A method for welding a rod-shaped conductor; a corresponding rod-shaped conductor assembly and application of the rod-shaped conductor assembly
Patent Information
- Application Number
- CN202280028670.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-16
- Filing Date
- 2022-04-07
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-04-07
AI Technical Summary
In the prior art, hairpins made of aluminum are prone to weld bead deviation during laser welding and cannot obtain sufficient cross-section to conduct current, resulting in unusable welding.
By guiding the processing laser beam during the laser welding process, a non-liquid oxide surface layer is formed, and a liquid rod-shaped conductor material is formed under the surface layer, and the stability of the oxide surface layer is controlled to ensure the shape and size of the weld bead.
Reliable welding is achieved, the current conduction characteristics between rod-shaped conductors are ensured, the problems of weld bead deformation and incomplete formation are avoided, and the reliability and efficiency of welding are improved.
Smart Images

Figure CN117279731B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for laser welding of bar conductors, preferably bent bar conductors, in particular hairpins, for electric motors or generators. Background Art
[0002] The bar conductor consists of an aluminum-containing bar conductor material having an aluminum content of at least 75% by weight, preferably at least 90% by weight,
[0003] wherein two bar conductors are arranged partially overlapping and positioned next to each other and are welded to each other by means of a processing laser beam, a weld bead being formed on the common base surface of the bar conductors lying next to each other, via which weld bead the bar conductors are connected to each other,
[0004] In particular, the common base surface is oriented horizontally.
[0005] This method is known from the Internet publication "STATOR HAIRPINS AUS ALUMINIUM ENTLACKEN UND SCHWEIβEN-GROβESEINSPARPOTENZIAL" of Clean-Lasersysteme of Herzogenrath (North Rhine-Westphalia, Germany), see https: / / www.cleanlaser.de / de / news / hairpins- aluminium / , May 3, 2021.
[0006] In the production of electric motors or generators, in addition to wound stators, stators made of metallic, usually bent, rod-shaped conductors ("bar conductors"), in particular so-called hairpins, are now used. The bar conductors are arranged so that they correspond to the provided electrical connections and are then welded to one another in order to form an electromagnet in this way. Compared to wound stators, hairpin technology offers advantages in terms of weight, costs and efficiency.
[0007] In this case, the bar conductors are usually welded by means of a laser beam. For this purpose, the laser beam is typically directed at the end sides of two overlapping bar conductors, which usually lie against each other. As a result, heat is introduced into the bar conductors, the bar conductors melt, and after solidification, the bar conductors are connected to each other via a solidified weld bead.
[0008] During welding, a sufficiently large cross-section must be produced through which the current can flow between the two rod-shaped conductors. If welding is not performed correctly, this can lead to ohmic heating, loss of efficiency or an unusable motor during operation.
[0009] Until now, mainly bar conductors made of copper have been used. An example for welding bar conductors containing copper is known from the subsequently published German patent application 10 2020113 179.8.
[0010] In the aforementioned Internet publication, the company Clean-Lasersysteme proposes the direct processing of hairpins made of aluminum as a copper replacement. To this end, the hairpins made of aluminum are welded to one another in a vacuum. The use of hairpins made of aluminum is intended to be particularly cost-effective. No further details about the method are mentioned.
[0011] However, welding of hairpins made of aluminum has proven difficult in practice. The weld bead generated by the laser beam tends to stray during the welding process, so that often no sufficient cross section is available for conducting the current and the weld is unusable. Summary of the invention
[0012] The object of the present invention is to provide a method for laser welding of rod-shaped conductors containing an aluminum alloy in order to produce a highly reliable and usable weld, in particular to achieve a sufficiently large cross section for conducting current.
[0013] This object is achieved according to the invention by a method of the type mentioned in the introduction, which method is characterized in that
[0014] During laser welding of a rod-shaped conductor, the processing laser beam is guided and the welding contour of the processing laser beam is positioned relative to the rod-shaped conductor and the feed speed v of the processing laser beam along the welding contour relative to the rod-shaped conductor is selected such that:
[0015] wherein during laser welding of the rod-shaped conductor, the weld bead has a non-liquid oxide surface layer, within which liquid rod-shaped conductor material accumulates during laser welding of the rod-shaped conductor,
[0016] wherein during the laser welding of the rod-shaped conductor, the non-liquid oxide surface layer is only partially broken away by the processing laser beam at the upwardly pointing end side of the weld bead in accordance with the weld contour,
[0017] wherein during the laser welding of the rod-shaped conductor the non-liquid oxide surface layer remains intact in a circumferential region of the weld bead which extends away from the upper end towards the rod-shaped conductor and around the entire weld bead.
[0018] In the context of the method according to the invention, it is proposed that, by suitable process control during the welding of two aluminum-containing rod-shaped conductors, a non-liquid oxide layer ("oxide layer") is formed in the region of the process zone and remains stable during the method. Liquid rod-shaped conductor material then forms below the oxide layer, which is held in a defined shape of the weld bead by the oxide layer. This allows a usable weld to be reliably produced.
[0019] When welding two metal-containing bar conductors, the production of a dimensionally stable weld bead is important, since the quality of the weld bead obtained has an influence on the current conduction characteristics between the bar conductors. At melting temperature, the viscosity and surface tension of aluminum are much lower than those of copper. This is why, during welding, the low-viscosity melt of the aluminum alloy tends to flow out of the region of the process zone where welding is carried out in an uncontrolled manner. This can lead to a severely deformed or incompletely formed weld bead, which results in a reduction in the cross section between the bar conductors in which the current can flow.
[0020] The advantages brought about by the use of aluminum-containing rod conductors, such as the cost savings already mentioned above and the weight reduction (element copper has a weight of 8.96 g / cm 3 The density of elemental aluminum is 2.7 g / cm 3 The density (more than three times that of the original) can be negated by defects or too small a cross section between the rod-shaped conductors.
[0021] In the method according to the invention, the process is carried out in such a way that during the laser welding of the rod-shaped conductor, a non-liquid oxide layer ("oxide surface") is present in the region of the process zone. The oxide surface circumvents the disadvantages of the low viscosity and surface tension of the aluminum-containing alloy melt. The oxide surface maintains the shape of the melt uniformly and forms a peripheral surface area ("side surface") which orients the melt upward and restricts it to the side. A uniform weld bead is thereby produced and the melt is prevented from flowing to the side. The viscosity and surface tension of the melt are no longer important.
