Double perovskite material and preparation method thereof and reversible proton ceramic electrochemical cell

By doping Cs+ in double perovskite materials, the oxygen vacancies and Lewis acidity of the oxide are improved, and the problem of low electrochemical performance of reversible proton ceramic electrochemical cells at medium and low temperatures is solved, and high catalytic activity and stability are achieved. Air electrodes significantly improve the electrochemical performance and stability of the battery.

CN117334933BActive Publication Date: 2024-11-26ZIJIN MINING RENEWABLE ENERGY & ADVANCED MATERIALS (CHANGSHA) CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310902714.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-21
Publication Date
2024-11-26
Estimated Expiration
2043-07-21

AI Technical Summary

Technical Problem

The existing reversible proton ceramic electrochemical cells have slow reaction kinetics of air electrodes at medium and low temperatures, resulting in low electrochemical performance and lack of stability, making it difficult to achieve high catalytic activity.

Method used

Using the bisperovskite material PrBa1-xCsxCo2O6-δ doped with low Lewis acid intensity cation Cs+ as the air electrode, the oxygen vacancies content and Lewis acidity polarization distribution of the oxide are enhanced through the A-position doping of Cs+, and redox and oxygen are enhanced. The catalytic activity of the precipitation reaction and the crystallinity strength and stability of the material are improved by specific preparation methods.

Benefits of technology

It significantly improves the electrochemical performance and stability of reversible proton ceramic electrochemical cells at medium and low temperatures, reduces polarization impedance, improves oxygen ion exchange kinetics and electrocatalytic activity, and achieves better electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117334933B_ABST
    Figure CN117334933B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of reversible proton ceramic electrochemical cells, and in particular to a double perovskite material and a preparation method thereof and a reversible proton ceramic electrochemical cell. The double perovskite material is expressed as: PrBa 0.9 Cs 0.1 Co 2 O 6‑δ , wherein δ is the oxygen vacancy content. The present invention also provides a method for preparing the double perovskite material and a reversible proton ceramic electrochemical cell comprising the double perovskite material. The Cs + The doped double perovskite material has good stability, low polarization impedance and high ORR / OER activity; the reversible proton ceramic electrochemical cell provided by the present invention has good stability, electrocatalytic activity and electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of reversible proton ceramic electrochemical cells, and in particular to a double perovskite material and a preparation method thereof, and a reversible proton ceramic electrochemical cell. Background Art

[0002] Due to the limited storage of fossil fuels and the increasing greenhouse gas emissions, there is an urgent need to find a clean and pollution-free energy conversion device to alleviate the current energy and environmental crisis. Reversible proton ceramic electrochemical cell (R-PCEC) technology can be used as one of the effective means to solve the current problem. When the reversible proton ceramic electrochemical cell operates in fuel cell mode, chemical energy can be converted into electrical energy; when it operates in electrolysis mode, electrical energy can be converted into chemical energy. In addition, R-PCEC based on proton conductor electrolyte has high proton conductivity and can operate at medium and low temperatures (400-700℃). The lower operating temperature of R-PCEC is not only beneficial to extend the life of the battery itself, but also to reduce production costs. However, as the operating temperature of R-PCEC decreases, the reaction kinetics of the air electrode becomes sluggish, which significantly reduces the electrochemical performance of R-PCEC. Therefore, designing an air electrode material with high catalytic activity for oxygen reduction (ORR) / oxygen evolution (OER) reactions and sufficient chemical stability under medium and low temperature conditions is one of the most significant challenges facing R-PCEC.

