etch parameters (e.g., for passivation layer 124), such as chamber pressure, room temperature, RF source power, RF bias power, RF waveform (e.g., continuous wave RF, pulsed RF, square pulse, sawtooth pulse, etc.), etch time, and the composition and flow rate of various process gases and carrier gases. Advantageously, the user can adjust the plasma 122 to meet a target local critical dimensional uniformity (LCDU).
[0089] Based on data from substrate sensors 528-534 and user-inputted process parameters, controller 536 generates control signals to temperature sensor 512 and heater 510 to regulate the heat within plasma chamber 123. When heater 510 heats plasma chamber 123, controller 536 continuously or periodically monitors temperature sensor 512 to track the temperature of plasma chamber 123, sending control signals to heater 510 to maintain the temperature within plasma chamber 123.
[0090] Once controller 536 determines, based on data provided by temperature sensor 512, that the target temperature of plasma chamber 123 has been reached, controller 536 generates control and data signals to activate first flow controller 520, second flow controller 522, and third flow controller 524. Based on user-input process parameters, controller 536 provides target flow rates for the precursor gas to first flow controller 520, for the mixed gas to second flow controller 522, and for the carrier gas to third flow controller 524. Once controller 536 determines that the corresponding flow rates have been established, controller 536 provides power to plasma chamber 123 to supply power to plasma 122 through bias and source electrodes. The power supplied to bias and source electrodes is adjustable based on measurements from VI sensor 526. First flow controller 520, second flow controller 522, and third flow controller 524 can each be a closed-loop control system connected to a flow rate sensor and an adjustable proportional valve, allowing each flow controller to continuously or periodically monitor and internally maintain the target flow rate for each gas via the flow rate sensor and adjustable proportional valve.
[0091] In some embodiments, once the controller 536 determines, based on user-input data, that the etching process time has been met, the controller 536 generates a control signal to deactivate the first flow controller 520, the second flow controller 522, and the third flow controller 524, which may be deactivated at the same or different times, depending on the circumstances.
[0092] Controller 536 may use or analyze substrate sensor data to determine when to end plasma step 120. For example, controller 536 may receive data from a residual gas analyzer to detect the end of plasma step 120. In another example, controller 536 may use elliptic polarization spectroscopy to detect the average film thickness of passivation layer 124, the exposed end 141 of Si layer 110, and / or the exposed end spacing 142 during plasma step 120, and indicate changes during plasma step 120. In yet another example, controller 536 may use elliptic polarization spectroscopy to detect the refractive index of the material at the surface 118 of Si layer 110 and the surface of substrate layer 106 (e.g., where passivation layer 124 is being formed) during plasma step 120, and indicate changes in film composition during plasma step 120. Controller 536 may automatically end plasma step 120 when the exposed end spacing 142 and / or etch width 144a (or another suitable measurement) target is achieved. In some embodiments, controller 536 may automatically adjust one or more parameters, such as the ratio of NF3 to H2 (or NH3) and / or the ratio of NF3 to Ar, for example, during plasma step 120, to achieve a desired etch profile of the film stack 104. Data from controller 536 and substrate sensors 528-534 may also be used to achieve a desired semiconductor substrate yield target. Further, data from controller 536 and substrate sensors 528-534 may be used to achieve a desired etch profile and composition of the film stack 104, as well as a desired semiconductor substrate yield, or alternatively, a combination thereof.
[0093] Although described for a specific application of forming nanowires / nanofa sheets for GAA devices, this disclosure can be used for any type of isotropic etching of Si with selective Ge-containing layers. Furthermore, while the etching performed is primarily described as forming recesses in the film stack 104 by removing portions of the Ge-containing layer 108 at opposite ends, processes 100 and 400 can be used to remove substantially all portions of the Ge-containing layer 108, which may be referred to as releasing the Si layer 110.
[0094] Although this disclosure describes particular process / method steps as occurring in a specific order, this disclosure contemplates process steps occurring in any suitable order. While this disclosure has been described with reference to illustrative embodiments, this description is not intended to be construed in a limiting sense. Various modifications and combinations of the illustrative embodiments and other embodiments of this disclosure will be apparent to those skilled in the art under the referenced description. Therefore, the appended claims are intended to cover any such modifications or embodiments.
Claims
1. A method for processing a semiconductor substrate, the method comprising: A semiconductor substrate comprising a film stack comprising a first silicon layer, a second silicon layer, and a first germanium-containing layer located between the first silicon layer and the second silicon layer is received. as well as The first germanium-containing layer is selectively etched by exposing the film stack to a plasma containing fluorine, nitrogen, and hydrogen agents. The plasma etching of the first germanium-containing layer simultaneously forms a passivation layer on the exposed surfaces of the first and second silicon layers to suppress the etching of the first and second silicon layers during plasma exposure. The passivation layer contains nitrides.
2. The method as described in claim 1, wherein, Plasma is generated from a gas containing inert gases.
3. The method as described in claim 1, wherein, The plasma is generated by a gas containing nitrogen trifluoride (NF3) gas, and the fluorine agent contains fluorine dissociated from the NF3 gas.
4. The method of claim 1, wherein, The plasma is generated by a gas containing H2 gas, and the hydrogen agent is hydrogen gas.
5. The method of claim 1, wherein, Plasma is generated by a combination of gases including: Nitrogen trifluoride (NF3), ammonia (NH3), and argon (Ar); NF3, NH3, nitrogen (N2), and Ar; NF3, hydrogen (H2), and Ar; or NF3, H2, Ar and N2.
6. The method of claim 1, wherein, The passivation layer formed on the exposed surfaces of the first and second silicon layers contains silicon nitride.
