A composite conductive agent slurry and its preparation method

By preparing a porous sodium borosilicate composite thermally conductive material combined with graphene and single-walled carbon nanotubes, the problems of self-discharge, difficult dispersion, and insufficient thermal conductivity of carbon nanotube conductive agents in lithium-ion batteries were solved, achieving high conductivity, good dispersion, and excellent heat dissipation, thereby improving battery performance and safety.

CN117219771BActive Publication Date: 2026-11-17广东嘉尚新能源材料有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311141508.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-06
Publication Date
2026-11-17
Estimated Expiration
2043-09-06

AI Technical Summary

Technical Problem

Existing carbon nanotube conductive agents in lithium-ion batteries suffer from problems such as self-discharge due to metal impurity oxidation, difficulty in dispersion, and inability to meet the thermal conductivity requirements under high-rate charge and discharge conditions.

Method used

A composite conductive agent slurry was prepared by combining porous sodium borosilicate composite thermal conductive material with graphene and single-walled carbon nanotubes, along with polyvinyl alcohol and polyurea-modified α-cyanoacrylate, and by ultrasonic treatment and vacuum degassing.

Benefits of technology

It improves conductivity, dispersion, and heat dissipation, extending the lifespan and safety of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004433614830000131
    Figure BDA0004433614830000131
Patent Text Reader

Abstract

This invention discloses a composite conductive agent slurry and its preparation method. The preparation method includes the following steps: 1) stirring a mixed solution of sodium borate and sodium silicate, then adding sodium bicarbonate, and continuing to stir and mix to obtain a composite solution; 2) cooling the composite solution, then placing it in a high-temperature furnace for heat treatment under a nitrogen or argon atmosphere to obtain a porous sodium borosilicate composite thermal conductive material; 3) adding single-walled carbon nanotubes, the porous sodium borosilicate composite thermal conductive material, and graphene to a solution containing polyvinyl alcohol, stirring and mixing, then adding polyurea-modified α-cyanoacrylate, and mixing the mixture with methyl acetate to obtain a primary solution; 4) subjecting the primary solution to ultrasonic treatment in a water bath environment using an ultrasonic treatment device, and then degassing it under vacuum to obtain the composite conductive agent slurry. The composite conductive agent provided by this invention has significantly improved conductivity, dispersibility, and heat dissipation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery materials technology, specifically to a composite conductive agent slurry and its preparation method. Background Technology

[0002] In the fabrication of lithium-ion batteries, conductive agents play a crucial role. Although their proportion in the overall composition is relatively small, they have a profound impact on battery performance, such as cycle performance, capacity utilization, and rate performance. The main function of conductive agents is to improve electronic conductivity. To ensure excellent charge-discharge performance of the electrodes, a certain amount of conductive agent is usually added during electrode manufacturing. This allows for the collection of micro-currents between active materials and between active materials and current collectors, reducing electrode contact resistance and accelerating electron movement. Furthermore, conductive agents can improve electrode processability, promote electrolyte penetration into the electrodes, and effectively increase the migration rate of lithium ions in the electrode material, reducing polarization, thereby improving electrode charge-discharge efficiency and the lifespan of the lithium battery.

[0003] Currently, conductive agents in lithium-ion batteries typically employ materials such as conductive graphite, acetylene black, or carbon nanotubes. Among these, carbon nanotubes (CNTs) are linear, one-dimensional carbonaceous materials with superior electrical conductivity and excellent mechanical properties. Because the amount of carbon nanotubes added to the electrode is relatively small, the reduction in electrode energy capacity is also relatively minimal.

[0004] However, existing carbon nanotube conductive agents still have some shortcomings: First, existing carbon nanotubes retain residual metal catalysts from the synthesis process. During high-potential charging and discharging of the battery, these metal impurities are easily oxidized and deposited on the negative electrode surface, leading to micro-short circuits inside the battery, severe self-discharge, and even safety accidents. Second, the strong van der Waals forces between carbon nanotubes make uniform dispersion in the active material difficult, easily causing aggregation and hindering conductivity. Finally, the limited performance of carbon nanotubes cannot meet the high thermal conductivity and heat dissipation requirements of battery electrodes under high-rate charging and discharging.