[0022] Aluminum stored in air spontaneously forms a thin layer of aluminum oxide (self-passivation) to protect it from corrosion. Thus, at the beginning of the welding method, the rod-shaped conductor material is already covered with an oxide surface layer, below which a liquid melt can form and accumulate. During laser welding, the thickness of the oxide surface layer increases compared to the thickness of the previous oxide surface layer of the solid rod-shaped conductor, in particular due to the temperatures reached during laser welding. Furthermore, during the method, new aluminum oxide can spontaneously form at locations where molten aluminum is exposed, in particular at locations in the oxide surface layer that are broken open by the machining laser beam. During the implementation of the method, the oxide surface layer that is present before the start of laser welding and / or the oxide surface layer that is newly formed during laser welding remains confined to the weld bead that is forming or growing for substantially the entire time, using the oxide surface layer that is present before the start of laser welding and / or the oxide surface layer that is newly formed during laser welding.
[0023] Within the framework of the invention, the process control is carried out in such a way that the dynamics of the melt are limited, in particular close to the peripheral area, and the formation of cracks in the peripheral area, from which the melt could flow out in an uncontrolled manner, which could lead to an inhomogeneous weld bead, is prevented. In order to limit the dynamics of the molten pool, the machining laser beam can be advanced along the welding contour, in particular at a sufficiently low feed rate. Furthermore, in order to avoid the appearance of cracks in the peripheral area of the oxide surface layer of the weld bead, the welding contour can be selected so that it is sufficiently spaced apart from the periphery of the rod-shaped conductor (or from the periphery of the side of the rod-shaped conductor facing the laser beam, the "end side"). Under the conditions described, the stability of the oxide surface layer is improved.
[0024] During the laser welding of the rod-shaped conductors, a molten pool is formed below the oxide surface layer. This is possible because the melting temperature of aluminum in elemental form is ≈660°C, which is significantly lower than the melting temperature of aluminum oxide, ≈2070°C (depending on the atmospheric conditions, the processing laser beam can also cause Al2O3 to dissociate instead of melting). The molten pool is heated until the required volume of liquid aluminum is obtained. This ensures that the cross-section between the rod-shaped conductors is large enough to achieve sufficiently high current conduction during the final solidification.
[0025] The machining laser beam interacts with the oxide surface layer substantially only in the region where the machining laser beam impinges on the oxide surface layer. The machining laser beam breaks the oxide surface layer only along its weld contour, so that the weld contour produces a track of breaks (or liquids) and there may also be broken (or liquid) areas inside the weld contour. In all other respects, the oxide surface layer is maintained and holds the molten rod-shaped conductor material together and in shape.
[0026] After the action of the machining laser beam has ended, the molten pool, which is still held in shape by the oxide surface layer, cools down. When solidifying, a defined weld bead is produced, wherein the connected rod-shaped conductor has a sufficiently large cross section and ensures sufficiently good current conduction. A usable weld is reliably produced.
[0027] Preferred variants of the invention
[0028] In a preferred variant of the method according to the invention, it is provided that
[0029] The welding contour of the processing laser beam is positioned relative to the rod-shaped conductor such that for the minimum distance d of the welding contour from the outer edge of the common base surface and for the extension L of the common base surface in the direction in which the minimum distance d lies the following applies:
[0030] d≥0.15*L, preferably d≥0.20*L, particularly preferably d≥0.25*L. This is a distance d which has proven effective in practice and by which the possibility of damage by oxide layers, in particular in the peripheral area, can be minimized.
[0031] A variant is particularly preferred in which the welding contour of the processing laser beam is positioned relative to the rod-shaped conductor such that for the minimum distance d of the welding contour from the outer edge of the common base surface the following applies:
[0032] d≥0.6 mm, preferably d≥0.8 mm, particularly preferably d≥1.0 mm. This also relates to the distance d, which has proven to be effective in practice and by which the possibility of damage to the oxide surface layer, in particular in the peripheral area, can be minimized.
[0033] In an advantageous variant, the following applies for the feed speed v of the machining laser beam along the welding contour of the machining laser beam relative to the rod-shaped conductor:
[0034] v≤1600 mm / s, preferably v≤1200 mm / s, particularly preferably v≤800 mm / s. The feed rate v has an influence on the dynamic properties of the melt produced below the non-liquid oxide surface layer. At the specified feed rate, in practice, the oxide surface layer exhibits good stability and forms a uniformly shaped weld bead.
[0035] A variant is preferred in which the laser welding is carried out in an oxygen-containing atmosphere, in particular in air. An oxygen-containing atmosphere stabilizes the oxide surface layer of the weld bead and promotes rapid reformation of aluminum oxide on exposed aluminum melt, for example in the path of the processing laser beam. In addition, an oxygen-containing atmosphere can be easily established; in particular when using air, no additional structures are required.
[0036] In a preferred variant of the method according to the invention, it is provided that, at least during the second half of the laser welding of the rod-shaped conductors, the peripheral area in which the non-liquid oxide surface layer remains intact extends over at least 3 / 4 of the height of the weld bead, preferably over at least 9 / 10 of the height of the weld bead. This ensures the formation of a dimensionally stable and uniform weld bead, the height of which, over the available cross section of the weld bead, establishes a practically sufficient electrical conduction of current between the rod-shaped conductors. Typically, the peripheral area extends over virtually the entire height of the weld bead.
[0037] A variant is also preferred, in which the two bar-shaped conductors are arranged with their end regions parallel to one another and abutting one another, in particular in which the end regions of the bar-shaped conductors are flatly pressed against one another, the front faces of the bar-shaped conductors are located at approximately the same height with respect to the direction of the longitudinal extension of the end regions of the bar-shaped conductors, and the machining laser beam is directed toward the front faces of the bar-shaped conductors, and the front faces thus provide a common base surface on which the weld bead is formed. The arrangement of the end faces at approximately the same height ensures that the corresponding melts formed by the machining laser beam at the end faces can be combined without problems to form a common, uniformly shaped (spherical) weld bead, and in particular the common weld bead does not have to form a slope. The end regions abutting one another reduce the risk of melt of the common weld bead flowing out between the bar-shaped conductors. By pressing the end regions together, the gap remaining between the end regions abutting one another can be minimized.
[0038] A further development of this variant is advantageous, which provides that the end region of the rod-shaped conductor points approximately vertically upward, in particular wherein the front face is oriented approximately horizontally. In this arrangement, the processing laser beam can easily reach the end face. The horizontal orientation of the end face ensures that the formed melt is not subject to any downward forces and the weld bead is stable.