[0003] In recent years, researchers have designed many air electrode materials, but most of them show moderate electrochemical performance in R-PCEC. 6-δ (PBC) has excellent electronic conductivity, oxygen ion conductivity, excellent oxygen surface exchange coefficient and oxygen ion diffusion kinetics, and it exhibits excellent electrochemical performance as the air electrode of solid oxide fuel cells (SOFC). Although cesium (Cs) is used in the design of perovskite solar cell materials, this is because the doping of Cs can improve the thermal stability and moisture resistance of the material's crystal structure. Density functional theory (DFT) calculations show that the improvement in the ORR activity of the air electrode after doping with Cs is mainly due to the electron pair offset caused by the polarization distribution of Lewis acidity intensity at the A and B sites, thereby reducing the oxygen vacancy formation energy of the oxide. At present, there are few reports on the application of air electrodes designed by doping Cs at the A site to R-PCEC. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a double perovskite material and a preparation method and a reversible proton ceramic electrochemical cell. +The present invention also provides the above-mentioned low Lewis acid strength cation Cs + Preparation method of doped double perovskite material. Based on the double perovskite material, the present invention also provides a reversible proton ceramic electrochemical cell, which has excellent electrochemical performance and also exhibits good stability.

[0005] Specifically, in the first aspect, the double perovskite material provided by the present invention has an expression of: PrBa 1-x Cs x Co2O 6-δ ; Where δ is the oxygen vacancy content.

[0006] According to the present invention, when an A-site dopant with lower acidity is doped, it is beneficial to improve the hydration capacity of the perovskite oxide. In addition, when Cs is used as an A-site cation dopant in the air electrode of a fuel cell, the kinetics of the redox reaction of the air electrode is closely related to the Lewis acid strength of the doped ion. + When used as an A-site dopant, the polarized distribution of the Lewis acid strength of the A-site and B-site ions leads to electron pair shift, increasing the oxygen vacancy content in the oxide, which in turn helps improve the oxygen exchange kinetics on the electrode surface and accelerate the redox reaction process. + The doping of low Lewis acid strength cation Cs + Partially replace Ba in double perovskite oxide PBC. Further, the present invention designs and prepares a new double perovskite material PrBa 1-x Cs x Co2O 6-δ (PBCsC) was used as the air electrode of R-PCEC to evaluate its electrocatalytic activity and water splitting ability at medium and low temperatures. It has important practical significance for designing an air electrode with high catalytic activity and stability and applying it to R-PCEC.

[0007] Preferably, the value range of x is 0.01 to 0.15.

[0008] More preferably, the value range of x is 0.05 to 0.125.

[0009] Preferably, the double perovskite material is a tetragonal layered perovskite structure. The double perovskite material has a perovskite structure doped with Cs at the A position. In the present invention, the ionic radius of Cs is 167 pm, and the ionic radius of Ba is 135 pm. The ionic radius of Ba is the closest to that of Cs (Pr 3+ and Pr4+ The ionic radius is 99 and 85 pm; Co 2+ ,Co 3+ ,Co 4+ The ionic radius is 74.5, 61, 53 pm), Cs + Substitute the Ba ions in the structure.

[0010] Further preferably, the lattice parameter a is b is c is

[0011] Further preferably, the expression of the double perovskite material is: PrBa 0.9 Cs 0.1 Co2O 6-δ , where 0.1≤δ≤0.3.

[0012] According to the present invention, experimental studies have further found that the PBCsC of the present invention using the above-mentioned x value has excellent electrocatalytic performance, especially when the preferred x=0.1 is used for partial substitution of Ba, which can unexpectedly make the reversible proton ceramic electrochemical cell have better electrochemical performance and stability than other values.

[0013] In a second aspect, the method for preparing the double perovskite material provided by the present invention comprises the following steps:

[0014] 1) dissolving praseodymium nitrate, barium nitrate, cesium nitrate and cobalt nitrate in water to obtain a mixed solution; then mixing the mixed solution, ethylenediaminetetraacetic acid, citric acid and ammonia water, and adjusting the pH to 7-8 to obtain a mixed solution;

[0015] 2) heating the mixed solution to a gel state, performing high temperature treatment at 200-250° C. to obtain a precursor, and calcining the precursor.