[0005] To address the aforementioned problems, this invention provides a composite conductive agent slurry and its preparation method. This novel composite conductive agent slurry possesses advantages such as high conductivity, good dispersibility, and excellent heat dissipation, effectively solving the problems existing in current carbon nanotube conductive agents and providing new possibilities for improving the performance and extending the lifespan of lithium-ion batteries. Summary of the Invention

[0006] The purpose of this invention is to address the shortcomings of existing technologies by providing a composite conductive agent slurry and its preparation method. The composite conductive agent slurry prepared by this invention has the advantages of high conductivity, good dispersibility, and excellent heat dissipation.

[0007] To achieve the above objectives, the present invention adopts the following technical solution:

[0008] A method for preparing a composite conductive agent slurry includes the following steps:

[0009] 1) Stir the mixed solution of sodium borate and sodium silicate magnetically at 75-85℃, then add sodium bicarbonate and continue stirring to obtain a composite solution;

[0010] 2) Cool the composite solution from step 1) and then place it in a high-temperature furnace. Heat it at 400-500℃ for 2-4 hours under a nitrogen or argon atmosphere to obtain a porous sodium borosilicate composite thermal conductive material.

[0011] 3) Add single-walled carbon nanotubes, porous sodium borosilicate composite thermal conductive material and graphene to a solution containing polyvinyl alcohol at a mass ratio of 10:(2~4):(3~6). After stirring and mixing, add polyurea-modified α-cyanoacrylate. Mix the mixture with methyl acetate at a mass ratio of (94~97):(3~6) to obtain the primary solution of composite conductive agent slurry.

[0012] 4) The primary solution from step 3) is subjected to ultrasonic treatment at a power of 200-300W and an oscillation frequency of 20-40kHz in a water bath at 85-90℃ for 30-60 minutes, and then subjected to vacuum degassing to obtain the composite conductive agent slurry.

[0013] Preferably, in step 1), the mass ratio of sodium borate, sodium silicate, and sodium bicarbonate is 10:(5-8):2.

[0014] Preferably, in step 4), the vacuum degassing process is as follows: the slurry is placed in a vacuum chamber, the vacuum degree is controlled at -0.08 to -0.15 MPa, and the holding time is 10-20 minutes.

[0015] Preferably, in step 3), after stirring and mixing, sodium sulfate stabilizer accounting for 2-4% of the total mass of the solution is added.

[0016] Preferably, in step 3), after stirring and mixing, nano-silica is added, accounting for 1-5% of the total mass of the solution.

[0017] Preferably, in step 3), after stirring and mixing, a nano-titanium oxide and tannic acid composition accounting for 1-5% of the total mass of the solution is added, wherein the mass ratio of nano-titanium oxide to tannic acid is (1-2):1.

[0018] Preferably, in step 3), after stirring and mixing, carbon nanofibers or boron nitrides accounting for 1 to 5% of the total mass of the solution are added.

[0019] Preferably, in step 3), after stirring and mixing, a composition of povidone and boric acid accounting for 1-5% of the total mass of the solution is added, wherein the mass ratio of povidone to boric acid is (1-2):1.

[0020] Preferably, in step 3), after stirring and mixing, a polydopamine and ethyl acetate composition accounting for 1-5% of the total mass of the solution is added, wherein the mass ratio of polydopamine to ethyl acetate is (1-2):1.

[0021] Preferably, in step 3), after stirring and mixing, a thiol-based compound accounting for 1-5% of the total mass of the solution is added, wherein the thiol-based compound is mercaptoacetic acid or methanethiol.

[0022] Preferably, in step 4), the ultrasonic treatment process also includes adding 1-5% of a polyoxyethylene surfactant by mass of the total solution.

[0023] Preferably, in step 4), the ultrasonic treatment process further includes introducing an inert gas into the mixture being treated using a bubbler.

[0024] Preferably, in step 3), the mass ratio of polyvinyl alcohol to polyurea-modified α-cyanoacrylate is (1-2):1.

[0025] Preferably, the synthesis of the polyurea-modified α-cyanoacrylate includes the following steps:

[0026] 1) Dissolve polyurea and methacrylate in anhydrous ethanol at a mass ratio of 1.2:1 to form a solution with a reaction concentration of 45%;

[0027] 2) Place the solution into the reactor and stir at 70-80℃ for 2-4 hours;

[0028] 3) After the reaction is complete, cool the reaction solution to room temperature;

[0029] 4) By vacuum freeze drying, the vacuum degree is first adjusted to 0.05~0.1MPa, and then the temperature is controlled at -40~-45℃ to remove the solvent, so as to obtain polyurea modified α-cyanoacrylate.