[0039] A further embodiment is also preferred, in which the machining laser beam impinges on the front face approximately vertically. This results in a particularly stable vapor capillary and reduces the dynamics of the molten pool, making it easier to form a defined weld bead.
[0040] A variant is preferred which provides that the bar-shaped conductors at least close to the common base surface, in particular in the respective end regions, each have a rectangular cross section with an edge length of between 0.2 mm and 10 mm, preferably between 1 mm and 8 mm, particularly preferably between 2 mm and 6 mm, in particular wherein in the respective bar-shaped conductors the long edge length L2 is a factor of the short edge length L kurz The cross-section of the two bar conductors to be welded is twice as long as that of the short edge, and the cross-sections of the two bar conductors to be welded are identical. These dimensions have proven to be effective in practice, in particular for the construction of electric motors. Typically, the long edges of the bar conductors abut against one another; this minimizes the cross-section in the weld bead through which the bar conductors can be connected to one another. If the long edge is chosen to be twice as long as the short edge, a square base surface can be provided by bar conductors of identical cross-section. The energy of the machining laser beam can be introduced particularly uniformly into the base surface, in particular by means of a circular welding profile.
[0041] Furthermore, a variant is preferred, which provides that the minimum distance d2 between the weld contour and the outer edge of the common base surface in the direction of the respective long edge is between 20% and 40%, preferably between 25% and 35%, of the associated long side length L2, and the minimum distance d1 between the weld contour and the outer edge of the common base surface in the direction of the respective short edge is between 20% and 40%, preferably between 25% and 35%, of twice the short side length L1. These are distances d2 and d1, which have proven to be effective in practice and by which the possibility of damage to the oxide surface layer, in particular in the peripheral area, can be minimized.
[0042] In an advantageous variant, the machining laser beam has a laser power P, wherein
[0043] 0.5kW≤P≤20kW,
[0044] Preferably 2kW≤P≤10kW,
[0045] Particularly preferably, 4kW≤P≤8kW,
[0046] and / or the wavelength of the processing laser beam is between 400 nm and 1200 nm. Said laser powers and wavelengths of the processing laser beam have proven in practice to be particularly effective for the method according to the invention. In particular, a uniform formation of the weld bead can be achieved during the welding process.
[0047] A variant is particularly preferred in which the welding contour is selected as linear, circular or elliptical and is traversed several times during the laser welding of the rod-shaped conductor, in particular in which the welding contour is generated by means of scanning optics. By traversing the welding contour several times during the laser welding of the rod-shaped conductor, the energy of the processing laser beam can be evenly distributed and in this case practically any desired energy can be introduced into the rod-shaped conductor by a corresponding number of traversings. Local overheating is avoided. Overall, a particularly uniform formation of the weld bead can be achieved. The scanning optics are typically designed with a mirror and two piezoelectric actuators so that the welding contour can be set on the rod-shaped conductor or the weld bead with little effort and can be traversed precisely, in particular also at a speed that cannot be achieved or can only be achieved with difficulty by mechanically moving the workpiece or the laser head. The shape of the welding contour can be matched to the shape and orientation of the rod-shaped conductor to be welded.
[0048] Furthermore, a variant is preferred in which a shaped laser beam having a core and a ring is selected as the processing laser beam at least temporarily, the ring surrounding the core in an annular manner, in particular in which the shaped laser beam is generated by means of a 2-in-1 fiber having a core fiber diameter KFD, in which 11 μm ≤ KFD ≤ 300 μm, preferably 50 μm ≤ KFD ≤ 100 μm, and a ring fiber diameter RFD, in which 50 μm ≤ RFD ≤ 1000 μm, preferably 200 μm ≤ RFD ≤ 400 μm. The use of a shaped laser beam makes it possible to reduce the overall melt pool dynamics and minimize welding defects such as spatter formation or pore formation, in particular at the beginning and end of the method. The power component of the laser power in the core can be selected or varied between 20% and 100%, preferably between 20% and 80%, particularly preferably between 40% and 60%. The distribution of the laser power between the core and the ring can be chosen to be constant throughout the welding process if desired, typically with a power component P of 40-60% in the core. kern Alternatively, it is also possible that the power component P kern is selected to be different in the first stage (initial stage), the main stage and the last stage (final stage) of the laser welding of the rod-shaped conductor. If necessary, in the main stage of laser welding (between the initial stage and the final stage), the power component P in the core can be selected kern 100% in order to increase the process speed, and in the first stage (initial stage) and / or the last stage (final stage) can be selected to be smaller and in particular to be continuously variable in order to minimize welding defects.
[0049] In a preferred further development of this variant, the power component P of the laser power in the core kern is selected to be smaller during the temporal first phase of the laser welding of the rod-shaped conductor than during the main phase of the laser welding of the rod-shaped conductor, in particular wherein the power component P of the laser power in the core kern During the first phase, the power is increased continuously, in particular wherein the first phase has a duration between 1 ms and 30 ms. When the machining laser beam is radiated (start of the initial phase), a smaller power component P is selected. kern This ensures that spatter is less formed, thereby preventing relatively large amounts of liquid melt and non-liquid oxide surface layers from being ejected from the process area early at the beginning of the initial phase, which would make it more difficult to form a uniform weld bead. kernThe power required for the main phase can be increased continuously. Typically, the first phase (initial phase) comprises a share of 10-30% of the total welding duration. During the first phase, the vapor capillary is formed. The first phase typically lasts at least a long time, because it takes a long time for the vapor capillary to reach at least 30% of its maximum capillary depth when laser welding rod-shaped conductors.
[0050] A further embodiment is also preferred in which the power component P of the laser power in the core kern is selected to be smaller during the temporal final phase of the laser welding of the rod-shaped conductor than during the main phase of the laser welding of the rod-shaped conductor, in particular wherein the power component P of the laser power in the core kern During the last phase, the smaller power component P is continuously reduced, in particular wherein the last phase has a duration between 1 ms and 30 ms. kern Ensure that the steam capillary can gradually disappear in a controlled manner; the power component P kern The continuous reduction of can cause the vapor capillary to disappear particularly gently. This ensures that no pores or only a few small pores are produced in the weld bead. This ensures a reliable and usable weld. Typically, the last phase (final phase) comprises 10-30% of the total welding duration.
[0051] The invention also relates to a bar conductor arrangement comprising at least two bar conductors welded by means of the above-described method according to the invention. The weld bead formed during welding is uniformly shaped and reliably provides a sufficient cross section for the flow of current between the welded bar conductors. Typically, a plurality of bar conductors (for example in a stator carrier) are welded one after the other, wherein a bar conductor is welded to another bar conductor at two legs (or to a power supply connection in the case of a bar conductor located at the end).
