Adhesive and preparation method thereof, composite insulating paper
By using epoxy resin as an adhesive, the problem of poor oil resistance of traditional polyurethane is solved, and the oil resistance and adhesion of composite insulating paper are improved. It is suitable for oil-cooled motor environments and ensures the stable operation of the motor.
Patent Information
- Application Number
- CN202210646985.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-09
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-06-09
AI Technical Summary
The NHN insulation paper used in traditional new energy vehicles has poor oil resistance as the adhesive polyurethane in oil-cooled motors, causing the insulation paper to dissolve in the oil and affecting the normal operation of the motor.
Epoxy resin is used as the main material of the adhesive, and is bonded with an overlapping structure of fiber paper and resin film to form a composite insulating paper with high oil resistance and cohesive strength.
The oil resistance of the composite insulating paper is improved, preventing stratification in oil, ensuring stable operation of the motor, and is suitable for oil-cooled motor environments.
Smart Images

Figure CN117247755B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer materials, and in particular to an adhesive and a preparation method thereof, and composite insulating paper. Background Art
[0002] At present, insulating paper is commonly used for slot insulation, inter-turn and inter-layer insulation, and gasket insulation of motors, and is a key insulating material in motor boxes. Traditional new energy vehicles usually use water-cooled motors, and the commercially available NHN insulating paper can meet the use requirements (where N is NOMEX paper, H represents polyimide film, and polyurethane glue is used to bond the layers). However, with the development of the new energy vehicle industry, oil-cooled motors have gradually replaced water-cooled motors. The adhesive polyurethane in the above NHN insulating paper has poor oil resistance and is very easy to swell in oil or even dissolve in oil, causing the NHN insulating paper to delaminate, affecting the normal operation of the motor. Summary of the invention
[0003] In view of this, the present application provides an adhesive and a preparation method thereof, and a composite insulating paper. The main material of the adhesive is epoxy resin, and the above adhesive is used to bond adjacent composite insulating paper layers to improve the oil resistance of the composite insulating paper, thereby providing a composite insulating paper suitable for oil-cooled motors.
[0004] The first aspect of the present application provides an adhesive, which includes the following raw materials in parts by weight: 25-60 parts of a first curing agent, 0.1-1 parts of an accelerator, 30-550 parts of a solvent, and 100 parts of an epoxy resin; wherein the crosslinking degree of the epoxy resin is 10%-40%.
[0005] Compared with the traditional adhesive for insulating paper - polyurethane, the above adhesive has better oil resistance and can prevent the occurrence of delamination caused by the insulating paper being immersed in oil for a long time.
[0006] Optionally, the viscosity of the adhesive at 25° C. is in the range of 500 mPa·s-5000 mPa·s. Preferably, the viscosity of the adhesive at 25° C. is in the range of 1000 mPa·s-3000 mPa·s.
[0007] Optionally, the epoxy resin includes a modified or unmodified epoxy resin; the unmodified epoxy resin includes at least one of bisphenol A epoxy resin and bisphenol F epoxy resin.
[0008] Optionally, the modified epoxy resin includes at least one of a dimer acid-modified epoxy resin, a phenoxy resin-modified epoxy resin and a rubber-modified epoxy resin.
[0009] Optionally, the first curing agent includes an anhydride curing agent.
[0010] Optionally, the anhydride curing agent includes at least one of phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride and methylnadic anhydride.
[0011] Preferably, the anhydride curing agent includes at least one of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride and methylnadic anhydride.
[0012] Optionally, the ratio of the epoxy equivalent of the epoxy resin to the active hydrogen equivalent of the first curing agent is 1:(0.6-0.9). Preferably, the ratio of the epoxy equivalent of the epoxy resin to the active hydrogen equivalent of the first curing agent is 1:(0.7-0.8).
[0013] Optionally, the solvent comprises at least one of ethyl acetate and butyl acetate. Preferably, the solvent is ethyl acetate.
[0014] Optionally, the accelerator includes at least one of a tertiary amine accelerator, an imidazole curing agent and a dicyandiamide accelerator.
[0015] Preferably, the accelerator comprises a tertiary amine accelerator. Further preferably, the accelerator is 2,4,6-tris(dimethylaminomethyl)phenol.
[0016] The second aspect of the present application provides a method for preparing an adhesive, comprising the following steps:
[0017] (1) adding a second curing agent to the epoxy resin, and heating the epoxy resin to obtain an epoxy resin having a crosslinking degree of 10% to 40%;
[0018] (2) The epoxy resin having a crosslinking degree of 10%-40% is uniformly mixed with a first curing agent, an accelerator and a solvent to obtain an adhesive; the adhesive comprises the following raw materials in parts by weight: 25-60 parts of a first curing agent, 0.1-1 parts of an accelerator, 30-550 parts of a solvent, and 100 parts of an epoxy resin.
