Epoxy type acrylate rubber with low brittle temperature and preparation method thereof
By adding low brittleness temperature functional monomers to acrylic rubber and conducting intermittent polymerization, the problem of insufficient brittleness temperature of existing rubber at low temperatures is solved, its low temperature resistance is significantly improved, and its application range is expanded.
Patent Information
- Application Number
- CN202311346865.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-18
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-10-18
AI Technical Summary
Existing acrylic rubber has insufficient brittleness temperature under low temperature conditions, making it difficult to meet the increasing demand for low temperature resistance, especially in fields where rubber and plastics are used together.
Use functional monomer raw materials with low brittleness temperature to increase the low-temperature resistance of rubber through intermittent polymerization, including the use of monomers such as ethoxyethyl acrylate, 2-ethylhexyl acrylate, and n-hexyl methacrylate. It combines epoxy-type cure point monomers and base acrylate monomers, emulsifies and polymerizes them to form a rubber with improved brittleness temperature.
The low-temperature resistance of acrylic rubber is significantly improved, allowing it to maintain toughness at lower temperatures, expanding its application fields and meeting the demand for use scenarios with higher low-temperature resistance.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of acrylic rubber manufacturing, and in particular to an epoxy acrylic rubber with a low brittle temperature and a manufacturing method thereof. Background Art
[0002] Acrylic rubber (ACM) is a type of elastic material made by copolymerizing acrylic esters with monomers that can provide cross-linking reactive groups. Its main chain is a saturated structure, so it has the properties of heat resistance, UV radiation resistance and ozone resistance; its side chain contains polar ester groups, so it also has excellent oil resistance. The main use of acrylic rubber is to make heat-resistant and oil-resistant seals and oil pipes, etc., mainly used in automobiles, motorcycles, petroleum, chemicals, machinery, power transformers and other fields.
[0003] A new development direction for the use of ACM in the future is to use rubber and plastic together to manufacture "rubber-plastic alloy", combining some advantages of rubber with plastic to increase the toughness of plastic, improve some defects and deficiencies in the performance of plastic, and create a "new material" with better suitability for use.
[0004] The physical and mechanical properties of acrylic rubber are affected by many factors, including: the structure of the rubber (the raw material ratio of the polymer), the molecular weight of the rubber, the rubber compounding processing technology, etc.
[0005] There are different types of acrylic rubber. According to the type of vulcanization point monomer, the commonly used ones are: active chlorine type, carboxylic acid type, epoxy type, double / multiple cross-linking point type, etc. According to the different temperature resistance grades of the rubber, it can be divided into: standard type, cold-resistant type, cold-resistant improved type, heat-resistant improved type, etc.
[0006] Different types of acrylic rubbers have different compounding and processing technologies. Different types of acrylic rubbers have different mechanical properties, advantages and disadvantages, and have different suitable application fields.
[0007] Epoxy rubber can be used in the field of ordinary heat-resistant and oil-resistant seals, and because it does not contain "chlorine" in its rubber structure, it can also be used in fields that are contraindicated with chlorine (such as the electronics field). In addition, because the epoxy rubber structure contains epoxy groups, it is convenient to carry out "grafting reaction", which creates favorable conditions for material modification and subsequent processing, and is more conducive to the manufacture of "rubber-plastic alloy", so it has good application prospects.
[0008] Acrylic rubber is resistant to high temperatures and oils. It can be used for a long time in hot oil at 150°C and can withstand temperatures up to 200°C for a short time (about 10 hours).
[0009] The low temperature resistance of existing acrylic rubber is not very good. The brittle temperature of standard rubber is about -10 to -15°C, the cold-resistant type is about -20°C, the cold-resistant improved type is about -30°C, and the super cold-resistant type is about -35 to -40°C.
[0010] With the development of science and technology, the requirements for the low-temperature resistance of rubber are gradually increased in some use processes. Especially in some fields where rubber and plastic are used together, there are higher requirements for the low-temperature resistance of rubber, which are difficult to meet with existing varieties. In order to make the application field of epoxy acrylate rubber wider and meet the needs of more usage scenarios, the present invention proposes an epoxy acrylate rubber with a low brittle temperature and a method for manufacturing the same. Summary of the invention
[0011] In view of the deficiencies of the prior art, the object of the present invention is to provide an epoxy-type acrylate rubber with a low brittle temperature and a method for preparing the same.