[0016] Preferably, in step 1), the molar ratio of metal element, ethylenediaminetetraacetic acid and citric acid is 0.5-1.5:0.5-1.5:1-2, preferably 1:1:1.5; wherein the metal element is the sum of Pr, Ba, Cs and Co. Experimental studies have found that the present invention uses a specific ratio of metal elements, ethylenediaminetetraacetic acid and citric acid, combined with the preferred calcination temperature of the present invention, can significantly improve the PrBa 0.9 Cs 0.1 Co2O 6-δ The phase effect (crystallization strength) makes PrBa 0.9 Cs 0.1 Co2O 6-δ Shows a better crystal structure.

[0017] Preferably, in step 2), the mixed solution is heated to a temperature of 80-100°C.

[0018] Preferably, in step 2), the high temperature treatment time is 2 to 6 hours, preferably 2 hours.

[0019] Preferably, in step 2), the calcination temperature is 950-1050° C., preferably 1000° C.; the calcination time is 2-4 h, preferably 2 h.

[0020] In the present invention, the raw materials used in combination with the preferred preparation conditions can achieve a better phase formation effect, which is conducive to the preparation of PrBa with better crystal strength and crystal structure. 0.9 Cs 0.1 Co2O 6-δ The further prepared reversible proton ceramic electrochemical cell can have better comprehensive performance in terms of electrochemical performance and stability.

[0021] In a third aspect, the present invention also provides an application of the double perovskite material, which is an application of the double perovskite material as an air electrode in a reversible proton ceramic electrochemical cell.

[0022] In a fourth aspect, the present invention also provides a reversible anode-supported proton ceramic electrochemical cell, the reversible proton ceramic electrochemical cell comprising an anode support layer, an electrolyte and an air electrode connected in sequence; the air electrode is composed of the above-mentioned (low Lewis acid strength cation Cs + It is prepared by doped) double perovskite material.

[0023] Preferably, the electrolyte material comprises BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ (BZCYYb1711), where δ is the oxygen vacancy content (0≤δ≤0.2).

[0024] Preferably, the material of the anode support layer comprises NiO and BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ Among them, NiO and BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ The mass ratio of is 5.5-6.5:3.5-4.5, preferably 6:4, and δ is the oxygen vacancy content.

[0025] Preferably, the reversible proton ceramic electrochemical cell further comprises a transition layer, which is disposed between the anode support layer and the electrolyte; preferably, the transition layer comprises NiO and BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ (BZCYYb1711); among them, NiO and BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ The mass ratio of is 5.5-6.5:3.5-4.5, preferably 6:4, and δ is the oxygen vacancy content.

[0026] According to the present invention, the term δ in each layer of the reversible proton ceramic electrochemical cell refers to the oxygen vacancy content. If the present invention does not limit its range, it means that the conventional oxygen vacancy content range in the art can be adopted, such as 0-0.5, 0.1-0.4 or 0.1-0.2.

[0027] In the present invention, the anode-supported proton ceramic electrochemical cell adopts a co-casting method, and the electrolyte layer, the transition layer and the anode layer are tightly connected without separation between the layers, which can significantly improve the stability of the half-cell structure, improve and reduce the resistance of the half-cell caused by the connection, and make the anode-supported proton ceramic electrochemical cell show more excellent electrochemical performance.

[0028] Further preferably, the method for preparing the reversible anode-supported protonic ceramic electrochemical cell comprises the following steps:

[0029] 1) preparing the material of the anode support layer, the material of the transition layer, the material of the electrolyte and the material of the air electrode into slurries respectively;

[0030] 2) Casting electrolyte slurry, transition layer slurry, and anode support layer slurry in sequence on a casting machine; then drying naturally for 10 to 14 hours, degreasing the naturally dried co-cast thin sheet, and calcining at high temperature to obtain an anode-supported half-cell; preferably, the heat treatment degreasing condition is a heat treatment at 500 to 700° C. for 1 to 3 hours; the high-temperature calcination condition is a high-temperature calcination at 1400 to 1500° C. for 4 to 6 hours;

[0031] 3) The material of the air electrode is prepared into a slurry, which is brushed onto the electrolyte surface of the half-cell and calcined at high temperature to obtain a reversible anode-supported proton ceramic electrochemical full cell; preferably, the high-temperature calcination condition is 800-1000° C. for 1-3 hours.