[0030] In addition, the present invention also provides a composite conductive agent slurry, which is prepared by the method for preparing composite conductive agent slurry described in any of the preceding paragraphs.

[0031] Compared with the prior art, the present invention has at least the following beneficial effects:

[0032] 1) This application incorporates sodium bicarbonate, sodium borate, and sodium silicate. Sodium bicarbonate decomposes at high temperatures to form a porous sodium borosilicate composite thermal conductive material with excellent thermal conductivity. This material can effectively transfer heat to the outside of the battery during operation, preventing overheating and improving battery stability and safety.

[0033] 2) This application incorporates graphene, an allotrope of carbon nanotubes with a similar chemical structure. The sp2 hybridized carbon atoms generate numerous delocalized π electrons, which bind to the carbon nanotubes through π-π interactions, thus separating the nanotubes and improving their dispersion. Furthermore, graphene possesses a very high specific surface area and conductivity, further enhancing the conductivity and stability of the composite conductive agent. Additionally, graphene exhibits a high thermal conductivity, allowing for rapid heat diffusion within the composite conductive agent, resulting in a more uniform temperature distribution and greater heat absorption in the phase change material. Therefore, the addition of graphene and carbon nanotubes improves the electrical conductivity of the composite conductive agent slurry, thereby enhancing the battery's discharge efficiency. Simultaneously, it also improves the thermal conductivity of the composite conductive agent slurry, reducing the internal temperature during battery operation and improving both battery efficiency and safety.

[0034] 3) This application introduces polyvinyl alcohol (PVA) as a dispersant. PVA can interact with the surface of carbon nanotubes (CNTs), reducing the mutual attraction between CNTs and preventing their aggregation, thereby effectively dispersing the carbon nanotube particles. This application also introduces polyurea-modified α-cyanoacrylate (POA) as a slurry stabilizer, which can improve the stability of the composite conductive agent slurry. PEA is a block copolymer of polyurea and methacrylate, and its presence helps to reduce the deposition, separation, or agglomeration of the dispersed phase in the slurry.

[0035] 4) By adding methyl acetate, this application serves two purposes. First, as a foaming agent, it thermally decomposes during the mixing process to generate bubbles. As the bubbles rise, they further improve the dispersion of the mixture and can also help the conductive agent slurry form a porous structure, further improving the heat dissipation effect. Second, as a dispersant, it can effectively disperse the conductive agent slurry and stabilize the dispersion state of carbon nanotubes.

[0036] 5) This application utilizes ultrasonic treatment to better disperse graphene and carbon nanotubes in the composite conductive agent slurry, further improving the conductivity and stability of the conductive agent. Furthermore, ultrasonic treatment overcomes the strong adsorption force of carbon nanotube aggregates and disrupts the entangled bonding of long carbon nanotube fibers, breaking down the carbon nanotube aggregates and dispersing them. This results in a more uniform distribution and better dispersion of the composite conductive agent slurry, thereby improving the battery's charge-discharge efficiency and cycle stability. In addition, this application employs vacuum degassing to remove air bubbles from the slurry, preventing them from affecting the uniformity of coating during subsequent processes, while simultaneously improving the contact between the battery cells and the battery's charge-discharge performance.

[0037] Therefore, the composite conductive agent provided by the present invention has significantly improved conductivity, dispersibility and heat dissipation, thereby improving the service life and safety of lithium-ion batteries. Detailed Implementation

[0038] To make the technical solutions and advantages of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0039] According to a first aspect of the present invention, the present invention provides a method for preparing a composite conductive agent slurry, comprising the following steps:

[0040] 1) Stir the mixed solution of sodium borate and sodium silicate magnetically at 75-85℃, then add sodium bicarbonate and continue stirring to obtain a composite solution;

[0041] 2) Cool the composite solution from step 1) and then place it in a high-temperature furnace. Heat it at 400-500℃ for 2-4 hours under a nitrogen or argon atmosphere to obtain a porous sodium borosilicate composite thermal conductive material.

[0042] 3) Add single-walled carbon nanotubes, porous sodium borosilicate composite thermal conductive material and graphene to a solution containing polyvinyl alcohol at a mass ratio of 10:(2~4):(3~6). After stirring and mixing, add polyurea-modified α-cyanoacrylate. Mix the mixture with methyl acetate at a mass ratio of (94~97):(3~6) to obtain the primary solution of composite conductive agent slurry.