[0012] In order to achieve the above object, the present invention adopts the following technical solutions:
[0013] The low brittle temperature epoxy acrylate rubber described in the technical solution includes, by weight, 5 parts of epoxy vulcanization point monomer raw materials, 75-95 parts of low brittle temperature functional monomer raw materials, 3 parts of emulsifier and 250 parts of deionized water.
[0014] Preferably, the above technical solution further comprises at most 20 parts of basic acrylic ester monomer raw materials.
[0015] In the above technical scheme, preferably, the epoxy type vulcanization point monomer raw material includes at least one of glycidyl acrylate, glycidyl methacrylate and glycidyl acrylate; the functional monomer raw material with low brittle temperature includes at least one of ethoxyethyl acrylate, 2-ethylhexyl acrylate, n-decyl methacrylate, n-dodecyl methacrylate and cinnamyl methacrylate.
[0016] In the above technical solution, preferably, the basic acrylic ester monomer raw material includes at least one of ethyl acrylate and methoxyethyl acrylate.
[0017] In the above technical solution, preferably, the emulsifier is sodium lauryl sulfate.
[0018] The method for producing a low brittle temperature epoxy acrylate rubber described in the technical solution comprises the following steps:
[0019] S1. The rubber raw material component is added to the mixing tank, stirred and mixed evenly to prepare a mixed monomer raw material;
[0020] S2. Deionized water and an emulsifier are added to the reactor and stirred to prepare an emulsion;
[0021] S3. Nitrogen is introduced into the reactor to replace the air;
[0022] S4. One-third of the mixed monomer raw material was added to the reactor for the first time, stirred for 10 minutes, and a monomer aqueous emulsion was prepared; a peroxide initiator solution having a concentration of 0.02% was added to the reactor to initiate the first polymerization reaction; after the reaction started, the heat released by the polymerization reaction raised the temperature of the monomer aqueous emulsion to 50 ℃ ~ 70 ℃; when the first polymerization reaction was completed, the temperature of the aqueous emulsion stopped rising, and cooling water was introduced into the reactor jacket to reduce the temperature of the rubber emulsion to 35 ℃ ~ 40 ℃;
[0023] S5. A second time, one-third of the mixed monomer raw material was added to the reactor and stirred for 10 minutes; a second time, a 0.02% peroxide initiator solution was added to the reactor to initiate a second polymerization reaction; when the second polymerization reaction was completed, cooling water was passed into the reactor jacket to reduce the temperature of the rubber emulsion to 35 ℃ ~ 40 ℃;
[0024] S6. One third of the mixed monomer feed was added to the reactor for the third time and stirred for 10 minutes; a peroxide initiator solution having a concentration of 0.02% was added to the reactor for the third time to initiate the third polymerization reaction;
[0025] S7. After the third polymerization reaction is completed, the rubber latex in the reactor is heated to 80 ° C and kept at 80 ° C for 1 hour;
[0026] S8. After the heat preservation is completed, the rubber latex is coagulated, the rubber particles are cleaned and dried to make rubber products.
[0027] In the above technical solution, preferably, the rubber raw material component includes epoxy type vulcanization point monomer raw material and low brittle temperature functional monomer raw material or basic acrylate monomer raw material, epoxy type vulcanization point monomer raw material and low brittle temperature functional monomer raw material.
[0028] In the above technical solution, preferably, the emulsification time in S2 is 10 minutes, and the temperature during the emulsification process is raised to 30°C to 40°C.
[0029] In the above technical solution, preferably, the polymerization reactions in S4, S5 and S6 are carried out at 30°C to 70°C.
[0030] In the above technical solution, preferably, the peroxide is ammonium persulfate.
[0031] Compared with the prior art, the epoxy acrylate rubber with low brittle temperature and the method for producing the same provided by the present invention have the following beneficial effects:
[0032] The present invention adds or increases a functional monomer raw material with a low brittle temperature that improves the low-temperature resistance of the rubber in a traditional manufacturing method. Different copolymers have different brittle temperatures, and copolymers of functional monomer raw materials with low brittle temperatures have lower brittle temperatures. Therefore, compared with traditional rubbers without the addition of functional monomer raw materials with low brittle temperatures, the rubber to which the functional monomer raw materials with low brittle temperatures are added has increased low-temperature resistance of the final rubber, thereby expanding the application field of acrylic rubber and meeting some scenarios with special requirements for the low-temperature resistance of rubber. DETAILED DESCRIPTION
[0033] An embodiment of the present invention provides an epoxy acrylate rubber with a low brittle temperature, which comprises, by weight, 5 parts of epoxy vulcanization point monomer raw materials, 75-95 parts of functional monomer raw materials with a low brittle temperature, 3 parts of emulsifier and 250 parts of deionized water.