[0019] The preparation method has simple process and strong controllability and is suitable for large-scale industrial production.
[0020] Optionally, step (1) further comprises adding a solvent to the epoxy resin.
[0021] Optionally, the second curing agent includes a polyamine curing agent or an acid anhydride curing agent. Preferably, the second curing agent is a polyamine curing agent. Further preferably, the second curing agent is an alicyclic amine curing agent.
[0022] Optionally, the polyamine curing agent includes at least one of isophorone diamine, methylcyclohexylamine, 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, menthane diamine, N-aminohexylpiperazine, divinyltriamine, methylenebiscyclohexylamine and dimethylaminopropylamine; the acid anhydride curing agent includes at least one of phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride and methylnadic anhydride.
[0023] A third aspect of the present application provides a composite insulating paper, which includes fiber paper and resin film arranged in overlapping layers; wherein the fiber paper and the resin film are bonded by a cured product of the adhesive provided in the first aspect of the present application.
[0024] Optionally, the fiber paper includes at least one of polyaramid fiber paper, polyester fiber paper, polysulfone amide fiber paper and inorganic fiber paper.
[0025] Optionally, the resin film includes at least one of a polyimide film, a polybutylene terephthalate film, a polybutylene naphthalate film and a polyphenylene sulfide film. Preferably, the resin film includes at least one of a polybutylene naphthalate film and a polyphenylene sulfide film.
[0026] Optionally, the composite insulating paper includes a first fiber paper, a resin film and a first fiber paper which are stacked in sequence. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a morphological photograph of the composite insulating paper prepared in Example 1 of the present application after the oil resistance test;
[0028] Figure 2 This is a morphology photo of the composite insulating paper prepared in Comparative Example 1 after oil resistance test;
[0029] Figure 3 This is a photo of the morphology of the composite insulating paper prepared in Example 2 after the oil resistance test;
[0030] Figure 4 This is a morphology photo of the composite insulating paper prepared in Comparative Example 3 after oil resistance test;
[0031] Figure 5 This is a photograph of the morphology of the composite insulating paper prepared in Example 4 after the oil resistance test. DETAILED DESCRIPTION
[0032] The technical solution of this application is described in detail below.
[0033] Generally, the composite insulating paper commonly used in the market is a three-layer structure of fiber paper-resin film-fiber paper, and polyurethane is often used as an interlayer adhesive. However, polyurethane has a weak polarity and is similarly miscible with oil. Long-term oil immersion will cause polyurethane to swell or even dissolve, resulting in the composite insulating paper being delaminated. To solve the above problem, an embodiment of the present application provides an adhesive.
[0034] Specifically, the adhesive provided in the embodiment of the present application includes the following raw materials in parts by weight: 25-60 parts of a first curing agent, 0.1-1 parts of an accelerator, 30-550 parts of a solvent, and 100 parts of an epoxy resin; wherein the crosslinking degree of the epoxy resin is 10%-40%.
[0035] The epoxy resin in the adhesive is an epoxy resin with a cross-linking degree of 10%-40%, so that the adhesive has a suitable cohesive strength. In the preparation process of composite insulating paper, some resin films, fiber papers, and adhesives will undergo multiple hot roller pressings. In this process, the adhesive with suitable cohesive strength can penetrate into the porous structure of the fiber paper under the action of high temperature and pressure, achieve preliminary bonding before curing, and make the initial bonding between the fiber paper and the resin film better, preventing the two from stratifying during the subsequent rolling process. At the same time, it can also avoid the adhesive dripping during the coating process, or escaping from the fiber paper and the resin film during the composite process, affecting the subsequent production. In addition, the reaction heat of the pre-cross-linked epoxy resin in the subsequent curing process will be significantly reduced, which will reduce the shrinkage caused by the intense curing heat release of the epoxy resin, thereby making the surface flatness of the composite insulating paper higher.
[0036] The above-mentioned adhesive is mainly made of epoxy resin, which has a large polarity and does not contain an ester group. After curing, the epoxy resin forms a three-dimensional insoluble and infusible polymer network with better oil resistance. It will not swell or dissolve during the oil immersion process, thereby ensuring that the composite insulating paper can maintain its intact structure during long-term oil immersion and stably play its role.