[0043] 4) The primary solution from step 3) is subjected to ultrasonic treatment at a power of 200-300W and an oscillation frequency of 20-40kHz in a water bath at 85-90℃ for 30-60 minutes, and then subjected to vacuum degassing to obtain the composite conductive agent slurry.

[0044] Compared with existing technologies, the composite conductive agent prepared by this invention has the following advantages:

[0045] 1) High conductivity: By selecting materials with good conductivity, such as single-walled carbon nanotubes and graphene, and then adding polyurea-modified α-cyanoacrylate to adjust the chemical composition, the resulting slurry ultimately possesses high conductivity. High conductivity ensures smooth current switching and transmission, significantly improving the functionality of electrical appliances and power conversion efficiency.

[0046] 2) Good dispersibility: Through the mixing method in step 3), and the addition of polyvinyl alcohol dispersant and polyurea-modified α-cyanoacrylate, the uniform distribution of various materials in the solution is ensured, eliminating the phenomena of separation and segregation. Therefore, the resulting slurry has good dispersibility. Especially in step 4, the ultrasonic treatment and vacuum degassing treatment make the various components more evenly distributed in the slurry. By increasing the contact area between materials, it is beneficial to improve its conductivity.

[0047] 3) Excellent heat dissipation: The high-temperature furnace treatment in step 2) creates a porous structure in the sodium borosilicate composite thermally conductive material. This structure increases the surface area of ​​the material, thereby improving heat dissipation efficiency. Simultaneously, the addition of graphene and single-walled carbon nanotubes in step 3), with their excellent thermal conductivity, also contributes to the good heat dissipation of the composite slurry. During current transmission, this heat dissipation performance helps protect components and extend equipment lifespan.

[0048] In one embodiment of this application, in step 1), the mass ratio of sodium borate, sodium silicate and sodium bicarbonate is 10:(5-8):2; preferably, the mass ratio is 10:6:2.

[0049] In one embodiment of this application, in step 4), the vacuum degassing process is as follows: the slurry is placed in a vacuum chamber, the vacuum degree is controlled at -0.08 to -0.15 MPa, and the holding time is 10-20 minutes.

[0050] In one embodiment of this application, step 3) further includes adding 2-4% sodium sulfate stabilizer by mass of the total solution after stirring and mixing. Adding sodium sulfate stabilizer can further improve the stability and conductivity of the composite conductive agent slurry.

[0051] In one embodiment of this application, step 3) further includes adding 1-5% nano-silica by mass of the total solution after stirring and mixing. The charge transfer interaction between silica and single-walled carbon nanotubes allows silica to be well adsorbed on the surface of the single-walled carbon nanotubes, thereby generating an effective charge on the surface of the single-walled carbon nanotubes and improving the dispersibility and stability of the carbon nanotubes.

[0052] In one embodiment of this application, step 3) further includes adding a nano-titanium oxide and tannic acid composition accounting for 1-5% of the total mass of the solution after stirring and mixing, wherein the mass ratio of nano-titanium oxide to tannic acid is (1-2):1. Although inorganic nanoparticles such as silica have good dispersion effects, their dispersibility changes with aging time. Stable metal particles readily interact with carbon nanotubes through charge transfer, exhibiting good affinity for carbon nanotubes. In this embodiment, titanium metal ions and tannic acid are coated onto the surface of carbon nanotubes through π-π interactions to form a stable metal-polyphenol coordination structure, further improving the conductivity, dispersibility, and thermal stability of carbon nanotubes.

[0053] In one embodiment of this application, step 3), after stirring and mixing, further includes adding 1-5% by mass of carbon nanofibers or boron nitrides to the total solution. Adding carbon nanofibers or boron nitrides can give the composite conductive agent higher electrical and thermal conductivity.

[0054] In one embodiment of this application, step 3), after stirring and mixing, further includes adding a composition of povidone and boric acid, accounting for 1-5% of the total mass of the solution, wherein the mass ratio of povidone to boric acid is (1-2):1. Povidone is an excellent dispersant; its addition can improve the dispersion effect of carbon nanotubes. Because povidone can form a stable layer on the surface compatible with the carbon nanotube interface, it can prevent the re-aggregation of carbon nanotubes and improve dispersion stability. Boric acid is added because it can form a compatible system with povidone, enhancing the thermal stability of povidone; furthermore, introducing boric acid into graphene and carbon nanotubes can increase the hole concentration, thereby transforming the material into a p-type, improving its conductivity and stability.