[0034] In order to better implement the invention, in this embodiment, the epoxy type vulcanization point monomer raw material includes at least one of glycidyl acrylate, glycidyl methacrylate and glycidyl acrylate; the epoxy type vulcanization point monomer raw material is used to realize the vulcanization processing in the rubber manufacturing process.
[0035] The functional monomer raw material with low brittle temperature includes at least one of ethoxyethyl acrylate, 2-ethylhexyl acrylate, n-decyl methacrylate, n-dodecyl methacrylate, and cinnamyl methacrylate. The functional monomer raw material with low brittle temperature forms a copolymer during the rubber manufacturing process. For example, the brittle temperature of poly 2-ethylhexyl acrylate is -85°C. The brittle temperature of the rubber product is reduced by adding the functional monomer raw material with low brittle temperature.
[0036] In order to better implement the present invention, in this embodiment, the basic acrylic acid ester monomer raw material includes at least one of ethyl acrylate and methoxyethyl acrylate.
[0037] In order to better implement the invention, in this embodiment, the emulsifier is sodium lauryl sulfate.
[0038] In order to better implement the present invention, in this embodiment, at most 20 parts of basic acrylic ester monomer raw material are also included.
[0039] A method for producing an epoxy-type acrylate rubber with a low brittle temperature provided by an embodiment of the present invention comprises the following steps:
[0040] S1. Add the rubber raw material component into a mixing tank, stir and mix evenly, and prepare a mixed monomer raw material; wherein the rubber raw material component includes an epoxy-type vulcanization point monomer raw material and a low brittle temperature functional monomer raw material or a basic acrylate monomer raw material, an epoxy-type vulcanization point monomer raw material and a low brittle temperature functional monomer raw material;
[0041] S2. Deionized water and an emulsifier are added to the reactor and stirred to prepare an emulsion;
[0042] S3. Nitrogen is introduced into the reactor to replace the air;
[0043] S4. One-third of the mixed monomer raw material was added to the reactor for the first time, stirred for 10 minutes, and a monomer aqueous emulsion was prepared; a peroxide initiator solution having a concentration of 0.02% was added to the reactor to initiate the first polymerization reaction, and the first polymerization reaction was carried out at 30 ℃ ~ 70 ℃; after the reaction started, the heat released by the polymerization reaction raised the temperature of the monomer aqueous emulsion to 50 ℃ ~ 70 ℃; when the first polymerization reaction was completed, the temperature of the aqueous emulsion stopped rising, and cooling water was introduced into the reactor jacket to reduce the temperature of the rubber emulsion to 35 ℃ ~ 40 ℃;
[0044] S5. A third of the mixed monomer raw material was added to the reactor for the second time and stirred for 10 minutes; a peroxide initiator solution having a concentration of 0.02% was added to the reactor for the second time to initiate a second polymerization reaction, and the second polymerization reaction was carried out at 30 ℃ ~ 70 ℃; when the second polymerization reaction was completed, cooling water was introduced into the reactor jacket to reduce the temperature of the rubber latex to 35 ℃ ~ 40 ℃; the second polymerization reaction was performed so that the molecular weight of the polymer generated by the first polymerization reaction increased;
[0045] S6. One third of the mixed monomer raw material was added to the reactor for the third time and stirred for 10 minutes; a peroxide initiator solution having a concentration of 0.02% was added to the reactor for the third time to initiate a third polymerization reaction, and the third polymerization reaction was carried out at 30 ℃ ~ 70 ℃; the third polymerization reaction continued to increase the molecular weight of the polymer to achieve the desired target requirements;
[0046] S7. After the third polymerization reaction is completed, the rubber latex in the reactor is heated to 80°C and kept at 80°C for 1 hour to ensure that the residual monomer raw materials in the rubber latex can be forced to react at high temperature to reduce the residual monomer raw materials;
[0047] S8. After the heat preservation is completed, the rubber latex is coagulated, the rubber particles are cleaned and dried to make rubber products.