[0037] In some embodiments of the present application, the crosslinking degree of the epoxy resin may be in the range of 10%-30%. In other embodiments, the crosslinking degree of the epoxy resin may be in the range of 20%-40%. In some other embodiments, the crosslinking degree of the epoxy resin may be in the range of 20%-30%. Exemplarily, the crosslinking degree of the epoxy resin may be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, etc.
[0038] In some embodiments of the present application, the epoxy resin includes a modified or unmodified epoxy resin. Among them, the unmodified epoxy resin includes at least one of bisphenol A epoxy resin and bisphenol F epoxy resin; the modified epoxy resin includes at least one of dimer acid modified epoxy resin, phenoxy resin modified epoxy resin and rubber modified epoxy resin. After curing, the above epoxy resin has good electrical insulation performance and corrosion resistance, and its cured product has high strength and bonding strength, and also has certain toughness and heat resistance. Among them, the toughness of the cured products of dimer acid modified epoxy resin, phenoxy resin modified epoxy resin and rubber modified epoxy resin is relatively better, and can be selected according to actual production needs.
[0039] In some embodiments of the present application, the first curing agent includes anhydride curing agent, and the anhydride curing agent includes at least one of phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride and methylnadic anhydride. In some specific embodiments, the first curing agent includes at least one of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride and methylnadic anhydride. The above-mentioned anhydride curing agent has excellent electrical properties (mainly referring to insulation performance), which is conducive to further improving the insulation of the above-mentioned epoxy resin cured product, so as to ensure that the insulation performance of the composite insulating paper is better. In addition, the curing rate of the anhydride curing agent is more suitable, which can provide a longer processing window for the preparation of composite insulating paper, is more conducive to the operation of production workers, and is conducive to ensuring that the quality of composite insulating paper is higher.
[0040] In some embodiments of the present application, the ratio of the epoxy equivalent of the epoxy resin to the active hydrogen equivalent of the first curing agent is 1: (0.6-0.9). In some specific embodiments, the ratio of the epoxy equivalent of the epoxy resin to the active hydrogen equivalent of the first curing agent can be 1: (0.7-0.8). Exemplarily, the ratio of the epoxy equivalent of the epoxy resin to the active hydrogen equivalent of the first curing agent can be 1: 0.6, 1: 065, 1: 0.7, 1: 0.75, 1: 0.8, 1: 0.85, 1: 0.9, etc. The ratio of the epoxy equivalent of the epoxy resin to the active hydrogen equivalent of the first curing agent can be controlled by adjusting the content of the first curing agent in the adhesive. The appropriate ratio between the two is conducive to ensuring that the crosslinking degree of the cured epoxy resin can meet the product requirements, thereby ensuring the bonding force and mechanical properties of the adhesive cured product, and then ensuring the high quality of the composite insulating paper. In addition, it can also avoid the waste caused by excessive first curing agent.
[0041] In some embodiments of the present application, the accelerator includes but is not limited to at least one of a tertiary amine accelerator, an imidazole curing agent and a dicyandiamide accelerator. In some specific embodiments, the accelerator includes a tertiary amine accelerator. Exemplarily, the tertiary amine accelerator can be triethanolamine, dimethylaniline, 2,4,6-tris(dimethylaminomethyl)phenol, etc. In some specific embodiments, the accelerator is 2,4,6-tris(dimethylaminomethyl)phenol. Tertiary amine accelerators are nucleophilic accelerators that can simultaneously catalyze epoxy resin and anhydride (first curing agent), which is beneficial to improving the production efficiency of composite insulating paper.
[0042] In some embodiments of the present application, the solvent includes but is not limited to at least one of ethyl acetate and butyl acetate. In some specific embodiments, the solvent is ethyl acetate. Ethyl acetate and butyl acetate are both good solvents for epoxy resins. The volatilization rates of the two are relatively fast, especially the volatilization rate of ethyl acetate is relatively faster, and it is easy to be removed from the system during the baking process, which is beneficial to improving the production efficiency and product quality of composite insulating paper.
[0043] In some embodiments of the present application, the viscosity of the adhesive at 25°C is in the range of 500mPa·s-5000mPa·s. In some specific embodiments, the viscosity of the above-mentioned adhesive at 25°C is in the range of 1000mPa·s-3000mPa·s. Exemplarily, the viscosity of the above-mentioned adhesive at 25°C can be 500mPa·s, 1000mPa·s, 1500mPa·s, 2000mPa·s, 2500mPa·s, 3000mPa·s, 3500mPa·s, 4000mPa·s, 4500mPa·s, 5000mPa·s, etc. The viscosity of the adhesive can be adjusted by adjusting the content of the solvent in the adhesive so that the adhesive has suitable fluidity, which is conducive to the application of the adhesive.