[0055] In one embodiment of this application, after stirring and mixing in step 3), a polydopamine and ethyl acetate composition comprising 1-5% of the total mass of the solution is added, wherein the mass ratio of polydopamine to ethyl acetate is (1-2):1. Polydopamine exhibits strong π-π interactions with carbon nanotubes, forming an effective and stable coating layer on the surface of the carbon nanotubes. Furthermore, the amino or hydroxyl groups on the surface of polydopamine form covalent bonds with the hydroxyl or amino groups of the ethyl acetate solution, thereby improving the dispersibility of the carbon nanotubes.

[0056] In one embodiment of this application, step 3) further includes adding a thiol-based compound, comprising 1-5% of the total mass of the solution, after stirring and mixing. The thiol-based compound is mercaptoacetic acid or methanethiol. The thiol groups form chemical bonds (SC bonds) with the surface of the carbon nanotubes, further enhancing the hydrophilicity and dispersibility of the carbon nanotubes. Mercaptoacetic acid is preferably used, as it is a compound possessing both thiol and carboxyl groups. It not only has strong reducing properties, but its sulfur atoms also form chemical bonds with the carbon nanotubes, thereby improving the stability of the nanotubes and the conductivity after treatment.

[0057] In one embodiment of this application, after stirring and mixing in step 3), a composition of polythiophene and polypyrrolidone, comprising 1-5% of the total mass of the solution, is added, wherein the mass ratio of polythiophene to polypyrrolidone is (1-2):1. Polythiophene contains thiophene groups, which are adsorbed onto the surface of carbon nanotubes in an entangled manner through π-π conjugation, effectively dispersing and stabilizing the carbon nanotubes. Furthermore, the polythiophene backbone has a high π-electron cloud density, thus exhibiting high electrical conductivity, which improves the overall conductivity of the carbon nanotubes, thereby enhancing the performance of the composite conductive agent. Polypyrrolidone possesses good heat resistance and acid / alkali resistance, and its ketone groups can form weak interactions with carbon nanotubes, allowing for better dispersion within the carbon nanotubes. Simultaneously, polypyrrolidone itself has a certain thermal conductivity, which can improve the thermal conductivity of the composite conductive agent. Therefore, in this embodiment, the simultaneous addition of polythiophene and polypyrrolidone not only improves the electrical conductivity of the composite conductive agent but also further enhances its dispersibility and heat dissipation.

[0058] In one embodiment of this application, step 4), during the ultrasonic treatment, further includes adding a polyoxyethylene surfactant at a concentration of 1-5% of the total mass of the solution. Adding the polyoxyethylene surfactant can reduce the surface tension of the composite conductive agent slurry, allowing the graphene and carbon nanotubes in the slurry to disperse better, which is beneficial for improving conductivity and dispersibility.

[0059] In one embodiment of this application, step 4) of the ultrasonic treatment further includes introducing an inert gas into the mixture being treated using a bubbler. Introducing inert gas using a bubbler can break up some aggregates in the mixture, achieving a better dispersion effect.

[0060] In one embodiment of this application, in step 3), the mass ratio of polyvinyl alcohol and polyurea-modified α-cyanoacrylate is (1-2):1.

[0061] In one embodiment of this application, the synthesis of the polyurea-modified α-cyanoacrylate includes the following steps:

[0062] 1) Dissolve polyurea and methacrylate in anhydrous ethanol at a mass ratio of 1.2:1 to form a solution with a reaction concentration of 45%;

[0063] 2) Place the solution into the reactor and stir at 70-80℃ for 2-4 hours;

[0064] 3) After the reaction is complete, cool the reaction solution to room temperature;

[0065] 4) By vacuum freeze drying, the vacuum degree is first adjusted to 0.05~0.1MPa, and then the temperature is controlled at -40~-45℃ to remove the solvent, so as to obtain polyurea modified α-cyanoacrylate.

[0066] According to a second aspect of the present invention, the present invention also provides a composite conductive agent slurry, which is prepared by the method for preparing composite conductive agent slurry described in any of the preceding paragraphs.

[0067] The present application will be further described below with reference to specific embodiments.

[0068] Example 1

[0069] This embodiment describes a method for preparing a composite conductive agent slurry, comprising the following steps:

[0070] 1) Stir the mixed solution of sodium borate and sodium silicate magnetically at 80°C, then add sodium bicarbonate and continue stirring to obtain a composite solution; wherein the mass ratio of sodium borate, sodium silicate and sodium bicarbonate is 10:6:2.