[0048] In order to better implement the present invention, in this embodiment, the emulsification time in S2 is 10 minutes, and the temperature during the emulsification process is raised to 30°C to 40°C.
[0049] In order to better implement the invention, in this embodiment, the peroxide is ammonium persulfate.
[0050] Through three "intermittent" polymerization reactions, the molecular weight of the polymer is continuously increased. Compared with one-time addition, three-time addition is more convenient for production operation, and one-time addition requires too high control of the dripping speed. If improperly controlled, the temperature may rise too high or the polymerization reaction may be interrupted. Three "intermittent" polymerization reactions are more convenient for controlling the reaction temperature, so that the polymerization reaction between the entire monomer raw materials can be more complete, reducing the residue of unreacted monomer raw materials and affecting the quality of rubber products.
[0051] The chemical structure of the monomer raw material contains double bonds. Under the action of the free radicals of the initiator, the double bonds are opened to form cross-linking points. When the cross-linking points between the acrylate monomers are "linked" to each other, a macromolecular polymer is formed, and the polymer molecules become larger and larger during the reaction until the target value is reached. At the same time, the functional monomer raw material with a low brittle temperature will also become a part of the polymer, thereby improving the low-temperature resistance of the formed rubber.
[0052] Example 1
[0053] An embodiment of the present invention provides an epoxy acrylate rubber with a low brittle temperature, which includes, by weight, 20 parts of a basic acrylate monomer raw material, 5 parts of an epoxy vulcanization point monomer raw material, 75 parts of a functional monomer raw material with a low brittle temperature, 3 parts of an emulsifier and 250 parts of deionized water.
[0054] Among them, the basic acrylic ester monomer raw material is 20 parts of ethyl acrylate;
[0055] The epoxy type vulcanization point monomer raw material is 5 parts of glycidyl acrylate;
[0056] The functional monomer raw material with low brittle temperature is 75 parts of 2-ethylhexyl acrylate;
[0057] The emulsifier is sodium lauryl sulfate.
[0058] A method for producing an epoxy-type acrylate rubber with a low brittle temperature provided by an embodiment of the present invention comprises the following steps:
[0059] S1 20 parts of ethyl acrylate, 5 parts of glycidyl acrylate and 75 parts of 2-ethylhexyl acrylate were added to a mixing tank, stirred and mixed to prepare a mixed monomer raw material;
[0060] S2. Deionized water and an emulsifier are added to the reactor and stirred to prepare an emulsion;
[0061] S3. Nitrogen is introduced into the reactor to replace the air;
[0062] S4. One-third of the mixed monomer raw material was added to the reactor for the first time, stirred for 10 minutes, and a monomer aqueous emulsion was prepared; a peroxide initiator solution having a concentration of 0.02% was added to the reactor to initiate the first polymerization reaction, and the first polymerization reaction was carried out at 30 ℃ ~ 70 ℃; after the reaction started, the heat released by the polymerization reaction raised the temperature of the monomer aqueous emulsion to 50 ℃ ~ 70 ℃; when the first polymerization reaction was completed, the temperature of the aqueous emulsion stopped rising, and cooling water was introduced into the reactor jacket to reduce the temperature of the rubber emulsion to 35 ℃ ~ 40 ℃;
[0063] S5. A third of the mixed monomer raw material is added to the reactor for the second time, and stirred for 10 minutes. The mixed monomer raw material enters the "micelles" of the monomer aqueous emulsion to form "micelles" containing "polymer" and "mixed monomer raw material"; a peroxide initiator solution having a concentration of 0.02% is added to the reactor for the second time to initiate a second polymerization reaction, and the second polymerization reaction is carried out at 30°C to 70°C; after the second polymerization reaction is completed, cooling water is introduced into the reactor jacket to reduce the temperature of the rubber emulsion to 35°C to 40°C; the second polymerization reaction increases the molecular weight of the polymer generated by the first polymerization reaction;
[0064] S6. One third of the mixed monomer raw material was added to the reactor for the third time and stirred for 10 minutes; a peroxide initiator solution having a concentration of 0.02% was added to the reactor for the third time to initiate a third polymerization reaction, and the third polymerization reaction was carried out at 30 ℃ ~ 70 ℃; the third polymerization reaction continued to increase the molecular weight of the polymer to achieve the desired target requirements;
[0065] S7. After the third polymerization reaction is completed, the rubber latex in the reactor is heated to 80°C and kept at 80°C for 1 hour to ensure that the residual monomer raw materials in the rubber latex can be forced to react at high temperature to reduce the residual monomer raw materials;
[0066] S8. After the heat preservation is completed, the rubber latex is coagulated, the rubber particles are cleaned and dried to make rubber products.