[0052] The invention also includes the use of a bar conductor assembly which is produced by welding two bar conductors by means of the above-described method according to the invention and which is installed in an electric motor or generator. The welding of the bar conductors is particularly reliable and is therefore also well suited for the high current intensities occurring in electric motors and generators. The low inherent weight of the bar conductors made of aluminum-containing bar conductor material is particularly advantageous in the case of electric motors which are intended for mobile applications, such as electric vehicles.
[0053] Further advantages of the present invention are obtained from the description and the drawings. According to the present invention, the above-mentioned features and the features further explained can also be used individually or in any combination of multiples. The embodiments shown and described should not be understood as exhaustive, but have exemplary features for summarizing the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] The invention is illustrated in the drawings and explained in more detail with reference to exemplary embodiments. In the drawings:
[0055] Figure 1 A schematic side view shows two bent-over bar conductors arranged partially one above the other, which are welded to one another within the scope of the invention;
[0056] Figure 2 A schematic oblique view shows the laser welding process before the start of the laser welding according to the invention. Figure 1 end regions of the two rod-shaped conductors abutting against each other;
[0057] Figure 3 A schematic side view shows the process of laser welding according to the invention. Figure 2 Two rod-shaped conductors and the weld beads formed;
[0058] Figure 4 Show Figure 2 A schematic top view of the end region of two rod-shaped conductors;
[0059] Figure 5 A schematic top view shows the end regions of two bar-shaped conductors in the variant in which the common base area is square;
[0060] Figure 6a A schematic diagram of a shaping processing laser beam for use in the present invention is shown in cross section with a core and a ring;
[0061] Figure 6b A schematic diagram showing an exemplary two-in-one optical fiber for use in the present invention with a core fiber and a ring fiber in a cross-sectional view, with the aid of which a shaped laser beam for laser welding according to the present invention can be provided;
[0062] Figure 7 A diagram showing the core laser power as a function of time for a shaping laser beam used in accordance with the present invention during laser welding of two rod-shaped conductors;
[0063] Figure 8a An experimental image showing the laser welding of two aluminum-containing rod-shaped conductors directly after completion of the laser welding process under conditions where the oxide surface layer of the weld bead is repeatedly broken and an inhomogeneous weld bead is formed;
[0064] Figure 8b The experimental images are shown directly after the end of the laser welding of two aluminum-containing rod conductors under the conditions of the method according to the invention, in which the oxide surface layer of the weld bead in the circumferential region remained intact and a homogeneous weld bead was formed. DETAILED DESCRIPTION
[0065] Figure 1 Two aluminum-containing bent bar conductors 1a, 1b are shown in a schematic side view. The bar conductors 1a, 1b are designed as so-called hairpins and are used to produce electrical machines, such as motors or generators. The bar conductors 1a, 1b are each approximately U-shaped and have two legs 2a, 3a and 2b, 3b and a middle part 4a, 4b, which connects the respective leg pairs to each other.
[0066] The bar conductors 1a, 1b should be connected to each other in an electrically conductive manner. To this end, according to the invention, the bar conductors 1a, 1b are welded to each other at their end regions 5a, 5b. For welding, the legs 3a of the first bar conductor 1a and the legs 3b of the second bar conductor 1b are arranged overlapping, in the variant shown here, butting against each other.
[0067] For the bar conductors 1a, 1b, an aluminum-containing bar conductor material is used, which has an aluminum content of at least 75% by weight, preferably at least 90% by weight. Possible aluminum-containing bar conductor materials that come into consideration are, for example, aluminum alloys from the 1000 to 6000 series group (for example material EN AW-1050A).
[0068] Figure 2 The end regions 5a, 5b of two bar conductors 1a, 1b before the start of laser welding according to the invention are shown in a schematic oblique view. The coordinate system is selected so that the x-axis points to the right, the y-axis points into the plane of the drawing, and the z-axis points upward. Here, the front faces 6a, 6b of the two bar conductors 1a, 1b are approximately the same height and are oriented horizontally. The front faces 6a, 6b of the two bar conductors 1a, 1b together form a common base surface 7. The end regions 5a, 5b of the bar conductors 1a, 1b each have a rectangular cross section in the xy plane. The long sides 8a, 8b of the cross section of the bar conductors 1a, 1b abut against each other in the end regions 5a, 5b of the legs 3a, 3b, which are pressed against each other (not specifically shown). The legs 3a, 3b are oriented vertically and parallel to each other so that the two end faces 6a, 6b and therefore the common base surface 7 are oriented upward.
[0069] The two end regions 5a, 5b are to be welded using a processing laser beam 11. For this purpose, a welding contour 12 is determined on the common base surface 7, which the processing laser beam 11 is then to pass over several times. In the exemplary embodiment shown here, the welding contour 12 is selected to be elliptical. Depending on how the rod-shaped conductor is dimensioned and what the possible welding requirements are, a linear welding contour (not shown here) or a circular welding contour (see FIG. 1 ) can also be selected. Figure 5). The dashed area 13 shows the area of the rod-shaped conductors 1a, 1b to be melted by the action of the processing laser beam 11. In an advantageous embodiment, the beam guidance of the processing laser beam 11 along the welding contour 12 can be performed by means of scanning optics (not specifically shown).
[0070] The machining laser beam 11 impinges approximately perpendicularly on the common base surface 7. It should be noted that during the production of different pairs of bar-shaped conductors 1a, 1b, the angle of incidence of the machining laser beam 11 can typically vary slightly, so that the bar-shaped conductors 1a, 1b, which are usually arranged on a stator carrier (not shown in detail), do not have to be moved too frequently. The machining laser beam 11 typically deviates from perpendicular incidence on the base surface 7 by no more than 40°, preferably no more than 20°.
[0071] The laser power P of the processing laser beam 11 can be selected such that 0.5 kW ≤ P ≤ 20 kW, preferably 2 kW ≤ P ≤ 10 kW, particularly preferably 4 kW ≤ P ≤ 8 kW holds true. Good results can thus be achieved in practice. For example, a power P of 6 kW can be used for welding two aluminum-containing rod-shaped conductors 1 a, 1 b. The wavelength of the processing laser beam 11 can be between 400 nm and 1200 nm. Examples of this are wavelengths of 450 nm (blue light), 515 nm (green light), 900 ± 100 nm (diode, NIR), 1030 nm (NIR), 1064 nm (NIR) and 1070 nm (NIR).
