An optoelectronic device that can be used in photodetectors and neuromorphic vision sensors, and its fabrication method.
By utilizing a GaN/Ga2O3/GaN dual heterojunction structure and controlling oxygen vacancies through bias voltage, the function switching between a photodetector and a neuromorphic vision sensor was achieved. This solved the problem that traditional devices struggle to balance fast light response and long-term photoconductivity, improving image recognition accuracy and reducing power consumption.
Patent Information
- Application Number
- CN202311180370.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-13
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-13
AI Technical Summary
Traditional photodetectors cannot achieve fast light response and long-term photoconductivity, making it difficult to meet the needs of photodetection and neuromorphic vision sensing in the same device.
By employing a GaN/Ga2O3/GaN double heterojunction structure, the photoresponse speed can be controlled by adjusting the ionization and deionization processes of oxygen vacancies in Ga2O3 and utilizing the bias voltage, thus switching the device's function.
This technology enables the conversion of the roles of photodetectors and neuromorphic vision sensors into a single device, improving the accuracy and efficiency of image recognition while reducing power consumption.
Smart Images

Figure CN117253939B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of optoelectronic device technology, and specifically refers to an optoelectronic device that can be used in photodetectors and neuromorphic vision sensors, and its preparation method. Background Technology
[0002] Photodetectors are indispensable key optoelectronic components in modern sensing, communication, and imaging systems. They can quickly and sensitively detect changes in light signals and convert them into digital signals for processing by computers or other digital devices. Photodetectors are characterized by fast light response and high sensitivity, thus having important applications in the field of optoelectronic imaging. Using photodetector arrays, weak light signals and moving objects can be quickly sensed and imaged. However, traditional photodetectors cannot memorize images, nor can they simulate the way the human visual system processes light signals.
[0003] Inspired by the human visual system, neuromorphic vision sensors are optoelectronic devices that process light information in a manner similar to the human eye, enabling the perception, memorization, and processing of light signals. Unlike traditional digital vision systems that convert the light intensity received by each pixel into digital values, neuromorphic vision sensors mimic the operation of neurons in the human brain. Therefore, they can not only achieve image noise reduction and contrast enhancement but also perform more adaptive image analysis and recognition. With the rapid development of bionic technology and intelligent manufacturing, neuromorphic vision sensors have become an indispensable part of the artificial intelligence era. However, the human retina cannot recognize continuous images at less than 24 frames per second (a refresh rate of approximately 40Hz). This makes it difficult for NVS (Near-Vision Sensor) to respond immediately to high-frequency light signals and quickly capture images. Therefore, if a photodetector and a neuromorphic vision sensor could be implemented on a single device and switched as needed, the integration of the device would be greatly improved, and the application range of optoelectronic devices would be broadened. However, photodetectors typically require a fast light response speed, while neuromorphic vision sensors require a long-term photoconductivity effect, i.e., a slower light response speed. Therefore, this contradiction in light response speed makes it very difficult to implement both types of devices on the same device. Summary of the Invention
[0004] To address the aforementioned problems, the present invention aims to provide an optoelectronic device and its fabrication method applicable to photodetectors and neuromorphic vision sensors. This device fabrication method is simple and its functionality can be switched according to requirements. As a photodetector, the device enables rapid optical imaging and optical communication. As a neuromorphic vision sensor, the device exhibits ultra-low power consumption and demonstrates excellent image sensing, memory, and neuromorphic preprocessing capabilities. Preprocessing images using a neuromorphic vision sensor significantly improves the accuracy and efficiency of image recognition.
[0005] To achieve the above objectives, the technical solution of the present invention is as follows:
[0006] An optoelectronic device applicable to photodetectors and neuromorphic vision sensors is disclosed. The device has a back-to-back GaN / Ga2O3 / GaN double heterojunction structure, consisting of a sapphire substrate with semi-cylindrical trenches, a GaN thin film with lath-shaped trenches, Ga2O3 nanowires, and a metal electrode from bottom to top. The GaN thin film is grown on the sapphire substrate, and lath-shaped trenches corresponding one-to-one with the semi-cylindrical trenches are formed on the GaN thin film. The Ga2O3 nanowires are grown on the sidewalls of the trenches in the GaN thin film, and the metal electrode is disposed on the GaN thin film without contacting the Ga2O3 nanowires.