[0044] The present application also provides a method for preparing an adhesive, comprising the following steps:
[0045] (1) adding a second curing agent to the epoxy resin, and heating the epoxy resin to obtain an epoxy resin having a crosslinking degree of 10% to 40%;
[0046] (2) The epoxy resin having a crosslinking degree of 10%-40% is uniformly mixed with a first curing agent, an accelerator and a solvent to obtain an adhesive; the adhesive comprises the following raw materials in parts by weight: 25-60 parts of a first curing agent, 0.1-1 parts of an accelerator, 30-550 parts of a solvent, and 100 parts of an epoxy resin.
[0047] The above-mentioned second curing agent with multifunctional groups can cause the epoxy group to undergo ring-opening copolymerization, and the polymerization degree of the low molecular weight epoxy resin can be controlled by controlling the reaction time or the amount of the second curing agent to form a certain three-dimensional infusible and insoluble polymer network (i.e., having a certain degree of crosslinking) so that it has a suitable cohesive strength. In addition, pre-crosslinking the epoxy resin first can control the degree of pre-crosslinking of the epoxy resin, so that the adhesive has a good cohesive strength, which is conducive to the application of the adhesive.
[0048] The preparation method has simple process and strong controllability and is suitable for large-scale industrial production.
[0049] In some cases, in step (1), the amount of the second curing agent is first calculated, and a certain amount of the second curing agent is added to the epoxy resin while stirring, and then heated until the second curing agent reacts completely to obtain an epoxy resin with a crosslinking degree of 10%-40%. The above-mentioned epoxy resin with a crosslinking degree of 10%-40% means that 10%-40% of the epoxy groups in the epoxy resin are reacted by the second curing agent. The amount of the second curing agent is calculated by the following formula:
[0050] M2 = (M1 / Eq) × preset crosslinking degree × AEW
[0051] Wherein, M1 is the mass of epoxy resin, M2 is the amount of the second curing agent, both in g; Eq is the epoxy equivalent of epoxy resin, in g / equivalent; AEW is the active hydrogen equivalent of the second curing agent.
[0052] In some embodiments of the present application, the second curing agent includes but is not limited to polyamine curing agents. In some specific embodiments, the second curing agent can be an alicyclic amine curing agent. Exemplarily, the above-mentioned polyamine curing agent includes but is not limited to at least one of isophorone diamine, methylcyclohexylamine, 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, menthane diamine and N-aminohexyl piperazine, divinyltriamine, methylenebiscyclohexaneamine and dimethylaminopropylamine. The curing rate of polyamine curing agents is relatively fast and the curing temperature is relatively low, which is conducive to improving production efficiency and shortening process cycles. Further, alicyclic amine curing agents can be cured at medium and low temperatures (generally, below room temperature is low temperature curing, room temperature to 50°C is room temperature curing, and 50°C-100°C is medium temperature curing), and it has good temperature resistance. At this time, in step (1), it is necessary to ensure that the second curing agent reacts completely, that is, it is necessary to control the crosslinking degree of the epoxy resin by controlling the amount of the second curing agent added to avoid reaction between the polyamine curing agent and the anhydride curing agent.
[0053] In some other embodiments of the present application, the second curing agent includes but is not limited to anhydride curing agents. The anhydride curing agents include but are not limited to at least one of phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride and methylnadic anhydride. Anhydride curing agents have good insulation properties. The first curing agent and the second curing agent are both anhydride curing agents. At this time, the insulation properties of the adhesive cured product can be further enhanced, and the reaction between the first curing agent and the second curing agent can also be avoided. At this time, in step (1), the crosslinking degree of the epoxy resin can also be controlled by controlling the degree of reaction.
[0054] In the present application, the heating temperature in step (1) can be determined according to the specific type of the second curing agent used.
[0055] In some embodiments of the present application, step (1) further includes adding a solvent to the epoxy resin. Exemplarily, the solvent includes at least one of ethyl acetate and butyl acetate. An appropriate solvent can play a diluting role to avoid the epoxy resin with a crosslinking degree of 10%-40% obtained after the crosslinking reaction from having too high a viscosity, which is not conducive to stirring and transfer.
[0056] The embodiment of the present application further provides a composite insulating paper, which includes fiber paper and resin film arranged in overlapping layers; wherein the fiber paper and the resin film are bonded by a cured product of the adhesive provided in the embodiment of the present application.
[0057] The composite insulating paper has excellent insulating properties and good oil resistance, and can maintain a complete structure during long-term oil immersion, stably play its role, and can be used to provide oil-cooled motors. In addition, the composite insulating paper has high surface flatness.