[0072] Figure 3 A schematic side view of the Figure 2 The two bar conductors 1a, 1b with the weld bead 19 in the second laser-welded half. The coordinate system is selected such that the x-axis points out of the plane of the drawing, the y-axis points to the right, and the z-axis points upwards. The end regions 5a, 5b of the bar conductors 1a, 1b can be seen during the laser welding, at which the weld bead 19 is formed at this upper end.
[0073] The processing laser beam 11 can be moved here over the welding contour 12, which is located on the upper end side 20 of the welding bead 19. Heat is thus introduced into the aluminum-containing rod-shaped conductor material. Here, liquid rod-shaped conductor material 15 (dashed reference line, because the liquid rod-shaped conductor material 15 is largely covered below the non-liquid oxide surface layer 14), i.e., aluminum-containing melt, forms and accumulates below the non-liquid oxide surface layer 14. The non-liquid oxide surface layer 14 then forms the boundary of the welding bead 19 and ensures that the shape of the liquid rod-shaped conductor material 15 is maintained and prevents the liquid rod-shaped conductor material 15 from flowing. The non-liquid oxide surface layer 14 is partially broken open by the processing laser beam 11, and in the variant shown, the processing laser beam 11 leaves a broken track 12a along the welding contour 12. As a result, the liquid rod-shaped conductor material 15 along the track 12a in the broken area is temporarily exposed. Behind the processing laser beam 11, the liquid rod-shaped conductor material 15 also begins to oxidize, so that a new oxide surface layer 14 is formed and the track 12a is closed again. In the variant shown, the track 12a extends over approximately 1 / 3 of the circumference of the welding contour 12, and then the non-liquid oxide surface layer 14 grows completely again on the welding contour. The method according to the invention is usually carried out in an oxygen-containing atmosphere (for example air), so that the non-liquid oxide surface layer 14 can be re-oxidized particularly quickly in the broken area by oxidation.
[0074] The non-liquid oxide layer 14 extends in the circumferential area 21 of the weld bead 19 from the upper end side 20 downward to the still solid end areas 5a, 5b of the rod-shaped conductors 1a, 1b and around the entire weld bead 19. In the variant shown here, the non-liquid oxide layer 14 is broken in the area of the path 12a (shown in black) along the weld contour 12 along which the machining laser beam 11 is moved. The exposed liquid rod-shaped conductor material 15 is reoxidized by the oxygen-containing atmosphere ( Figure 5 In the variant shown here, the non-liquid oxide surface layer 14 of the upper end side 20 remains intact. In other variants, the inner area of the welding contour 12 can also be completely broken open and remain essentially broken open during the welding process (not shown here).
[0075] The solder bead 19 has an overall height H in the z direction (along the extension direction of the end regions 5a, 5b of the rod-shaped conductors 1a, 1b). sp , and the peripheral area 21 of the weld bead 19 where the non-liquid oxide surface layer 14 remains intact has a height H unv . Height H unvTypically, it extends from the lower end of the weld bead 19 to the region in which the machining laser beam 11 moves over the weld contour 12. Since the machining laser beam 11 partially breaks open the non-liquid oxide surface layer 14 and thus exposes the liquid rod-shaped conductor material 15, the region of the upper end face 20 located within the weld contour 12 is no longer considered an undamaged part of the circumferential surface region 21. In the variant shown here, H unv At height H sp It has proven to be advantageous if the height H unv At height H sp extends over at least 3 / 4 of the sp The H extends over at least 9 / 10 of the end face 20 so that a defined weld bead 19 can be formed. In many cases of use, in a weld bead 19 formed largely flat at the end face 20, H unv Almost throughout the entire height H sp The upper portion of the housing is extended (not specifically shown).
[0076] At the end of welding, after the action of the machining laser beam 11 has ended, the liquid rod-shaped conductor material 15 cools down, while continuing to be held in shape by the non-liquid oxide surface layer 14, and finally solidifies. The rod-shaped conductors 1a, 1b are then electrically conductively connected to each other via the weld bead 19. Here, the weld bead 19 is placed on the two rod-shaped conductors 1a, 1b and covers the entire surface area at the ends of the rod-shaped conductors. The quality of the electrically conductive connection between the two rod-shaped conductors 1a, 1b is essentially determined by the connected cross-section 22. The connected cross-section 22 is a surface that allows current to be conducted from the first rod-shaped conductor 1a to the second rod-shaped conductor 1b. Figure 3 In the case of the clearly defined solder bead 19 shown, the connected cross section 22 corresponds to the cross section of the solder bead 19 in the contact plane of the longitudinal sides of the legs 3a, 3b of the bar-shaped conductors 1a, 1b that abut against one another.
[0077] Figure 4 Show Figure 2 Schematic top view of the end regions 6a, 6b of two bar-shaped conductors 1a, 1b. The coordinate system is selected such that the x-axis points to the right, the y-axis points upwards and the z-axis extends outwards from the plane of the drawing. The front faces 6a, 6b form a common base surface 7, on which an elliptical welding contour 12 is shown. The bar-shaped conductors 1a, 1b form in the end regions 5a, 5b a respective rectangular cross section 9a, 9b corresponding to each of the end faces 6a, 6b visible here. In this variant, the rectangular cross sections 9a, 9b in the end regions 5a, 5b of the two bar-shaped conductors 1a, 1b are identical. In practice, the side length of the cross sections 9a, 9b is usually between 0.2 mm and 10 mm, preferably between 1 mm and 8 mm, particularly preferably between 2 mm and 6 mm.
[0078] The rectangular front end faces 6a, 6b have a long side length L2 and a short side length L kurz The common base surface 7 is described by the long side length L2 and twice the short side length L1. It should be noted that for greater clarity, Figure 3 A narrow gap is shown between the front faces 6a, 6b in FIG. In practice, the bar-shaped conductors 1a, 1b abut against each other so that the spacing is almost 0, thus 2*L kurz =L1.
[0079] The minimum distance between the weld contour 12 and the outer edge 18 of the common base surface 7 in the direction of the short edge 17 (along the short edge) is referred to as the minimum distance d1. The minimum distance between the weld contour 12 and the outer edge 18 of the common base surface 7 in the direction of the long edge 16 (along the long edge) is referred to as the minimum distance d2. In practice, it has been shown that the circumference of the non-liquid oxide surface layer generally remains undamaged during welding if d1 is selected between 20% and 40% of the length L1, preferably between 25% and 35% of the length L1, and d2 is selected between 20% and 40% of the length L2, preferably between 25% and 35% of the length L2.