[0007] The aforementioned optoelectronic device, which can be used in photodetectors and neuromorphic vision sensors, has a GaN thin film thickness of 500 nm to 5 μm, a trench depth of GaN thin film extending into the sapphire substrate to insulate the GaN thin films on both sides, a trench width between 5 and 50 μm, and a trench spacing of 1 to 5 mm.
[0008] The aforementioned optoelectronic device, which can be used in photodetectors and neuromorphic vision sensors, uses Ga2O3 nanowires to connect the GaN thin films on both sides of the GaN thin film trench in a bridging or through manner to form a conductive channel. The length of the Ga2O3 nanowires is between 5 and 100 μm.
[0009] The aforementioned optoelectronic device, which can be used in photodetectors and neuromorphic vision sensors, has Ti / Au or Cr / Au metal electrodes.
[0010] A method for fabricating an optoelectronic device that can be used in photodetectors and neuromorphic vision sensors includes the following steps:
[0011] Step 1: Cut grooves into the GaN thin film grown on sapphire;
[0012] Step 2: The Au catalyst is evaporated onto the sidewalls of the GaN trench using an electron beam.
[0013] Step 3: Place the metal Ga into a quartz boat with grooves, and place the GaN / sapphire with Au catalyst vertically in the grooves of the quartz boat, with the GaN film facing the metal Ga and at a certain distance from the metal Ga.
[0014] Step 4: Place the quartz boat into a quartz tube with one end open, and place the quartz tube into the inner cavity of the tube furnace. After heating the tube furnace to a certain temperature, introduce Ar / O2 gas. After reacting for a certain time, allow the tube furnace to cool naturally to room temperature. Ga2O3 nanowires are obtained in the GaN thin film trench.
[0015] Step 5: Prepare metal electrodes on the GaN film surface on both sides of the GaN thin film trench to form the final optoelectronic device that can be used for photodetectors and neuromorphic vision sensors.
[0016] In the method for fabricating optoelectronic devices that can be used in photodetectors and neuromorphic vision sensors, the number of GaN thin film trenches in step 1 is 1 to 100.
[0017] In the method for preparing optoelectronic devices that can be used in photodetectors and neuromorphic vision sensors, the thickness of the Au catalyst in step 2 is 1-5 nm.
[0018] In the method for fabricating optoelectronic devices that can be used in photodetectors and neuromorphic vision sensors, in step 3, the distance between the GaN thin film and the metallic Ga is 0.5 to 2 cm.
[0019] In the method for preparing optoelectronic devices that can be used in photodetectors and neuromorphic vision sensors, in step 4, the heating temperature of the tube furnace is 900-1050℃ and the reaction time is 15-30 minutes.
[0020] The design concept of this invention is:
[0021] This invention constructs a GaN / Ga2O3 / GaN trench-bridged double heterojunction optoelectronic device, utilizing a bias voltage to control oxygen vacancies (V0) in Ga2O3. O The content of V can be adjusted to control the photoresponse speed of the device. Specifically, Ga2O3 contains a large amount of V. O When a high voltage is applied to the device, the electrically neutral V O Under ultraviolet light irradiation, positively charged oxygen vacancies are generated. And electrons. After being exposed to light, due to the presence of an energy barrier, They do not immediately recombine with electrons. This results in a sustained photoconductivity (PPC) effect and a non-volatile photocurrent. On the other hand, when a lower voltage is applied to the device, because the lower voltage has less impact on the heterojunction band structure, when the device is exposed to ultraviolet light, the photogenerated electrons generated in GaN are more easily injected into Ga2O3 through the GaN / Ga2O3 interface. The increase in electron concentration in Ga2O3 accelerates... The recombination rate with electrons, thus forming V O Therefore, the PPC effect is significantly suppressed, and the device exhibits volatile photocurrent. Thus, based on this voltage-modulated photoresponse speed, we can achieve the switching between photodetector and neuromorphic vision sensor functions on a single device simply by adjusting the bias voltage.