7. The method of claim 1, wherein, The first germanium-containing layer is a silicon-germanium (SiGe) layer containing fifty percent or less germanium.
8. The method of claim 7, wherein: The first germanium-containing layer contains less than or equal to 15 percent germanium; and The selectivity of the first germanium-containing layer to the first silicon layer and the second silicon layer is greater than or equal to 70:
1.
9. The method of claim 1, wherein, Selectively etching the first germanium-containing layer includes selectively etching the ends of the first germanium-containing layer to form a recess between the first silicon layer and the second silicon layer in the film stack.
10. The method of claim 1, wherein, As the first germanium-containing layer is selectively etched, additional surfaces of the first and second silicon layers are exposed, and a passivation layer is formed on these additional surfaces by plasma.
11. The method of claim 1, wherein, Selectively etching the first germanium-containing layer includes selectively removing all of the first germanium-containing layer between the first silicon layer and the second silicon layer.
12. The method of claim 1, wherein, Before selectively etching the first germanium-containing layer: A native oxide layer exists on the surface of the membrane stack; and The method further includes etching the natural oxide layer.
13. The method of claim 1, wherein: The film stack further includes a second germanium-containing layer and a third silicon layer, the second germanium-containing layer being located between the second silicon layer and the third silicon layer; and The method includes selectively etching a second germanium-containing layer by exposing the film stack to plasma, wherein the plasma forms a passivation layer on the exposed surface of a third silicon layer to suppress etching of the third silicon layer during the exposure of the film stack to plasma.
14. A method for processing a semiconductor substrate, the method comprising: A semiconductor substrate is positioned in the plasma chamber of a plasma tool. The semiconductor substrate includes a film stack comprising silicon layers and germanium-containing layers arranged in an alternating stacked manner, having at least two silicon layers and at least two germanium-containing layers. A plasma containing fluorine, nitrogen, and hydrogen is generated in the plasma chamber of a plasma tool. This plasma is produced by a gas containing fluorine, nitrogen, hydrogen, and an inert gas. In the plasma chamber of a plasma tool, a film stack is exposed to plasma, which causes a nitride passivation layer to form on the exposed surface of the silicon layer, and selectively etches the opposite exposed end of the germanium-containing layer to form a recess in the germanium-containing layer relative to the opposite exposed end of the silicon layer. The nitride passivation layer inhibits the etching of the silicon layer by the plasma.
15. The method of claim 14, wherein: Fluorine-containing gases include nitrogen trifluoride (NF3), sulfur hexafluoride (SF6), or carbon tetrafluoride (CF4); and Fluorine agents contain fluorine that dissociates from the fluorine-containing gas.
16. The method of claim 14, wherein: Hydrogen-containing gases include H2 or ammonia (NH3); and The hydrogen agent contains hydrogen dissociated from the hydrogen-containing gas.
17. The method of claim 14, wherein: Nitrogen-containing gases include N2, nitrogen trifluoride (NF3), or ammonia (NH3); and The nitrogen agent contains nitrogen dissociated from the nitrogen-containing gas.
18. The method of claim 14, wherein: Nitrogen-containing gases and fluorine-containing gases are part of the same gas mixture; or Nitrogen-containing gases and hydrogen-containing gases are part of the same gas mixture.
19. The method of claim 14, wherein: The flow rate of the inert gas is greater than the flow rate of the fluorine-containing gas; and The flow rate of the fluorine-containing gas is greater than that of the hydrogen-containing gas.
20. The method of claim 14, wherein, The inert gas is argon (Ar).
21. The method of claim 14, wherein, The gases that generate plasma include: Nitrogen trifluoride (NF3), ammonia (NH3), and argon (Ar); NF3, NH3, nitrogen (N2), and Ar; NF3, hydrogen (H2), and Ar; or NF3, H2, Ar and N2.
22. The method of claim 14, wherein, The nitride passivation layer formed on the exposed surface of the silicon layer contains silicon nitride.
23. A method for processing a semiconductor substrate, the method comprising: A semiconductor substrate is positioned in the plasma chamber of a plasma tool. The semiconductor substrate includes a film stack comprising a first layer of a first material and a second layer of a second material arranged in an alternating stacked configuration. The first material is a germanium-containing material comprising a concentration of 10% to 50% germanium, and the second material comprises silicon. Generating plasma for selectively etching a first layer of a first material, the plasma generation includes introducing a gas comprising fluorine, nitrogen, hydrogen, and an inert gas into a plasma chamber, and maintaining the pressure in the plasma chamber at less than 50 millitors; and The membrane stack is exposed to plasma in a plasma chamber for a period of time, and the plasma causes a nitride passivation layer to form on the exposed surface of the second layer of the second material, and selectively etches the opposite exposed end of the first layer of the first material to form a recess in the first layer of the first material relative to the opposite exposed end of the second layer of the second material.
24. A method for processing a semiconductor substrate, the method comprising: A semiconductor substrate comprising a film stack comprising a first silicon layer, a second silicon layer, and a first germanium-containing layer located between the first silicon layer and the second silicon layer is received. as well as The first germanium-containing layer is selectively etched by exposing the film stack to a plasma containing fluorine, nitrogen, and hydrogen agents. The plasma etching of the first germanium-containing layer simultaneously forms a passivation layer on the exposed surfaces of the first and second silicon layers to suppress the etching of the first and second silicon layers during the exposure of the film stack to the plasma. The gas used to generate the plasma is oxygen-free, and the passivation layer contains nitrides.
Citation Information
Patent Citations
Substrate processing method and storage medium
CN110476225A
Isotropic silicon and silicon-germanium etching with tunable selectivity