[0058] In the present application, the above-mentioned overlapping fiber paper A and resin film B refer to multiple layers of fiber paper A and resin film B stacked in sequence, and the resin film B is located between two layers of fiber paper A. Exemplarily, the structure of the composite insulating paper can be AB, ABA, ABABA, etc.
[0059] In some embodiments of the present application, the composite insulating paper includes but is not limited to a first fiber paper, a resin film and a first fiber paper stacked in sequence.
[0060] In some embodiments of the present application, the fiber paper includes but is not limited to at least one of polyaramid fiber paper, polyester fiber paper, polysulfone fiber paper and inorganic fiber paper. The materials of each layer of fiber paper may be the same or different. The above fiber papers are all commercially available products, such as Nomex series products of DuPont and TufQUIN series products of 3M. The above types of fiber papers have good insulation performance and temperature resistance, which can ensure that the quality of the prepared composite insulation paper is high.
[0061] In some embodiments of the present application, the resin film includes but is not limited to at least one of a polyimide film, a polybutylene terephthalate film, a polybutylene naphthalate film and a polyphenylene sulfide film. In some specific embodiments, the resin film includes at least one of a polybutylene naphthalate film and a polyphenylene sulfide film. The materials of each layer of resin film may be the same or different. The above-mentioned types of fiber paper have good insulation, heat resistance and oil resistance, among which polybutylene naphthalate film and polyphenylene sulfide film have better heat resistance and oil resistance. The use of the above-mentioned types of resin films can ensure that the obtained composite insulating paper is of high quality and can be immersed in oil for a long time without stratification.
[0062] In some cases, the composite insulating paper provided in the embodiments of the present application can be prepared by the following steps:
[0063] (1) applying an adhesive to the upper and lower surfaces of a resin film, and removing the solvent in the adhesive after baking;
[0064] (2) The fiber paper is pressed onto the upper and lower surfaces of the resin film by rollers, and the adhesive is cured by heating to obtain the composite fiber paper provided in the embodiment of the present application;
[0065] The curing temperature can be determined according to the type of the first curing agent selected.
[0066] The preparation method has simple process and high production efficiency.
[0067] Example 1
[0068] In 100 parts by weight of rubber-modified epoxy resin (rubber content 40%), 50 parts by weight of ethyl acetate was added for dilution, and then 2.5 parts by weight of the second curing agent - isophorone diamine was added under stirring, and then heated to 80°C and stirred until the reaction was complete to obtain an epoxy resin with a crosslinking degree of 20% diluted with ethyl acetate. Then, according to 100 parts by weight of epoxy resin with a crosslinking degree of 20%, 37.9 parts by weight of the first curing agent - methyltetrahydrophthalic anhydride, 0.25 parts by weight of the accelerator - 2,4,6-tris (dimethylaminomethyl) phenol, and 138 parts by weight of ethyl acetate, the other components were added in sequence and stirred evenly to obtain the adhesive provided in Example 1 of the present application.
[0069] Use a dry laminating machine to dip-coat the above-mentioned adhesive on both sides of the polyethylene naphthalate film, dry it in a three-section oven at 75°C, 85°C, and 75°C, respectively, and press and laminate two sheets of polyaramid fiber paper on both sides of the dried polyethylene naphthalate film coated with the adhesive, then roll it up, and then cure it at 80°C for 12h, 110°C for 6h, and 150°C for 2h to obtain the composite insulating paper S1 provided in the embodiment of the present application.
[0070] Example 2
[0071] The difference from Example 1 is that 50 parts by weight of ethyl acetate are added to 100 parts by weight of rubber-modified epoxy resin (rubber content 40%) for dilution, and then 1.25 parts by weight of the second curing agent, isophorone diamine, is added under stirring, and then heated to 80° C. and stirred until the reaction is complete, to obtain an ethyl acetate-diluted epoxy resin with a crosslinking degree of 10%.
[0072] Then, according to 100 parts by weight of an epoxy resin with a crosslinking degree of 10%, 42.64 parts of a first curing agent - methyltetrahydrophthalic anhydride, 1 part of an accelerator - 2,4,6-tris(dimethylaminomethyl)phenol, and 35 parts of ethyl acetate, other components are added in sequence and stirred evenly to obtain the adhesive provided in the embodiment of the present application.
[0073] The prepared composite insulating paper is recorded as S2.
[0074] Example 3
[0075] The difference from Example 1 is that 50 parts by weight of ethyl acetate are added to 100 parts by weight of rubber-modified epoxy resin (rubber content 40%) for dilution, and then 3.75 parts by weight of the second curing agent, isophorone diamine, are added under stirring, and then heated to 80° C. and stirred until the reaction is complete, to obtain an ethyl acetate-diluted epoxy resin with a crosslinking degree of 30%.