[0022] Compared with existing technologies, the advantages of the optoelectronic device of the present invention, which can be used in photodetectors and neuromorphic vision sensors, are as follows:
[0023] 1) Under ultraviolet light irradiation, V in Ga2O3 O The ionization and deionization processes can be effectively regulated by voltage. Therefore, the optical response speed of the device can be controlled simply by changing the voltage applied to it.
[0024] 2) Based on the unique photoelectric characteristics of the device under different voltages, the device can realize the functions of both a photodetector and a neuromorphic vision sensor, and can switch between them by voltage regulation.
[0025] 3) When the device disclosed in this invention is used as an ultraviolet photodetector, it can realize functions such as fast optical imaging and optical communication based on its ultra-fast light response speed.
[0026] 4) When the device disclosed in this invention is used as a neuromorphic visual sensor, it can exhibit various neuronal / synaptic functions similar to the learning and memory behaviors of the human brain. In particular, when the neuromorphic visual sensor is used for image preprocessing, its contrast enhancement and noise reduction functions can significantly improve the accuracy and speed of image recognition while reducing power consumption. Attached Figure Description
[0027] Figure 1 (a) is a schematic diagram of the three-dimensional structure of the GaN / Ga2O3 / GaN device, and (b) is a magnified view of a portion of it. In the figures, 1 represents sapphire, and 2 represents the trench.
[0028] Figure 2 This is a schematic diagram of an apparatus for preparing GaN / Ga2O3 / GaN heterojunctions. In the diagram, 3 is a tube furnace, 4 is a reactor tube, 5 is a quartz tube, 6 is a quartz boat, and 7 is GaN / sapphire.
[0029] Figure 3 This is a scanning electron microscope (SEM) image of Ga2O3 nanowires.
[0030] Figure 4 These are the transient optical response curves of the device under 222nm illumination and different bias voltages.
[0031] Figure 5 In the diagram, (a) is a schematic diagram of the band structure of the GaN / Ga2O3 / GaN heterojunction under no illumination and without applied bias voltage; (b) is a schematic diagram of the band structure and carrier transport of the GaN / Ga2O3 / GaN heterojunction under ultraviolet illumination and with applied large bias voltage; and (c) is a schematic diagram of the band structure and carrier transport of the GaN / Ga2O3 / GaN heterojunction under ultraviolet illumination and with applied small bias voltage.
[0032] Figure 6 It is the X-ray photoelectron spectroscopy (XPS) of Ga2O3 nanowires.
[0033] Figure 7 It is the transient optical response curve of the device in a single cycle under a small bias voltage (0.5V).
[0034] Figure 8 It is the photoelectric imaging function realized when the device is used as a photodetector (0.5V).
[0035] Figure 9 When the device is used as a photodetector (0.5V), it utilizes the Morse code information obtained by the device for information transmission.
[0036] Figure 10 When the device is used as a neuromorphic visual sensor, the behavior of the device is transformed from short-term plasticity (STP) to long-term sustainability (LTP) through the number of pulses.
[0037] Figure 11 It refers to the experiential learning behavior of a device when it is used as a neuromorphic vision sensor, including the processes of learning, forgetting, and relearning.
[0038] Figure 12 This is the device power consumption calculated at an ultra-low operating voltage (0.1mV) when the device is used as a neuromorphic vision sensor.
[0039] Figure 13 The image mappings are the light response images after the device is observed (a) 1 time, (b) 3 times and (c) 10 times when it is used as a neuromorphic vision sensor.
[0040] Figure 14 When the device is used as a neuromorphic vision sensor, (a) the contrast enhancement and noise reduction effect of the device, and (b) the recognition accuracy curves before and after image preprocessing. Detailed implementation method:
[0041] In practical implementation, the optoelectronic device structure of this invention, applicable to photodetectors and neuromorphic vision sensors, is a back-to-back GaN / Ga2O3 / GaN double heterojunction. The GaN is a GaN thin film with a central trench, and the Ga2O3 is Ga2O3 nanowires grown on the sidewalls of the GaN trench. By controlling the ionization and deionization processes of oxygen vacancies in the Ga2O3, the device exhibits volatile and non-volatile photocurrents under low and high bias voltages, respectively. Based on this characteristic, the device can switch between its roles as a photodetector and a neuromorphic vision sensor simply by changing its bias voltage.