[0080] Figure 5 In the variant in which the common base surface 7 is formed in a square, similar Figure 4 Schematic top view of the front faces 6a, 6b of the two bar-shaped conductors 1a, 1b shown in FIG. The coordinate system is selected so that the x-axis points to the right, the y-axis points upwards and the z-axis extends outwards from the plane of the drawing. The front faces 6a, 6b abut one another continuously at the long edges 8a, 8b. The minimum distance between the circular welding contour 12 and the outer edge 18 of the common base surface 7 is called the minimum distance d. The common base surface 7 has an extension L in the direction in which the minimum distance d lies. In the variant shown here, approximately d=0.25*L applies. In practice, the minimum distance d between the welding contour 12 and the outer edge 18 of the common base surface 7 is selected so that d≥15% of the length L, preferably ≥20% of the length L, particularly preferably ≥25% of the length L. The risk of tearing off the non-liquid oxide surface in the peripheral area during welding is thereby reduced to a minimum. If, for example, a pair of bar conductors 1a, 1b is selected with an extension of L=4 mm, which corresponds to dimensions customary in practice, the minimum distance d can be ≥0.6 mm, preferably ≥0.8 mm, particularly preferably ≥1 mm.
[0081] Figure 5Also shown is a machining laser beam 11 on the welding contour 12, which moves past the welding contour 12 at a feed speed v. In practice, it has been found that the feed speed v for the machining laser beam 11 can be advantageously selected such that v≤1600 mm / s, preferably v≤1200 mm / s, particularly preferably v≤800 mm / s. With such a selected feed speed v (e.g. 800 mm / s), the dynamic behavior of the liquid rod-shaped conductor material within the non-liquid oxide surface layer is low and the risk of crack formation in the peripheral region of the non-liquid oxide surface layer is particularly low.
[0082] Within the scope of the laser welding according to the invention, it is advantageous if the processing laser beam 11 is selected as a shaping laser beam 11 a which at least temporarily has a core 23 and a ring 24 . Figure 6a An example of a beam cross section of such a shaped laser beam 11a is shown. The ring 24 surrounds the core 23. This makes it possible to reduce welding defects, in particular at the beginning and at the end of laser welding.
[0083] The shaped laser beam 11a is generated by, for example, a two-in-one optical fiber 27; Figure 6b The cross section of an exemplary two-in-one optical fiber 27 is shown, with which a shaped laser beam for laser welding according to the present invention can be provided. The two-in-one optical fiber 27 has a core optical fiber 25 and a ring optical fiber 26 surrounding the core optical fiber. For example, the core optical fiber diameter KFD of the two-in-one optical fiber 27 can be selected to be 11μm≤KFD≤300μm, preferably 50μm≤KFD≤100μm, and for example, the ring optical fiber diameter RFD of the two-in-one optical fiber 27 can be selected to be 50μm≤RFD≤1000μm, preferably 200μm≤RFD≤400μm.
[0084] The power component P in the core kern and the power component P in the ring ring It can be provided that the primary laser beam is partially introduced into the core fiber 25 and partially introduced into the ring fiber 26, for example by means of an optical wedge (not specifically shown) which is partially pushed into the primary laser beam. Within the framework of the invention, the power distribution between the core and the ring can be selected to be constant or can also be varied over the entire duration of the laser welding of the rod-shaped conductor. kern is the total laser power P of the processing laser beam ges The power component P can be changed by, for example, moving an optical wedge (not specifically shown) to change the components of the original laser beam in the input core fiber 25 and the ring fiber 26 so that the power component P kern , P ring Typically, the total laser power P ges=P kern +P ring is chosen to be constant during the entire welding period.
[0085] In an advantageous variant of the laser welding according to the invention, Figure 7 The constant total laser power P is shown in ges The power component P kern The graph of , as a function of time t, is performed as follows:
[0086] The laser welding of two rod-shaped conductors comprises a first phase (initial phase) EP, a main phase HP and a final phase (final phase) LP, during which a movement is made through the welding contour (for example, a plurality of passes through an elliptical or circular trajectory). In this case, the feed speed can typically be selected to be constant within the total welding duration GD. In the temporal first phase EP (between the time points t0 and t1) and in the temporal final phase LP (between the time points t2 and t3) of the laser welding of the rod-shaped conductors, the power component P of the laser power in the core kern is chosen to be lower than the power component in the main phase HP in between (between time points t1 and t2).
[0087] When the shaped laser beam 11a is injected at the beginning of the first phase EP in time (at time point t0), the low laser power P in the core kern The formation of spatter is reduced, thereby preventing a larger amount of non-liquid oxide surface (and liquid melt) from being ejected. The power component P in the core kern Here, it starts from 30% and then increases (here linearly) in a first temporal phase EP until the desired value of the main phase HP is reached. The choice of the duration of the first phase EP can depend, for example, on whether the vapor capillary generated by the shaped laser beam has reached a certain capillary depth (for example 30% of its maximum capillary depth). The first temporal phase EP of the laser welding usually comprises 10-30% of the total welding duration GD of the welding of the two rod-shaped conductors and can last, for example, between 1 ms and 30 ms.
[0088] In the main phase HP (between time points t1 and t2), the desired component P of the laser power in the core is then kern The movement continues past the welding contour 12. In the variant shown, P kern In the main phase, it is 100%, that is, the ring portion is not irradiated; alternatively, it is also possible to select a P between 60% and 90%, for example. kern .
[0089] After the main phase HP (from time t2 onwards), the component P of the laser power in the core kernThe temperature is reduced again (here linearly) until the desired value (here again 30%) is reached. This ensures that the vapor capillaries generated by the shaped laser beam disappear uniformly, so that only a few pores or no pores at all are obtained in the cooled rod-shaped conductor material. The temporal last phase LP of the laser welding usually comprises 10-30% of the total welding duration GD of the welding and can last, for example, between 1 ms and 30 ms.
[0090] Figure 8a An experimental image of two aluminum-containing rod-shaped conductors is shown directly after the end of laser welding (that is to say before the weld bead solidifies and after the processing laser beam has taken effect), wherein an inhomogeneous weld bead is formed. In this example, the feed speed v for the processing laser beam was selected to be v=3200 mm / s, and the laser power P for the processing laser beam was selected to be P=6 kW; the laser wavelength was 1030 nm, and the total welding time was 85 ms; the rod-shaped conductor was made of the aluminum alloy EN AW-1050A, and the cross-sectional area of the individual hairpins was 2×4 mm, and the welding contour with a circular diameter of 2 mm was located in the center of the end faces of the hairpins that abutted against each other. The high feed speed v causes high dynamics in the melt. As a result, the oxide layer is broken open many times and its union is destroyed, and the low-viscosity melt flows uncontrolled. In the described manner, a defined weld bead with a roughly spherical shape cannot be obtained. This can be seen in the example of FIG. 1 . Figure 8a Irregularly shaped weld beads and scattered wires are seen at the end faces.