[0071] 2) Cool the composite solution from step 1) and then place it in a high-temperature furnace. Heat it at 450°C for 3 hours under a nitrogen or argon atmosphere to obtain a porous sodium borosilicate composite thermal conductive material.

[0072] 3) Add single-walled carbon nanotubes, porous sodium borosilicate composite thermal conductive material, and graphene to a solution containing polyvinyl alcohol in a mass ratio of 10:3:5. After stirring and mixing, add polyurea-modified α-cyanoacrylate. Mix the mixture with methyl acetate in a mass ratio of 95:5 to obtain the primary solution of the composite conductive agent slurry; wherein the mass ratio of polyvinyl alcohol to polyurea-modified α-cyanoacrylate is 1:1.

[0073] 4) The primary solution from step 3) is subjected to ultrasonic treatment at a power of 250W and an oscillation frequency of 30kHz in a 90℃ water bath environment for 45 minutes. Then, the slurry is placed in a vacuum chamber with the vacuum degree controlled at -0.15MPa and the holding time is 15 minutes to obtain the composite conductive agent slurry.

[0074] Example 2

[0075] Unlike Example 1, the synthesis of polyurea-modified α-cyanoacrylate in this example includes the following steps:

[0076] 1) Dissolve polyurea and methacrylate in anhydrous ethanol at a mass ratio of 1.2:1 to form a solution with a reaction concentration of 45%;

[0077] 2) Place the solution into the reactor and stir at 75°C for 3 hours;

[0078] 3) After the reaction is complete, cool the reaction solution to room temperature;

[0079] 4) By using vacuum freeze-drying, the vacuum level is first adjusted to 0.08 MPa, and then the temperature is controlled at -40℃ to remove the solvent, thus obtaining polyurea-modified α-cyanoacrylate. Removing the solvent through vacuum freeze-drying ensures the purity of the obtained polyurea-modified α-cyanoacrylate and avoids potential pyrolysis or other heat-induced degradation problems.

[0080] The rest is the same as in Example 1, and will not be repeated here.

[0081] Example 3

[0082] Unlike Example 1, in step 3) of this example, after stirring and mixing, sodium sulfate stabilizer accounting for 3% of the total mass of the solution is added.

[0083] The rest is the same as in Example 1, and will not be repeated here.

[0084] Example 4

[0085] Unlike Example 1, in step 3) of this example, after stirring and mixing, nano-silica accounting for 3% of the total mass of the solution is added.

[0086] The rest is the same as in Example 1, and will not be repeated here.

[0087] Example 5

[0088] Unlike Example 1, in step 3) of this example, after stirring and mixing, a nano-titanium oxide and tannic acid composition accounting for 3% of the total mass of the solution is added, wherein the mass ratio of nano-titanium oxide and tannic acid is 2:1.

[0089] The rest is the same as in Example 1, and will not be repeated here.

[0090] Example 6

[0091] Unlike Example 1, in step 3) of this example, after stirring and mixing, 3% of boron nitride by mass of the total solution is added.

[0092] The rest is the same as in Example 1, and will not be repeated here.

[0093] Example 7

[0094] Unlike Example 1, in step 3) of this example, after stirring and mixing, a composition of povidone and boric acid accounting for 3% of the total mass of the solution is added, wherein the mass ratio of povidone to boric acid is 2:1.

[0095] The rest is the same as in Example 1, and will not be repeated here.

[0096] Example 8

[0097] Unlike Example 1, in step 3) of this example, after stirring and mixing, a polydopamine and ethyl acetate composition accounting for 3% of the total mass of the solution is added, wherein the mass ratio of polydopamine to ethyl acetate is 2:1.

[0098] The rest is the same as in Example 1, and will not be repeated here.

[0099] Example 9

[0100] Unlike Example 1, in step 3) of this example, after stirring and mixing, a thiol-based compound accounting for 3% of the total mass of the solution is added. The thiol-based compound is mercaptoacetic acid.

[0101] The rest is the same as in Example 1, and will not be repeated here.

[0102] Example 10

[0103] Unlike Example 1, in step 3) of this example, after stirring and mixing, a polythiophene and polypyrrolidone composition accounting for 3% of the total mass of the solution is added, wherein the mass ratio of polythiophene to polypyrrolidone is 2:1.

[0104] The rest is the same as in Example 1, and will not be repeated here.

[0105] Example 11

[0106] Unlike Example 1, in step 4) of this example, during the ultrasonic treatment process, a polyoxyethylene surfactant accounting for 3% of the total mass of the solution is added.