[0032] More preferably, the substrate is a polymer film.

[0033] More preferably, the electrolyte layer slurry is obtained by ball milling BZCYYb1711 powder, a dispersant and anhydrous ethanol.

[0034] More preferably, the transition layer slurry is obtained by blending BZCYYb1711 powder, nano nickel oxide, graphite, a dispersant, anhydrous ethanol and butyl acetate, and ball milling for 12 hours.

[0035] More preferably, the anode support layer slurry is obtained by mixing BZCYYb1711, nickel oxide, graphite, a dispersant, anhydrous ethanol and butyl acetate, and ball milling for 10 to 14 hours.

[0036] More preferably, the air electrode slurry is PrBa 0.9 Cs 0.1 Co2O 6-δ The material is blended with pine alcohol; the slurry composition is 1g: 0.5-0.7g of PrBa 0.9 Cs 0.1 Co2O 6-δ and terpineol.

[0037] More preferably, in the anode-supported half-cell, the thickness of the electrolyte layer is 7 to 9 μm, the thickness of the anode support layer is 600 to 700 μm, and the thickness of the transition layer is 16 to 22 μm.

[0038] In the present invention, experimental studies have found that when the above-mentioned preferred high-temperature calcination temperature and time parameters are used to prepare an anode-supported half-cell, the mechanical strength of the half-cell can be improved by adjusting the thickness of the anode support layer, and the anode-supported half-cell can exhibit better structural stability.

[0039] The beneficial effects of the present invention are at least that: the low Lewis acid strength cation Cs + Doped double perovskite material is a double perovskite material PrBaCo2O 6-δ Based on the sol-gel method, the element is doped at the A position. Anode-supported reversible proton ceramic electrochemical cell air electrode material PrBa prepared by sol-gel method 0.9 Cs 0.1 Co2O 6-δ (PBCsC). The anode-supported reversible proton ceramic electrochemical cell air electrode material of the present invention has lower polarization impedance and higher electrocatalytic activity. The polarization resistance of the anode-supported single cell NiO-BZCYYb1711||transition layer NiO-BZCYYb1711||BZCYYb1711||PBCsC prepared by the present invention at 650°C, 600°C, 550°C and 500°C is 0.045Ωcm respectively. 2 , 0.094Ωcm 2, 0.273Ωcm 2 and 1.037Ωcm 2 , the maximum power density is: 1.66W cm -2 ,1.19W cm -2 ,0.72W cm -2 , and 0.41 W cm -2 When humidified air was introduced into the air electrode side, the R-PCEC was operated in the electrolysis mode, and the current density was -2.85 A cm at 650 °C, 600 °C, 550 °C, and 500 °C and 1.3 V, respectively. -2 , -1.48A cm -2 , -0.71Acm -2 , and -0.31A cm -2 The anode-supported reversible proton ceramic electrochemical cell of the present invention has excellent stability, oxygen ion exchange kinetics, electrocatalytic activity and electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the embodiments of the present invention and the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0041] Figure 1 The air electrode material PrBa involved in Example 1 of the present invention 0.9 Cs 0.1 Co2O 6-δ XRD refinement pattern of (PBCsC) after calcination at 1000℃ for 2 hours;

[0042] Figure 2 The air electrode material PrBa involved in Example 1 of the present invention 0.9 Cs 0.1 Co2O 6-δ XRD pattern of (PBCsC) and electrolyte BZCYYb powder after co-firing at 950℃ for 2h in a high-temperature muffle furnace;

[0043] Figure 3 The air electrode material PrBa involved in Example 1 of the present invention 0.9 Cs 0.1 Co2O 6-δ (PBCsC), XRD pattern after treatment at 600 °C and 30% water for 10 h;

[0044] Figure 4 The air electrode material PrBa involved in Example 1 of the present invention0.9 Cs 0.1 Co2O 6-δ (PBCsC), high temperature in situ XRD pattern after calcination at 1000 °C for 2 h;