[0076] Then, according to 100 parts by weight of 30% cross-linking epoxy resin, 33.163 parts by weight of the first curing agent - methyltetrahydrophthalic anhydride, 0.25 parts by weight of accelerator - 2,4,6-tris (dimethylaminomethyl) phenol, and 260 parts by weight of solvent - ethyl acetate, other components are added in sequence and stirred evenly to obtain the adhesive for composite insulating paper.
[0077] Use a dry laminating machine to dip-coat the above-mentioned adhesive onto both sides of the polyethylene naphthalate film, and dry it in a three-section oven for about 1 minute at drying temperatures of 75°C, 85°C, and 75°C, respectively. After drying, press and laminate it with polyaramid fiber paper, then roll it up, and then cure it at 80°C for 12 hours, 110°C for 6 hours, and 150°C for 2 hours to obtain the composite insulating paper S3 provided in the embodiment of the present application.
[0078] Example 4
[0079] The difference from Example 1 is: The difference from Example 1 is: 50 parts by weight of ethyl acetate are added to 100 parts by weight of rubber-modified epoxy resin (rubber content 40%) for dilution, and then 5 parts by weight of the second curing agent, isophorone diamine, are added under stirring, and then heated to 80°C and stirred until the reaction is complete to obtain an ethyl acetate-diluted epoxy resin with a crosslinking degree of 40%.
[0080] Then, 100 parts by weight of epoxy resin with a crosslinking degree of 40%, 28.4 parts of the first curing agent - methyltetrahydrophthalic anhydride, 0.1 parts of the accelerator - 2,4,6-tris (dimethylaminomethyl) phenol, 510 parts of ethyl acetate, and other components are added in sequence and stirred evenly to obtain the adhesive provided in the embodiment of the present application. The obtained composite insulating paper is recorded as S4.
[0081] In order to highlight the beneficial effects of the embodiments of the present application, the following comparative examples are provided.
[0082] Comparative Example 1
[0083] 100 parts by weight of LOCTITE LIOFOL LA 2681 (polyester polyol, component A of polyurethane glue) and 61.43 parts by weight of ethyl acetate were mixed evenly, and then 10 parts by weight of LOCTITE LIOFOL LA5500 (isocyanate, component B of polyurethane glue) were added and stirred to mix evenly to obtain an adhesive.
[0084] Use a dry laminating machine to dip-coat the adhesive on both sides of the polyimide film and dry it in three ovens at temperatures of 60°C, 70°C, and 60°C. After drying, press two sheets of polyaramid fiber paper at 60°C and laminate them on both sides of the dried polyimide film coated with the adhesive. Then roll them up and cure them at 60°C for 3 days to obtain composite insulating paper DS1.
[0085] Comparative Example 2
[0086] The difference from Example 1 is that the epoxy resin in the adhesive is an uncrosslinked epoxy resin. The adhesive contains the following raw materials in parts by weight: 100 parts of uncrosslinked epoxy resin, 47.4 parts of methyltetrahydrophthalic anhydride, 0.25 parts of 2,4,6-tris(dimethylaminomethyl)phenol, and 138 parts of ethyl acetate. The other components are added in sequence and stirred evenly to obtain the adhesive.
[0087] Use a dry laminating machine to dip-coat the above adhesive on both sides of the polyethylene naphthalate film, dry it in a three-section oven at 75°C, 85°C, and 75°C, respectively, and press and laminate two polyaramid fiber papers on both sides of the dried polyethylene naphthalate film coated with the adhesive, then roll it up and cure it at 80°C for 12h, 110°C for 6h, and 150°C for 2h to obtain composite insulating paper DS2.
[0088] Comparative Example 3
[0089] In 100 parts by weight of rubber-modified epoxy resin (rubber content 40%), 50 parts by weight of ethyl acetate was added for dilution, and then 0.625 parts by weight of the second curing agent, isophorone diamine, was added under stirring, and then heated to 80°C and stirred until the reaction was complete to obtain an ethyl acetate-diluted epoxy resin with a crosslinking degree of 5%.
[0090] Then, according to 100 parts by weight of epoxy resin with a crosslinking degree of 5%, 45 parts by weight of the first curing agent - methyltetrahydrophthalic anhydride, 0.25 parts by weight of the accelerator - 2,4,6-tris (dimethylaminomethyl) phenol, and 138 parts by weight of ethyl acetate, other components are added in sequence and stirred evenly to obtain an adhesive.