[0091] and Figure 8b An experimental image of two aluminum-containing rod-shaped conductors is shown under the conditions of the method according to the invention directly after the end of laser welding (before the weld bead solidifies and after the processing laser beam takes effect), in which a uniform weld bead is formed. In this example, the feed speed v for the processing laser beam was selected to be v=800 mm / s, and the laser power P for the processing laser beam was selected to be P=6 kW; the laser wavelength was 1030 nm, and the total welding time was 85 ms; the rod-shaped conductor was made of the aluminum alloy EN AW-1050A, and the cross-section of the individual hairpins was 2×4 mm, and the welding contour with a circular diameter of 2 mm was located in the center of the end faces of the hairpins that abutted against each other. At the feed speed v selected here, the non-liquid oxide surface layer in the peripheral area remains intact during processing by the processing laser beam. The non-liquid oxide surface layer is only partially broken open on the trajectory of the processing laser beam. In this way, a defined weld bead with an intact non-liquid oxide surface layer and a roughly spherical shape can be obtained, as in Figure 8b As can be clearly seen in .
[0092] Reference numerals list
[0093] 1a, 1b Rod-shaped conductor
[0094] 2a, 2b (outer) legs
[0095] 3a, 3b (Inner) Leg
[0096] 4a, 4b Middle part
[0097] 5a, 5b End region
[0098] 6a, 6b Front face
[0099] 7 Common base
[0100] 8a, 8b Long side
[0101] 9a, 9b Cross section
[0102] 11 Processing laser beam
[0103] 11a Shaping the laser beam
[0104] 12 Welding profile
[0105] 13 Regions
[0106] 14 Non-liquid oxide surface
[0107] 15 Liquid rod-shaped conductor material
[0108] 16 Long Edge
[0109] 17 Short Edge
[0110] 18 Outer edge
[0111] 19 Welding beads
[0112] 20 End side
[0113] 21 Circumference area
[0114] 22 Connected cross-section
[0115] 23 Core
[0116] 24 Ring
[0117] 25-core fiber
[0118] 26 Ring Fiber
[0119] 27 2-in-1 optical fiber
[0120] dMinimum spacing
[0121] d1 minimum spacing (along the short edge direction)
[0122] d2 minimum spacing (along the long edge direction)
[0123] EP Phase 1 (Initial Phase)
[0124] HP Main Stage
[0125] H sp Bead height
[0126] H unv Height of undamaged peripheral area
[0127] KFD core fiber diameter
[0128] LP final stage (final stage)
[0129] L extension (along the direction of the minimum spacing d)
[0130] L1 Twice the shorter side length
[0131] L2 long side length
[0132] L kurz Short side length
[0133] P Laser power
[0134] P ges Total laser power
[0135] P kern Laser power in the core
[0136] P ring Laser power in the ring
[0137] RFD Ring Fiber Diameter
[0138] v Feed rate.
Claims
1. A method for laser welding rod-shaped conductors (1a, 1b), in, The bar-shaped conductor (1a, 1b) consists of an aluminum-containing bar-shaped conductor material having an aluminum content of at least 75% by weight, Two bar conductors (1a, 1b) are arranged partially overlapping and lying side by side and are welded to one another by means of a processing laser beam (11), a weld bead (19) being formed on a common base surface (7) of the bar conductors (1a, 1b) lying side by side, by means of which the bar conductors (1a, 1b) are connected to one another. It is characterized in that During laser welding of the bar-shaped conductors (1a, 1b), the processing laser beam (11) is guided in such a way that a welding contour (12) of the processing laser beam (11) is positioned relative to the bar-shaped conductors (1a, 1b) and a feed speed v of the processing laser beam (11) along the welding contour (12) relative to the bar-shaped conductors (1a, 1b) is selected such that: During laser welding of the rod-shaped conductor (1a, 1b), the weld bead (19) has a non-liquid oxide surface layer (14), inside which liquid rod-shaped conductor material (15) accumulates, wherein during laser welding of the rod-shaped conductors (1a, 1b), the non-liquid oxide surface layer (14) is only partially broken open by the processing laser beam (11) at the upwardly pointing end side (20) of the weld bead (19) corresponding to the weld contour (12), - wherein, during laser welding of the rod-shaped conductor (1a, 1b), the non-liquid oxide surface layer (14) remains intact in a peripheral region (21) of the weld bead (19), the peripheral region extending downwardly away from the upper end side (20) towards the rod-shaped conductor (1a, 1b) and around the entire weld bead (19).
2. The method according to claim 1, characterized in that The welding contour (12) of the processing laser beam (11) is positioned relative to the rod-shaped conductor (1a, 1b) such that for a minimum distance d of the welding contour (12) from an outer edge (18) of the common base surface (7) and for an extension L of the common base surface (7) in the direction in which the minimum distance d lies the following applies: d≥0.15*L.
3. The method according to claim 2, characterized in that The minimum distance d and the extension L apply: d≥0.20*L.
4. The method according to claim 2, characterized in that: The minimum distance d and the extension L apply: d≥0.25*L.
5. The method according to any one of claims 1 to 4, characterized in that A welding contour (12) of the machining laser beam (11) is positioned relative to the rod-shaped conductor (1a, 1b) such that for a minimum distance d between the welding contour (12) and an outer edge (18) of the common base surface (7): d≥0.6mm.
6. The method according to claim 5, characterized in that The minimum distance d applies when: d≥0.8mm.
7. The method according to claim 5, characterized in that The minimum distance d applies when: d≥1.0mm.
8. The method according to any one of claims 1 to 4, characterized in that For the feed speed v of the machining laser beam (11) along the welding contour (12) of the machining laser beam (11) relative to the rod-shaped conductor (1a, 1b), the following applies: v≤1600mm / s.
9. The method according to claim 8, characterized in that The feed speed v applies for: v≤1200mm / s.
10. The method according to claim 8, characterized in that The feed speed v applies for: v≤800mm / s.
11. The method according to any one of claims 1 to 4, characterized in that The laser welding is performed in an oxygen-containing atmosphere.