[0045] Figure 5 The X-ray photoelectron spectra (XPS) of the air electrode materials PBCsC and PBC involved in Example 1 of the present invention, wherein a is Pr 3d and b is Co 2p;

[0046] Figure 6 The O1s X-ray photoelectron spectra of the air electrode materials PBCsC (6a) and PBC (6b) involved in Example 1 of the present invention;

[0047] Figure 7 This is a relaxation characterization diagram of the air electrode materials PBCsC and PBC involved in Example 1 of the present invention;

[0048] Figure 8 The area ratio impedance diagram (8a) and impedance stability diagram (8b) of the symmetrical battery PBCsC as the electrode and BZCYYb1711 as the electrolyte support in humidified air (3% H2O) involved in Example 1 of the present invention;

[0049] Fig. 9 The electrochemical stability of the symmetrical battery PBCsC and PBC as electrodes and BZCYYb1711 as the electrolyte support in humidified air (3% H2O) according to Example 1 of the present invention;

[0050] Fig.10 The infrared spectra of PBCsC and PBC oxide involved in Example 1 of the present invention after being treated at 600° C. in air containing 30% water vapor for 50 hours;

[0051] Fig.11 When PBCsC is used as the air electrode in Example 2 of the present invention, the highest power density diagram of a single cell (Ni-BZCYYb1711||transition layer Ni-BZCYYb1711||BZCYYb1711||PBCsC) prepared with Ni-BZCYYb1711 as the fuel electrode support is tested in the FC mode (humidified hydrogen is introduced into the anode side and ambient air is introduced into the oxygen electrode side) in the range of 650-500°C;

[0052] Fig.12When PBCsC is used as the air electrode in Example 2 of the present invention, a single cell (Ni-BZCYYb1711||transition layer Ni-BZCYYb1711||BZCYYb1711||PBCsC) prepared with Ni-BZCYYb1711 as the fuel electrode support is tested in the EC mode (humidified hydrogen is introduced into the anode side and humidified air is introduced into the oxygen electrode side) in the range of 650 to 500°C, and the current density diagram corresponding to 1.3V;

[0053] Fig.13 This is an operational stability diagram of a single cell (Ni-BZCYYb1711||transition layer Ni-BZCYYb1711||BZCYYb1711||PBCsC) prepared in Example 2 of the present invention with PBCsC as the air electrode and Ni-BZCYYb1711 as the anode support, tested at 650°C in a single cell fuel cell mode and an electrolytic cell mode;

[0054] Fig.14 A graph of the cycle stability of a single cell (Ni-BZCYYb1711||transition layer Ni-BZCYYb1711||BZCYYb1711||PBCsC) prepared in Example 2 of the present invention with PBCsC as the air electrode and Ni-BZCYYb1711 as the fuel electrode support and tested at 600°C;

[0055] Fig.15 A graph showing the variation of the Faraday efficiency of a single cell with the applied current density of a single cell (Ni-BZCYYb1711||transition layer Ni-BZCYYb1711||BZCYYb1711||PBCsC) prepared in Example 2 of the present invention with PBCsC as the air electrode and Ni-BZCYYb1711 as the anode support layer;

[0056] Fig.16 This is a graph showing the change in hydrogen production rate with applied current density of a single cell (Ni-BZCYYb1711||transition Ni-BZCYYb1711||BZCYYb1711||PBCsC) prepared in Example 2 of the present invention with PBCsC as the air electrode and Ni-BZCYYb1711 as the anode support layer. DETAILED DESCRIPTION

[0057] In order to make the purpose, technical solution and advantages of the embodiments of the invention clearer, the technical solution in the embodiments of the invention is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the invention, not all of the embodiments. Based on the embodiments of the invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the invention.

[0058] Unless otherwise specified, the raw materials and reagents used in the following examples are all commercially available products or can be prepared by known methods. If no specific techniques or conditions are specified in the examples, they are all conventional methods or the techniques or conditions described in the literature in this field, or according to the product instructions. If the manufacturers of the reagents and instruments are not specified, they are all conventional products that can be purchased through regular channels.

[0059] The present invention will be further described below with reference to the embodiments.