[0042] The present invention will now be further described with reference to the accompanying drawings and specific embodiments.
[0043] Reference Figure 1 The present invention discloses an optoelectronic device that can be used in photodetectors and neuromorphic vision sensors. From bottom to top, the device comprises a sapphire 1 with semi-cylindrical grooves 2, a GaN thin film with lath-shaped grooves, Ga2O3 nanowires, and a Ti / Au electrode. The GaN thin film has lath-shaped grooves that correspond one-to-one with the semi-cylindrical grooves 2. The Ti / Au electrode is disposed on the GaN thin film and does not contact the Ga2O3 nanowires. The Ga2O3 nanowires are grown on the sidewalls of the GaN thin film grooves.
[0044] Reference Figure 2 The apparatus for preparing GaN / Ga2O3 / GaN heterojunction of the present invention includes a reactor tube 4 horizontally inserted into a tube furnace 3, a quartz tube 5 horizontally placed in the center of the inner cavity of the reactor tube 4, the quartz tube 5 being open on the left and closed on the right, a quartz boat 6 with a groove placed in the center of the quartz tube 5, metal Ga being placed inside the quartz boat 6, and GaN / sapphire 7 being vertically placed in the groove of the quartz boat 6 with the GaN film facing the metal Ga, the left end of the reactor tube 4 being the Ar / O2 inlet end, and the right end of the reactor tube 4 being the outlet end.
[0045] Example:
[0046] like Figures 1-2 As shown, this embodiment describes a method for fabricating optoelectronic devices, including photodetectors and neuromorphic vision sensors. The specific steps are as follows:
[0047] 1) Using mechanical cutting, eight parallel grooves were cut into the GaN thin film grown on sapphire 1. The groove width was 25 μm, the spacing between the grooves was 2 mm, and the depth of the grooves was about 10 μm.
[0048] 2) Au catalyst was evaporated onto the sidewalls of GaN trenches using photolithography and electron beam evaporation methods, with a thickness of 3 nm.
[0049] 3) Place 1.5g of metallic Ga into a quartz boat 6 with a groove, and place the GaN / sapphire 7 with Au catalyst vertically in the groove of the quartz boat 6, with the GaN film facing the metallic Ga and 1.5cm away from Ga.
[0050] 4) Place the quartz boat 6 into the quartz tube 5, which is open at one end, and place the quartz tube 5 inside the reaction tube 4 of the tube furnace 3. Heat the tube furnace 3 to 1000℃ and then introduce Ar / O2 gas (mixed in a 95:5 volume ratio) at a rate of 14 standard cubic centimeters per minute (sccm), with a heating rate of 15℃ / minute. After reacting for 20 minutes, stop heating and allow the tube furnace 3 to cool naturally to room temperature. Ga2O3 nanowires can then be obtained on the sidewalls of the GaN thin film trenches.
[0051] 5) Using a mask combined with electron beam evaporation, an 8×8 array of Ti / Au electrodes is fabricated on the GaN film surface on both sides of the 8 GaN film trenches, forming a final optoelectronic device that can be used in photodetectors and neuromorphic vision sensors.
[0052] Reference Figure 3 The SEM images of Ga2O3 nanowires show that Ga2O3 nanowires are grown on both sides of the trenches of the GaN thin film in a trench bridging or through-growing manner to form conductive channels.
[0053] Reference Figure 4 The transient photoresponse curve of the device under 254nm light illumination shows that the device exhibits non-volatility of photocurrent at high voltage (5V). However, at low voltage (0.5V), the photocurrent of the device quickly recovers to its initial state after the ultraviolet light is removed, showing the volatility of photocurrent. This indicates that the device exhibits two different photoresponse states under different operating voltages: fast photoresponse and slow photoresponse.