[0067] In order to better implement the present invention, in this embodiment, the emulsification time in S2 is 10 minutes, and the temperature during the emulsification process is raised to 30°C to 40°C.
[0068] In order to better implement the invention, in this embodiment, the peroxide is ammonium persulfate.
[0069] Example 2
[0070] An embodiment of the present invention provides an epoxy acrylate rubber with a low brittle temperature, which includes, by weight, 10 parts of a basic acrylate monomer raw material, 5 parts of an epoxy vulcanization point monomer raw material, 85 parts of a functional monomer raw material with a low brittle temperature, 3 parts of an emulsifier and 250 parts of deionized water.
[0071] Among them, the basic acrylic acid ester monomer raw material is 10 parts of methoxyethyl acrylate;
[0072] The epoxy type vulcanization point monomer raw material is 5 parts of glycidyl acrylate;
[0073] The functional monomer raw material with low brittle temperature is 85 parts of n-decyl methacrylate;
[0074] The emulsifier is sodium lauryl sulfate.
[0075] The method for manufacturing a low brittle temperature epoxy acrylate rubber provided in Example 2 of the present invention is consistent with that in Example 1.
[0076] Example 3
[0077] An embodiment of the present invention provides an epoxy acrylate rubber with a low brittle temperature, which comprises, by weight, 5 parts of a basic acrylate monomer raw material, 5 parts of an epoxy vulcanization point monomer raw material, 90 parts of a functional monomer raw material with a low brittle temperature, 3 parts of an emulsifier and 250 parts of deionized water.
[0078] Among them, the basic acrylic acid ester monomer raw material is 5 parts of ethyl acrylate;
[0079] The epoxy type vulcanization point monomer raw material is 5 parts of glycidyl methacrylate;
[0080] The functional monomer raw material with low brittle temperature is 90 parts of n-dodecyl methacrylate;
[0081] The emulsifier is sodium lauryl sulfate.
[0082] The method for manufacturing a low brittle temperature epoxy acrylate rubber provided in Example 3 of the present invention is consistent with that in Example 1.
[0083] Example 4
[0084] An embodiment of the present invention provides an epoxy acrylate rubber with a low brittle temperature, which comprises, by weight, 5 parts of a basic acrylate monomer raw material, 5 parts of an epoxy vulcanization point monomer raw material, 90 parts of a functional monomer raw material with a low brittle temperature, 3 parts of an emulsifier and 250 parts of deionized water.
[0085] Among them, the basic acrylic acid ester monomer raw material is 5 parts of ethyl acrylate;
[0086] The epoxy type vulcanization point monomer raw material is 5 parts of glycidyl methacrylate;
[0087] The functional monomer raw material with low brittle temperature is 90 parts of cinnamyl methacrylate;
[0088] The emulsifier is sodium lauryl sulfate.
[0089] The method for manufacturing a low brittle temperature epoxy acrylate rubber provided in Example 4 of the present invention is consistent with that in Example 1.
[0090] Example 5
[0091] An embodiment of the present invention provides an epoxy acrylate rubber with a low brittle temperature, which comprises, by weight, 5 parts of epoxy vulcanization point monomer raw materials, 95 parts of functional monomer raw materials with a low brittle temperature, 3 parts of emulsifier and 250 parts of deionized water.
[0092] Among them, the epoxy type vulcanization point monomer raw material is 5 parts of glycidyl methacrylate;
[0093] The functional monomer raw material with low brittle temperature is 60 parts of ethoxyethyl acrylate and 35 parts of 2-ethylhexyl acrylate;
[0094] The emulsifier is sodium lauryl sulfate.
[0095] The method for manufacturing a low brittle temperature epoxy acrylate rubber provided in Example 5 of the present invention is consistent with that in Example 1.