[0060] The embodiment of the present invention relates to a low Lewis acid strength cation Cs + Preparation and characterization of doped air electrode materials, the composition of which is PrBa 0.9 Cs 0.1 Co2O 6-δ (PBCsC). By using the perovskite material PrBaCo2O 6-δ The Cs ion doping at the A position in the anode improves the oxygen reduction / evolution reaction activity and stability of the anode-supported reversible proton ceramic electrochemical cell. + A-site doping, PrBa 0.9 Cs 0.1 Co2O 6-δ The catalytic activity and stability of the (PBCsC) air electrode have been improved. At 650°C, the maximum output power of a single cell composed of Ni-BZCYYb1711|transition layer Ni-BZCYYb1711|BZCYYb1711|PBCsC in FC mode reached 1.66W cm -2 , and the polarization resistance of the battery is only 0.045Ωcm 2 When air containing 3% water vapor was introduced into the air electrode side, a -2.85A cm -2 The present invention uses a low Lewis acid strength cation Cs + The doping of PrBaCo2O can significantly reduce 6-δ The polarization impedance of the air electrode is reduced and the electrochemical performance of the whole battery is improved. The current density can also be greatly increased in the electrolysis mode, while also showing excellent stability.

[0061] In addition, there are relatively few studies on the cycle stability of reversible proton ceramic electrochemical cells supported by medium and low temperature anodes, and there are very few methods for characterizing the stability of reversible proton ceramic electrochemical cells. In order to characterize the cycle stability of the reversible proton ceramic electrochemical cell involved in the present invention, the embodiment of the present invention also provides a characterization test method. The main steps are: brush the air electrode material on the electrolyte membrane of the anode-supported proton conductor single cell, introduce hydrogen containing 3% water vapor on the anode side, and introduce air containing 3% water vapor on the air electrode side. The single cell is tested for cycle stability, that is, by applying ±0.5A cm -2 The anode-supported reversible protonic ceramic electrochemical cell was operated alternately in fuel cell mode and electrolyzer mode with a current of 100 Ω, thereby evaluating the electrochemical stability of the air electrode.

[0062] In the following examples: the comparative sample PBC, whose composition is PrBaCo2O 6-δ , and its preparation process is the same as that in the embodiment.

[0063] Example 1

[0064] This embodiment provides an anode-supported reversible proton ceramic electrochemical cell air electrode material PrBa 0.9 Cs 0.1 Co2O 6-δ The preparation method comprises the following specific steps:

[0065] 1) According to the stoichiometric ratio, praseodymium nitrate, barium nitrate, cesium nitrate and cobalt nitrate are mixed in the following manner: PrBa 0.9 Cs 0.1 Co2O 6-δ The stoichiometric ratio of (PBCsC) was added to the deionized water solution in sequence. Subsequently, citric acid was added at 1.5 times the molar amount of the metal ions, and ethylenediaminetetraacetic acid was added at 1 times the molar amount of the metal ions; wherein praseodymium nitrate, barium nitrate, cesium nitrate, cobalt nitrate, citric acid and ethylenediaminetetraacetic acid were purchased from Aladdin Chemical Reagent Network.

[0066] 2) After adding the complexing agent to the solution containing the metal ions, adding ammonia water, adjusting the pH value to 7-8, and then heating and stirring under magnetic stirring until the water evaporates to obtain a gel-like substance;

[0067] 3) placing the gel-like substance in a forced air drying oven at 250° C. to dry for 2 hours to obtain a fluffy porous precursor;

[0068] 4) The precursor is placed in a high temperature muffle furnace and calcined at 1000°C for 2 hours to obtain the desired air electrode material powder PrBa 0.9 Cs 0.1 Co2O 6-δ(denoted as PBCsC) where 0.1≤δ≤0.3.