[0107] The rest is the same as in Example 1, and will not be repeated here.

[0108] Example 12

[0109] Unlike Example 1, in step 4) of this example, the ultrasonic treatment process also includes introducing an inert gas into the mixture being treated using a bubbler.

[0110] The rest is the same as in Example 1, and will not be repeated here.

[0111] Comparative Example 1

[0112] Unlike Example 1, sodium bicarbonate is not added in step 1) of this comparative example.

[0113] The rest is the same as in Example 1, and will not be repeated here.

[0114] Comparative Example 2

[0115] Unlike Example 1, in step 3) of this comparative example, polyurea-modified α-cyanoacrylate is not added.

[0116] The rest is the same as in Example 1, and will not be repeated here.

[0117] Comparative Example 3

[0118] Unlike Example 1, methyl acetate is not added in step 3) of this comparative example.

[0119] The rest is the same as in Example 1, and will not be repeated here.

[0120] The composite conductive agent slurries prepared in Examples 1-12 and Comparative Examples 1-3 were respectively used to make negative electrode sheets and lithium-ion batteries, and their electrochemical performance was tested. The test results are shown in Table 1.

[0121] The method for determining the stability of conductive paste is as follows: the conductive paste is placed at room temperature, and the presence of agglomeration is observed visually, with the time recorded.

[0122] Method for determining the resistivity of slurry electrode: The four-probe method described in DB13 / T 5026.3-2019 is used for detection.

[0123] Table 1

[0124]

[0125] As can be seen from the test results in the table above, the composite conductive agent slurry prepared in this application has high conductivity, and the conductive slurry can be stored at room temperature for more than 3 months. The conductive slurry has good stability, and the heat dissipation performance and high-temperature cycling performance of the electrode and battery made using the composite conductive agent slurry of this application are effectively improved.

[0126] Comparative Examples 1 and 1-3 show that adding sodium bicarbonate can effectively improve the heat dissipation performance of the electrode. This is because the decomposition of sodium bicarbonate at high temperatures allows sodium borosilicate to form a porous composite thermally conductive material, thus giving the electrode excellent thermal conductivity and heat dissipation. Adding polyurea-modified α-cyanoacrylate improves the stability of the conductive paste, as its presence helps reduce the deposition, separation, or agglomeration of the dispersed phase in the paste. Adding methyl acetate effectively enhances the stability and thermal conductivity of the conductive paste. This is because the mixture decomposes during stirring, generating bubbles. As these bubbles rise, they further improve the dispersion of the mixture and allow the conductive paste to form a porous structure, further improving heat dissipation. Furthermore, it acts as a dispersant, effectively dispersing the conductive paste and stabilizing the carbon nanotube dispersion.

[0127] Comparing Examples 1 and 3-5, it is evident that the stability of the conductive paste can be effectively improved by further adding sodium sulfate stabilizer, nano-silica, nano-titanium oxide, and a tannic acid composition. In particular, the stability and conductivity of the conductive paste are even more superior when the nano-titanium oxide and tannic acid composition is added.

[0128] As can be seen from the comparison between Example 1 and Example 6, the electrical and thermal conductivity of the electrode can be further improved by adding boron nitride.

[0129] Comparing Examples 1 and 7-11, it is evident that further addition of a polyvinylpyrrolidone and boric acid composition, a polydopamine and ethyl acetate composition, mercaptoacetic acid, a polythiophene and polypyrrolidone composition, and a polyoxyethylene surfactant can further enhance the stability of the conductive paste and improve the electrical conductivity or thermal conductivity of the electrode. In particular, the improvement in overall performance is even more pronounced when adding the polyvinylpyrrolidone and boric acid composition, mercaptoacetic acid, and the polythiophene and polypyrrolidone composition. This indicates that the addition of these substances allows for better interaction with the carbon nanotubes in the conductive paste, thereby effectively improving the dispersion and thermal stability of the carbon nanotubes.

[0130] As can be seen from the comparison between Example 1 and Example 12, during the ultrasonic treatment process, the use of a bubbler to introduce inert gas into the mixture being treated can further break up some of the aggregates in the mixture, achieve a better dispersion effect, and keep the conductive paste stable.

[0131] Based on the disclosure and teachings of the foregoing specification, those skilled in the art can make changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments described above, and any obvious improvements, substitutions, or modifications made by those skilled in the art based on the present invention are within the scope of protection of the present invention. Furthermore, although some specific terms are used in this specification, these terms are only for convenience of explanation and do not constitute any limitation on the present invention.