[0096] In this Example 5, no basic acrylic acid ester monomer raw material is added. Since the brittle temperature of the polymer of ethyl acrylate is relatively high, the addition of ethyl acrylate is not very beneficial to the reduction of the brittle temperature of the rubber. Although the latex coagulation time of the rubber prepared is prolonged without adding the basic acrylic acid ester monomer raw material, it does not affect the low temperature resistance of the rubber and the use of the rubber as a whole.
[0097] Compared with Example 5, in Example 1, the amount of ethyl acrylate added is 20 parts because the brittle temperature of the polymer of 2-ethylhexyl acrylate is -85°C. After the two are added together into the rubber preparation raw materials, the brittle temperature is balanced, and the brittle temperature of Example 1 and Example 5 can both reach about -50°C.
[0098] In order to ensure that the brittle temperature meets the actual use scenarios of the rubber, but too low a brittle temperature will also have a certain impact on other properties of the rubber. Therefore, in the actual production process, the brittle temperature value of the rubber can be adjusted by adding different monomer raw material components and types of monomer raw materials.
[0099] Comparative Example 1
[0100] The raw materials of acrylic acid ester monomers include 75 parts of ethyl acrylate, 20 parts of n-butyl acrylate, 5 parts of epoxy monomer raw materials, 3 parts of emulsifier and 250 parts of deionized water.
[0101] The manufacturing method of the epoxy type acrylate rubber provided in this comparative example 1 is consistent with that in Example 1.
[0102] Comparative Example 2
[0103] The raw materials of acrylic acid ester monomers include 45 parts of ethyl acrylate, 25 parts of n-butyl acrylate, 25 parts of methoxyethyl acrylate, the raw materials of epoxy monomers include 5 parts of glycidyl methacrylate, 3 parts of emulsifier and 250 parts of deionized water.
[0104] The manufacturing method of the epoxy type acrylate rubber provided in this comparative example 2 is consistent with that in example 1.
[0105] The brittle temperature performance test was performed on Examples 1 to 5 and Comparative Examples 1 to 2, as shown in Table 1.
[0106] Table 1
[0107] Brittle temperature, °C Example 1 -58 Example 2 -56 Example 3 -49 Example 4 -48 Example 5 -50 Comparative Example 1 -21 Comparative Example 2 -28
[0108] It can be seen from Table 1 that the rubbers prepared in Examples 1 to 5 after adding functional monomer raw materials with low brittle temperatures that improve the low-temperature resistance of the rubber have lower brittle temperatures than the rubbers prepared in Comparative Examples 1 to 2, that is, the low-temperature resistance of the rubber is improved.
[0109] In summary, the present invention provides a low-temperature resistant epoxy acrylate rubber and a manufacturing method thereof. The rubber raw materials are mixed and stirred by adding or increasing a functional monomer raw material with a low brittle temperature to prepare a mixed monomer raw material. The emulsion prepared by mixing deionized water and an emulsifier is heated to 30°C to 40°C. When nitrogen is filled to remove the air in the reactor, one-third of the mixed monomer raw material is added to the emulsion, and ammonium persulfate with a concentration of 0.02% is added to initiate the first polymerization reaction in the reactor. When the emulsion reaches a temperature of 50°C to 70°C, if the temperature does not continue to rise, it means that the reaction is basically completed. The emulsion temperature is lowered to 35 to 40°C, one-third of the mixed monomer raw material is added for the second time, and the mixture is stirred for 10 minutes. The initiator solution with a concentration of 0.02% is added for the second time to initiate the second polymerization reaction, so that the polymer molecular chain grows. Then the third polymerization reaction is initiated in the same way. After the third polymerization reaction is completed, the temperature of the rubber latex is directly raised to 80°C without cooling down, and kept warm for 1 hour to force the residual monomers in the emulsion to react at high temperature and reduce the residual amount of monomer raw materials. After the insulation is completed, the rubber product is made, and the functional monomer raw materials with low brittle temperature are polymerized with the epoxy type vulcanization point monomer raw materials and the basic acrylate monomer raw materials to form a polymer. The polymer formed by the added functional monomer raw materials with low brittle temperature that improves the low temperature resistance of the rubber reduces the brittle temperature of the rubber, thereby improving the low temperature resistance of the final rubber product.
[0110] In the description of the present invention, “plurality” means two or more than two, unless otherwise clearly and specifically defined.