12. The method according to claim 11, characterized in that The laser welding is performed in air.
13. The method according to any one of claims 1 to 4, characterized in that At least during the second half of the laser welding of the rod-shaped conductors (1a, 1b), the peripheral area (21) where the non-liquid oxide surface layer (14) remains intact is located at a height (H) of the weld bead (19). sp ) extends over at least 3 / 4 of the 14. The method according to claim 13, characterized in that The peripheral area (21) is at a height (H) of the welding bead (19). sp ) extends over at least 9 / 10 ).
15. The method according to any one of claims 1 to 4, characterized in that The two bar-shaped conductors (1a, 1b) are arranged parallel to each other and abutting each other with their end regions (5a, 5b), wherein the front faces (6a, 6b) of the bar-shaped conductors (1a, 1b) are located at the same height with respect to the direction of the longitudinal extension of the end regions (5a, 5b) of the bar-shaped conductors (1a, 1b), The machining laser beam (11) is directed toward the front end faces (6a, 6b) of the rod-shaped conductors (1a, 1b), and the front end faces (6a, 6b) provide the common base surface (7) on which the welding bead (19) is formed.
16. The method according to claim 15, characterized in that in, The end regions (5a, 5b) of the bar-shaped conductors (1a, 1b) are pressed flat against one another.
17. The method according to claim 15, characterized in that The end regions (5a, 5b) of the bar-shaped conductors (1a, 1b) point vertically upwards.
18. The method according to claim 17, characterized in that The front faces (6a, 6b) are oriented horizontally.
19. The method according to claim 15, characterized in that The machining laser beam (11) is incident perpendicularly on the front face (6a, 6b).
20. The method according to any one of claims 1 to 4, characterized in that The bar-shaped conductors (1a, 1b) each have a rectangular cross section (9a, 9b) at least close to the common base surface (7), the rectangular cross section having a side length (L) between 0.2 mm and 10 mm. kurz , L2).
21. The method according to claim 20, characterized in that The bar-shaped conductors (1a, 1b) each have a rectangular cross section (9a, 9b) in a respective end region (5a, 5b).
22. The method according to claim 20, characterized in that The rectangular cross section has a side length (L between 1 mm and 8 mm) kurz , L2).
23. The method according to claim 20, characterized in that The rectangular cross section has a side length (L kurz , L2).
24. The method according to claim 20, characterized in that In the corresponding rod-shaped conductor (1a, 1b), the long side length L2 is equal to the short side length L kurz and the cross-sections (9a, 9b) of the two welded bar-shaped conductors (1a, 1b) are the same.
25. The method according to claim 20, characterized in that A minimum distance d2 between the welding contour (12) and the outer edge (18) of the common base surface (7) in the direction of the corresponding long edge (16) is between 20% and 40% of the corresponding long side length L2, and a minimum distance d1 between the welding contour (12) and the outer edge (18) of the common base surface (7) in the direction of the corresponding short edge (17) is between 20% and 40% of twice the short side length L1.
26. The method according to claim 25, characterized in that The minimum distance d2 is between 25% and 35% of the associated long side length L2.
27. The method according to claim 25, characterized in that The minimum distance d1 is between 25% and 35% of twice the short side length L1.
28. The method according to any one of claims 1 to 4, characterized in that The machining laser beam (11) has a laser power P, wherein 0.5 kW≤P≤20 kW, and / or the wavelength of the machining laser beam (11) is between 400 nm and 1200 nm.
29. The method according to claim 28, characterized in that 2kW≤P≤10kW.
30. The method according to claim 28, characterized in that 4kW≤P≤8kW.
31. The method according to any one of claims 1 to 4, characterized in that The welding contour (12) is selected to be linear, circular or oval and is passed over multiple times during the laser welding of the rod-shaped conductors (1a, 1b).
32. The method according to claim 31, characterized in that The welding contour (12) is generated by means of scanning optics.
33. The method according to any one of claims 1 to 4, characterized in that A shaped laser beam (11a) having a core (23) and a ring (24) which surrounds the core (23) in an annular manner is selected as the machining laser beam (11) at least temporarily.
34. The method according to claim 33, characterized in that The shaped laser beam (11a) is generated by means of a two-in-one optical fiber (27), the two-in-one optical fiber having a core fiber diameter KFD, wherein 11 μm≤KFD≤300 μm, and the two-in-one optical fiber having a ring fiber diameter RFD, wherein 50 μm≤RFD≤1000 μm.
35. The method according to claim 34, characterized in that 50μm≤KFD≤100μm.
36. The method according to claim 34, characterized in that 200μm≤RFD≤400μm.
37. The method according to claim 33, characterized in that The power component P of the laser power in the core (23) kern is selected to be smaller during a first temporal phase (EP) of the laser welding of the bar-shaped conductors (1a, 1b) than during a main phase (HP) of the laser welding of the bar-shaped conductors (1a, 1b).
38. The method according to claim 37, characterized in that The power component P of the laser power in the core (23) kern It increases continuously during the first phase (EP).
39. The method according to claim 37, characterized in that The first phase (EP) has a duration between 1 ms and 30 ms.
40. The method according to claim 33, characterized in that The power component P of the laser power in the core (23) kern During a temporal last phase (LP) of the laser welding of the bar-shaped conductors (1a, 1b) is smaller than during a main phase (HP) of the laser welding of the bar-shaped conductors (1a, 1b).
41. The method according to claim 40, characterized in that The power component P of the laser power in the core (23) kern Decreases continuously during the last phase (LP).
42. The method according to claim 40, characterized in that The last phase (LP) has a duration between 1 ms and 30 ms.
43. The method according to any one of claims 1 to 4, characterized in that The bar-shaped conductors (1a, 1b) are bent bar-shaped conductors (1a, 1b).
44. The method according to claim 43, characterized in that The bar-shaped conductor (1a, 1b) is a bent bar-shaped conductor (1a, 1b) used for a hairpin of a motor or a generator.
45. The method according to any one of claims 1 to 4, characterized in that The aluminum-containing rod-shaped conductor material has an aluminum content of at least 90% by weight.
46. The method according to any one of claims 1 to 4, characterized in that The common base surface (7) is oriented horizontally.
47. A bar-type conductor arrangement comprising at least two bar-type conductors (1a, 1b) welded by means of a method according to any one of claims 1 to 46.
48. An application of a rod-shaped conductor assembly, wherein: The bar-type conductor arrangements are each produced by welding two bar-type conductors (1a, 1b) by means of a method according to any one of claims 1 to 46, and are installed in an electric motor or a generator.