[0054] Reference Figure 5 and Figure 6 In order to reveal Figure 4 The device exhibits different photoresponse characteristics under different voltages. Figure 5 First, a schematic diagram of the band structure of the GaN / Ga2O3 / GaN heterojunction under no illumination and without applied bias voltage is given. The heterojunction under high voltage ( Figure 5 b) Because Ga2O3 contains a large amount of V O ( Figure 6 ), electrically neutral V O It will generate a positive charge under ultraviolet light. And electrons. After being exposed to light, due to the existence of the energy barrier, They do not immediately recombine with electrons. This results in the PPC effect and a non-volatile photocurrent in the device. At low voltages ( Figure 5 c) Because low voltage has a relatively small impact on the band structure of back-to-back double heterojunctions, when the heterostructure is exposed to ultraviolet light, photogenerated electrons in GaN have a greater chance of crossing the GaN / Ga2O3 interface and being injected into Ga2O3. The increase in electron concentration in Ga2O3 will accelerate this process. Recombination with electrons forms V O Therefore, the PPC effect of the device is significantly suppressed at low voltages, thus exhibiting non-volatile photocurrent. Based on this voltage-modulated photoresponse speed, we can switch between the roles of photodetector and neuromorphic vision sensor on a single device simply by adjusting the bias voltage.
[0055] Reference Figure 7 As can be seen from the transient photoresponse curve of the device in a single cycle at a low voltage (0.5V), the device, as a photodetector, has a very fast photoresponse speed, and its photoresponse rise time (T) is very short. r The photoresponse fall time is only 118 μs, and the photoresponse fall time (T) is only 118 μs. d The wavelength is only 167 μs.
[0056] Reference Figure 8 When used as a photodetector, the device can achieve rapid photoelectric imaging.
[0057] Reference Figure 9 When used as a photodetector, the device can transmit Morse code information.
[0058] Reference Figure 10 Repeated learning helps the brain process and store information. Memory levels are affected by the frequency, duration, and intensity of learning; through repeated learning, a shift from STP (Solution-to-Person) to LTP (Long-Term) can be achieved. Figure 10 As shown, when the device is used as a neuromorphic visual sensor, the device current increases significantly with the increase of the number of light pulses applied to the device, which means that the device needs a longer time to remember the image before forgetting it. This transition from STP to LTP is very similar to the process of image memory in the human brain. Therefore, the level of image memory of the device can be adjusted by regulating the number of light pulses, which means that our device is feasible in simulating the image learning and memory capabilities of the human brain.
[0059] Reference Figure 11 The plasticity of neural synapses causes the human brain to undergo a "learning-forgetting-relearning" process when memorizing images. To simulate this experiential learning behavior, we used 30 consecutive light pulses to stimulate the device. Figure 11 As shown, under continuous light pulse stimulation, the device current steadily increases. After a light pulse stimulation, the device current begins to decrease, corresponding to the forgotten portion during the learning process. To recover the forgotten portion, light pulses are applied to the device again. It can be seen that only 8 light pulses are needed to recover the previous learning level, which is far fewer than the number of pulses required for the initial learning.
[0060] Reference Figure 12 In addition to simulating various functions of biological neural synapses, an ideal neuromorphic device should also have low power consumption. Traditional complementary metal-oxide-semiconductor (CMOS) devices require approximately 900 pJ of energy to simulate a single event, while the human brain consumes only 1–10 fJ. Based on a unique device structure design, the device's minimum power consumption is only 3.26 fJ per event, comparable to the power consumption of the human brain.
[0061] Reference Figure 13In the human visual system, repeated stimulation of retinal cells by images leads to an increase in the synaptic weights between visual neurons. This results in a clearer memory of the image in the brain and a lower likelihood of forgetting. Therefore, based on the synaptic plasticity exhibited by the device, it effectively simulates the image memory and forgetting functions of human vision.
[0062] Reference Figure 14 Through image preprocessing using a neuromorphic vision sensor, the main features of the output image are highlighted, while background noise is significantly suppressed. Figure 14 a). The output image has higher contrast compared to the input image. We constructed a neuromorphic vision system using a neuromorphic vision sensor and an artificial neural network (ANN) to perform image recognition tasks. It can be seen that without image preprocessing via the neuromorphic vision sensor, achieving an image recognition rate of 99.0% requires 125 iterations ( Figure 14 (b) After preprocessing with a neuromorphic vision sensor, the same recognition rate could be achieved in just 47 iterations. These results demonstrate that using a neuromorphic vision sensor for image preprocessing can enable feature extraction and improve image recognition rate and speed.