[0111] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the scope of protection of the invention. Obviously, the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on these embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field can still combine, add, delete or make other adjustments to the features in the various embodiments of the present invention according to the circumstances without conflict, without making creative work, so as to obtain different other technical solutions that do not deviate from the concept of the present invention in essence, and these technical solutions also belong to the scope of protection of the present invention.
Claims
1. An epoxy-type acrylate rubber with a low brittle temperature, characterized in that: The composition includes 5 parts of epoxy curing point monomer raw materials, 75-95 parts of low brittle temperature functional monomer raw materials, 3 parts of emulsifier and 250 parts of deionized water, and also includes up to 20 parts of basic acrylate monomer raw materials. The epoxy type vulcanization point monomer raw material includes at least one of glycidyl acrylate, glycidyl methacrylate and glycidyl acrylate; The functional monomer raw material with low brittle temperature includes at least one of ethoxyethyl acrylate, 2-ethylhexyl acrylate, n-decyl methacrylate, n-dodecyl methacrylate, and cinnamyl methacrylate; The basic acrylic acid ester monomer raw material includes at least one of ethyl acrylate and methoxyethyl acrylate.
2. The epoxy-type acrylate rubber with low brittle temperature according to claim 1, characterized in that: The emulsifier is sodium lauryl sulfate.
3. A method for producing an epoxy-type acrylate rubber with a low brittle temperature according to any one of claims 1 or 2, characterized in that: The following steps are involved: S1. The rubber raw material component is added to the mixing tank, stirred and mixed evenly to prepare a mixed monomer raw material; S2. Deionized water and an emulsifier are added to the reactor and stirred to prepare an emulsion; S3. Nitrogen is introduced into the reactor to replace the air; S4. One third of the mixed monomer raw materials were added to the reactor for the first time, and stirred for 10 minutes to prepare a monomer aqueous emulsion; a peroxide initiator solution with a concentration of 0.02% was added to the reactor to initiate the first polymerization reaction; after the reaction started, the heat released by the polymerization reaction raised the temperature of the monomer aqueous emulsion to 50°C~70°C; after the first polymerization reaction was completed, the temperature of the aqueous emulsion stopped rising, and cooling water was introduced into the jacket of the reactor to reduce the temperature of the rubber emulsion to 35°C~40°C; S5. A third of the mixed monomer raw material was added to the reactor for the second time and stirred for 10 minutes; a peroxide initiator solution having a concentration of 0.02% was added to the reactor for the second time to initiate a second polymerization reaction; when the second polymerization reaction was completed, cooling water was introduced into the reactor jacket to reduce the temperature of the rubber latex to 35°C~40°C; S6. One third of the mixed monomer feed was added to the reactor for the third time and stirred for 10 minutes; a peroxide initiator solution having a concentration of 0.02% was added to the reactor for the third time to initiate the third polymerization reaction; S7. After the third polymerization reaction is completed, the rubber latex in the reactor is heated to 80 ° C and kept at 80 ° C for 1 hour; S8. After the heat preservation is completed, the rubber latex is coagulated, the rubber particles are cleaned and dried to make rubber products.
4. The method for producing the epoxy type acrylate rubber with low brittle temperature according to claim 3, characterized in that: The rubber raw material components include epoxy type vulcanization point monomer raw materials and low brittle temperature functional monomer raw materials or basic acrylate monomer raw materials, epoxy type vulcanization point monomer raw materials and low brittle temperature functional monomer raw materials.
5. The method for producing the epoxy type acrylate rubber with low brittle temperature according to claim 3, characterized in that: The emulsification time in S2 is 10 minutes, and the temperature rises to 30°C-40°C during the emulsification process.
6. The method for producing the epoxy type acrylate rubber with low brittle temperature according to claim 3, characterized in that: The polymerization reactions in S4, S5 and S6 are carried out at 30°C to 70°C.
7. The method for producing the epoxy type acrylate rubber with low brittle temperature according to claim 3, characterized in that: The peroxide is ammonium persulfate.
Citation Information
Patent Citations
Preparation method of raw oil-extended alkyl acrylate copolymer (ACM)
CN102643383A
Micro-crosslinking low temperature resistant raw acrylic rubber and preparation method thereof
CN107915807A
Polyacrylate emulsion and preparation method thereof
CN112194760A
Preparation process of easy processing cold resisting type polyacrylate rubber
CN1861678A
Method of manufacturing aqueous emulsion
KR100894447B1