[0091] Use a dry laminating machine to dip-coat the above adhesive on both sides of the polyethylene naphthalate film, dry it in a three-section oven at 75°C, 85°C, and 75°C, respectively, and press and laminate two polyaramid fiber papers on both sides of the dried polyethylene naphthalate film coated with the adhesive, then roll it up, and then cure it at 80°C for 12h, 110°C for 6h, and 150°C for 2h to obtain composite insulating paper DS3.
[0092] Comparative Example 4
[0093] 50 parts by weight of ethyl acetate was added to 100 parts by weight of rubber-modified epoxy resin (rubber content 40%) for dilution, and then 6.25 parts by weight of the second curing agent, isophorone diamine, was added under stirring, and then heated to 80°C and stirred until the reaction was complete to obtain an epoxy resin with a crosslinking degree of 50% diluted with ethyl acetate. Then, 100 parts by weight of epoxy resin with a crosslinking degree of 50%, 23.7 parts by weight of the first curing agent, methyltetrahydrophthalic anhydride, 0.25 parts by weight of accelerator, 2,4,6-tris(dimethylaminomethyl)phenol, and 138 parts by weight of ethyl acetate were added in sequence and stirred to obtain an adhesive.
[0094] Use a dry laminating machine to dip-coat the above adhesive on both sides of the polyethylene naphthalate film, dry it in a three-section oven at 75°C, 85°C, and 75°C, respectively, and press and laminate two polyaramid fiber papers on both sides of the dried polyethylene naphthalate film coated with the adhesive, then roll it up, and then cure it at 80°C for 12h, 110°C for 6h, and 150°C for 2h to obtain composite insulating paper DS4.
[0095] The properties of the composite insulating paper prepared in each embodiment and comparative example are tested below, and the preparation process of the composite insulating paper is observed:
[0096] (1) Test of the degree of crosslinking of epoxy resin: The pre-crosslinked epoxy resin used in each embodiment and the pre-crosslinked epoxy resin without solvent were respectively tested using a Fourier transform infrared tester using the attenuated total reflectance (ATR) method, and the 913 cm-1 of the two samples was read. -1 The peak area A of the characteristic peak near (epoxy group) EP Front, A EP Houhe 1610cm -1 The peak area A of the characteristic peak near (benzene ring group) BZ Front, A BZ After that, the cross-linking degree calculation formula is:
[0097] Crosslinking degree = 100% - (A EP后 / A BZ后 ) / (A EP前 / A BZ前 )
[0098] Among them, A EP Front, A BZ The former are the strength of epoxy group and benzene ring group in pre-crosslinked epoxy resin, A EP After, A BZ The strength of epoxy groups and benzene ring groups in the pre-crosslinked epoxy resin after solvent removal. The results are summarized in Table 1.
[0099] (2) Monitoring of glue dripping and overflowing: During the preparation of composite fiber paper, observe whether there is glue dripping after the adhesive is applied, before the sample enters the drying tunnel, and before the resin film is composited with the fiber paper; during the composite process of the fiber paper and the resin film, observe whether there is glue overflowing. The results are summarized in Table 2.
[0100] (3) Adhesion evaluation: Take the composite insulating paper prepared in each embodiment and comparative example, paste adhesive tape on both sides of the composite insulating paper, cut into 25 mm × 200 mm strip specimens, peel off the specimens at the ends, and then perform a peel strength test according to GB / T2792-2014 "Test method for peel strength of adhesive tape". Average peel strength <2N / 25mm is poor, 2N / 25mm≤average peel strength <6N / 25mm is medium, and average peel strength ≥6N / 25mm is good. The results are summarized in Table 2.
[0101] (4) Oil resistance test: The composite insulating paper samples (10 cm×10 cm) prepared in each embodiment and comparative example were immersed in a container containing polishing oil, and then subjected to high and low temperature tests: 40 h at 150°C and 8 h at -40°C as one cycle, and the test was repeated for 8 cycles. After the test, the appearance of the composite insulating paper samples was observed to see if they were intact, delaminated, or bubbling, and the results were recorded. The results are summarized in Table 2.
[0102] Table 1 Crosslinking degree test results of pre-crosslinked epoxy resin used in each embodiment
[0103] Experiment number Measured cross-linking degree Example 1 19.14% Example 2 10.26% Example 3 29.79% Example 4 40.87%
[0104] Table 2 Summary of test results of embodiments and comparative examples
[0105]
[0106]
[0107] It can be seen from the data in Table 1 that the adhesive provided in the embodiment of the present application has good adhesion, and no glue dripping or overflowing occurs during the application process. Figure 1 The morphology of composite insulating paper S1 after oil resistance test is shown in Figure 1. The results show that the S1 sample is intact, without delamination or bubbles. It can be seen that the composite insulating paper provided in the embodiment of the present application has excellent oil resistance and can maintain a complete structure even during long-term oil immersion.