[0063] The results of the embodiments show that the GaN / Ga2O3 / GaN heterojunction optoelectronic device of the present invention can realize the conversion between photodetector and neuromorphic vision sensor on a single device simply by adjusting the bias voltage, and both exhibit excellent device performance. Furthermore, the device has a simple fabrication process, which is beneficial for its widespread application in the field of optoelectronic devices.
[0064] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any modifications or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. An optoelectronic device useful for photodetectors and neuromorphic vision sensors, comprising: a substrate; a plurality of nanowires disposed on the substrate; a plurality of nanowire junctions disposed on the substrate; and a plurality of nanowire junctions disposed on the substrate. The device has a back-to-back GaN / Ga2O3 / GaN double heterojunction structure. From bottom to top, it consists of a sapphire substrate with semi-cylindrical trenches, a GaN thin film with lath-shaped trenches, Ga2O3 nanowires, and a metal electrode. The GaN thin film is grown on the sapphire substrate, and lath-shaped trenches are formed on the GaN thin film that correspond one-to-one with the semi-cylindrical trenches. The Ga2O3 nanowires are grown on the sidewalls of the trenches in the GaN thin film. The metal electrode is disposed on the GaN thin film and does not contact the Ga2O3 nanowires. By changing the bias voltage of the device, the device can switch between the roles of a photodetector and a neuromorphic vision sensor.
2. The optoelectronic device for use in photodetectors and neuromorphic vision sensors according to claim 1, wherein, The GaN film thickness is 500 nm to 5 μm. The trench depth of the GaN film extends into the sapphire substrate to insulate the GaN films on both sides. The trench width is between 5 and 50 μm, and the spacing between the trenches is 1 to 5 mm.
3. The optoelectronic device for use in photodetectors and neuromorphic vision sensors according to claim 1, wherein, Ga2O3 nanowires connect GaN films on both sides of GaN film trenches in a bridging or through manner to form conductive channels. The length of the Ga2O3 nanowires is between 5 and 100 μm.
4. The optoelectronic device for use in photodetectors and neuromorphic vision sensors according to claim 1, wherein, The metal electrode is either Ti / Au or Cr / Au.
5. A method of producing an optoelectronic device according to one of claims 1 to 4, for use in photodetectors and neuromorphic vision sensors, characterized in that, Includes the following steps: Step 1: Cut grooves into the GaN thin film grown on sapphire; Step 2: The Au catalyst is evaporated onto the sidewalls of the GaN trench using an electron beam. Step 3: Place the metal Ga into a quartz boat with grooves, and place the GaN / sapphire with Au catalyst vertically in the grooves of the quartz boat, with the GaN film facing the metal Ga and at a certain distance from the metal Ga. Step 4: Place the quartz boat into a quartz tube with one end open, and place the quartz tube into the inner cavity of the tube furnace of the tube furnace. After heating the tube furnace to a certain temperature, introduce Ar / O2 gas. After reacting for a certain time, allow the tube furnace to cool naturally to room temperature. Ga2O3 nanowires are obtained in the GaN thin film trench. Step 5: Prepare metal electrodes on the GaN thin film surface on both sides of the GaN thin film trench to form the final optoelectronic device that can be used for photodetectors and neuromorphic vision sensors.
6. The method of claim 5, wherein, In step 1, the number of GaN thin film trenches is 1 to 100.
7. The method of claim 5, wherein the method further comprises: In step 2, the thickness of the Au catalyst is 1~5 nm.
8. The method for fabricating an optoelectronic device applicable to photodetectors and neuromorphic vision sensors according to claim 5, characterized in that, In step 3, the distance between the GaN thin film and the metallic Ga is 0.5~2 cm.
9. The method of claim 5, wherein, In step 4, the heating temperature of the tube furnace is 900~1050 °C, and the reaction time is 15~30 minutes.