Claims

1. A method for preparing a composite conductive agent slurry, characterized in that, Includes the following steps: 1) Stir the mixed solution of sodium borate and sodium silicate magnetically at 75-85℃, then add sodium bicarbonate and continue stirring to obtain a composite solution; 2) Cool the composite solution from step 1) and then place it in a high-temperature furnace. Heat it at 400-500℃ for 2-4 hours under a nitrogen or argon atmosphere to obtain a porous sodium borosilicate composite thermal conductive material. 3) Add single-walled carbon nanotubes, porous sodium borosilicate composite thermal conductive material and graphene to a solution containing polyvinyl alcohol at a mass ratio of 10:(2~4):(3~6). After stirring and mixing, add polyurea-modified α-cyanoacrylate. Mix the mixture with methyl acetate at a mass ratio of (94~97):(3~6) to obtain the primary solution of composite conductive agent slurry. 4) The primary solution from step 3) is subjected to ultrasonic treatment at a power of 200-300W and an oscillation frequency of 20-40kHz in a water bath at 85-90℃ for 30-60 minutes, and then subjected to vacuum degassing to obtain the composite conductive agent slurry.

2. The method of claim 1, wherein the composite conductive agent slurry is prepared by mixing the conductive agent, the binder, and the solvent. In step 1), the mass ratio of sodium borate, sodium silicate, and sodium bicarbonate is 10:(5-8):

2.

3. The method of claim 1, wherein the composite conductive agent slurry is prepared by mixing the conductive agent, the binder, and the solvent. In step 4), the vacuum degassing process is as follows: the slurry is placed in a vacuum chamber, the vacuum degree is controlled at -0.08 to -0.15 MPa, and the holding time is 10-20 minutes.

4. The method of claim 1 to 3, wherein the composite conductive agent slurry is prepared by adding the conductive agent to the solvent and then adding the binder to the mixture. In step 3), after stirring and mixing, sodium sulfate stabilizer accounting for 2-4% of the total mass of the solution is added.

5. The method of claim 1 to 3, wherein the composite conductive agent slurry is prepared by adding the conductive agent to the solvent and then adding the binder to the mixture. In step 3), after stirring and mixing, a nano-titanium oxide and tannic acid composition accounting for 1-5% of the total mass of the solution is added, wherein the mass ratio of nano-titanium oxide and tannic acid is (1-2):

1.

6. The method of claim 1 to 3, wherein the composite conductive agent slurry is prepared by adding the conductive agent to the solvent and then adding the binder to the mixture. In step 3), after stirring and mixing, a composition of povidone and boric acid, accounting for 1-5% of the total mass of the solution, is added, wherein the mass ratio of povidone to boric acid is (1-2):

1.

7. The method of claim 1 to 3, wherein the composite conductive agent slurry is prepared by adding the conductive agent to the solvent and then adding the binder to the mixture. In step 4), the ultrasonic treatment process also includes adding 1-5% of a polyoxyethylene surfactant by mass of the total solution.

8. The method for preparing the composite conductive agent slurry according to claim 1, characterized in that, In step 3), the mass ratio of polyvinyl alcohol and polyurea-modified α-cyanoacrylate is (1-2):

1.

9. The method for preparing the composite conductive agent slurry according to any one of claims 1 to 8, characterized in that, The synthesis of the polyurea-modified α-cyanoacrylate includes the following steps: 1) Dissolve polyurea and methacrylate in anhydrous ethanol at a mass ratio of 1.2:1 to form a solution with a reaction concentration of 45%; 2) Place the solution into the reactor and stir at 70-80℃ for 2-4 hours; 3) After the reaction is complete, cool the reaction solution to room temperature; 4) By vacuum freeze drying, the vacuum degree is first adjusted to 0.05~0.1MPa, and then the temperature is controlled at -40~-45℃ to remove the solvent, so as to obtain polyurea modified α-cyanoacrylate.

10. A composite conductive agent slurry, characterized in that: It is prepared by the method of any one of claims 1 to 9 for the preparation of composite conductive agent slurry.

Citation Information

Patent Citations

  • Far infrared heat-radiation ceramic slurry, fiber cloth, thin film and preparation methods thereof

    CN103570360A

  • Hydrophilic nano onion carbon conductive paste and preparation method and application thereof

    CN116525311A