[0108] In contrast, the composite insulating paper obtained by using the conventional adhesive in Comparative Example 1 exhibits overall delamination after oil immersion (see Figure 2). In the adhesives prepared in Comparative Examples 2 and 3, the epoxy resins therein were not pre-crosslinked or had a low crosslinking degree, and glue dripping and overflowing occurred during the application process, resulting in poor adhesion of the final composite insulating paper, and bubbles and delamination occurred in local areas after oil immersion (see Figure 3 and Figure 4 ). In the adhesive prepared in Comparative Example 4, the epoxy resin crosslinking degree is too large, resulting in too little initial bonding force of the adhesive to the fiber paper and the resin film. The quality of the composite insulating paper prepared is poor, and bubbles and delamination also appear in local areas after the oil resistance test (see Figure 5 ).
[0109] The above is an exemplary embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made thereto without departing from the principles of the present application. These improvements and modifications are also considered to be within the scope of protection of the present application.
Claims
1. An adhesive, It is characterized in that The adhesive comprises the following raw materials in parts by weight: 25-60 parts of a first curing agent, 0.1-1 parts of an accelerator, 30-550 parts of a solvent, and 100 parts of an epoxy resin; wherein the crosslinking degree of the epoxy resin is 10%-40%; the first curing agent comprises an anhydride curing agent; the ratio of the epoxy equivalent of the epoxy resin to the active hydrogen equivalent of the first curing agent is 1:(0.6-0.9); The epoxy resin includes modified or unmodified epoxy resin; the unmodified epoxy resin includes at least one of bisphenol A epoxy resin and bisphenol F epoxy resin; the modified epoxy resin includes at least one of dimer acid modified epoxy resin, phenoxy resin modified epoxy resin and rubber modified epoxy resin.
2. The adhesive according to claim 1, It is characterized in that The acid anhydride curing agent includes at least one of phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride and methylnadic anhydride.
3. The adhesive according to claim 1, It is characterized in that The accelerator includes at least one of a tertiary amine accelerator, an imidazole curing agent and an organic urea accelerator.
4. The adhesive according to claim 1, It is characterized in that The solvent includes at least one of ethyl acetate and butyl acetate.
5. A method for preparing an adhesive, It is characterized in that The following steps are involved: (1) adding a second curing agent to an epoxy resin, and obtaining an epoxy resin having a crosslinking degree of 10% to 40% by heating reaction; wherein the amount of the second curing agent is calculated by the following formula: 2 =(M 1 / Eq)×predetermined cross-linking degree×AEW; where M 1 is the mass of epoxy resin, M 2 is the dosage of the second curing agent, in g; Eq is the epoxy equivalent of the epoxy resin, in g / equivalent; AEW is the active hydrogen equivalent of the second curing agent; (2) The epoxy resin having a crosslinking degree of 10%-40% is uniformly mixed with a first curing agent, an accelerator and a solvent to obtain an adhesive; the adhesive comprises the following raw materials in parts by weight: 25-60 parts of a first curing agent, 0.1-1 parts of an accelerator, 30-550 parts of a solvent, and 100 parts of an epoxy resin.
6. The preparation method according to claim 5, It is characterized in that The second curing agent includes a polyamine curing agent or an acid anhydride curing agent; the polyamine curing agent includes at least one of isophorone diamine, methylcyclohexylamine, 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, menthane diamine, N-aminohexylpiperazine, divinyltriamine, methylenebiscyclohexylamine and dimethylaminopropylamine; the acid anhydride curing agent includes at least one of phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride and methylnadic anhydride.
7. A composite insulating paper, It is characterized in that The composite insulating paper comprises fiber paper and resin film which are overlapped in layers; wherein the fiber paper and the resin film are bonded by a cured product of the adhesive as described in any one of claims 1 to 4.
8. The composite insulating paper according to claim 7, It is characterized in that The fiber paper includes at least one of polyaramid fiber paper, polyester fiber paper, polysulfone amide fiber paper and inorganic fiber paper; the resin film includes at least one of polyimide film, polybutylene terephthalate film, polybutylene naphthalate film and polyphenylene sulfide film.
Citation Information
Patent Citations
Preparation method for epoxy-resin-combined modified vegetable-fiber insulation paper
CN105484103A
Injection moldable bismaleimide molding plastic and preparation method thereof
CN109575597A