[0069] Example 2

[0070] In this embodiment, a PrBa provided in Example 1 is provided. 0.9 Cs 0.1 Co2O 6-δ (PBCsC) is used as the air electrode of the battery to prepare a reversible anode-supported proton ceramic electrochemical cell of Ni-BZCYYb1711|transition layer Ni-BZCYYb1711|BZCYYb1711|PBCsC, which specifically comprises the following steps:

[0071] (1) Preparation of electrolyte layer slurry: 3 g BZCYYb1711 powder, 0.1 g fish oil dispersant, 0.8 g anhydrous ethanol, and 0.8 g butyl acetate were uniformly mixed to obtain BZCYYb1711 electrolyte layer slurry; Preparation of transition layer slurry: 1.2 g BZCYYb1711 powder, 1.8 g nano nickel oxide, 0.3 g graphite, 0.1 g fish oil dispersant, 0.75 g anhydrous ethanol, and 0.75 g butyl acetate were uniformly mixed to obtain Ni-BZCYYb1711 transition layer slurry; Preparation of anode support layer slurry: 10 g BZCYYb1711, 15 g nickel oxide, 1.5 g graphite, 1 g fish oil dispersant, 3 g anhydrous ethanol, and 3 g butyl acetate were uniformly mixed to obtain anode slurry; the above slurries were placed on a drum ball mill and ball milled for 30 to 40 hours.

[0072] (2) The electrolyte slurry, transition layer slurry and anode slurry after ball milling and blending are sequentially cast on a PET (polyethylene terephthalate) release film polymer film, and then the co-cast electrolyte layer-transition layer-anode support layer film is placed in the air to dry naturally for 12 hours, and then a molding mold with a diameter of 15 mm is used to cut it into several thin slices with a diameter of 15 mm, and the thin slices are placed in a muffle furnace and degreased at 600°C for 2 hours; finally, the degreased thin slices are placed in a high-temperature muffle furnace and calcined at 1450°C for 5 hours to obtain the desired anode-supported half-cell; wherein the prepared anode-supported half-cell includes a BZCYYb1711 electrolyte layer (thickness of 7 to 9 μm), a Ni-BZCYYb1711 transition layer (thickness of 30 μm) and a Ni-BZCYYb1711 anode support layer (thickness of 600 to 700 μm);

[0073] (3) Weigh 1 g of the air electrode powder PrBa prepared in Example 1 0.9 Cs 0.1 Co2O 6-δ Mix evenly with 0.6 g of pinene alcohol to obtain the desired air electrode slurry.

[0074] (4) The prepared air electrode slurry was brushed onto the electrolyte membrane of the half-cell and then placed in an oven at 70°C. After the cathode slurry was dried, the assembled full cell was calcined at 950°C for 2 h in a high-temperature muffle furnace for electrochemical performance testing in FC and EC modes.

[0075] Characterization results

[0076] 1. XRD characterization

[0077] Figure 1 PrBa 0.9 Cs 0.1 Co2O 6-δ The XRD refinement of the (PBCsC) powder after calcination at 1000℃ for 2h shows that the synthesized PBCsC exhibits a single double perovskite phase structure. At the same time, the XRD refinement results show that the synthesized PBCsC is a tetragonal layered perovskite structure with a lattice parameter of (Refinition parameters: GOF = 2.13).

[0078] Figure 2 The chemical compatibility of the synthesized air electrode material PBCsC and the electrolyte BZCYYb1711 powder. As can be seen from the figure, after PBCsC and BZCYYb1711 were mixed and calcined at 950℃ for 2h in a high-temperature muffle furnace, no chemical reaction occurred, indicating that PBCsC material has good chemical compatibility with BZCYYb1711 powder.

[0079] Figure 3 PrBa 0.9 Cs 0.1 Co2O 6-δ XRD image of (PBCsC) powder after treatment at 600℃ in air containing 30% water vapor for 10h. The main peak of the XRD image of the treated PBCsC is obviously shifted to a lower angle, which may be due to the expansion of the lattice caused by the entry of water vapor into the lattice.

[0080] Figure 4 PrBa 0.9 Cs 0.1 Co2O 6-δ High-temperature in-situ XRD image of (PBCsC) powder. It can be seen from the figure that no impurity phase is generated in the continuous heating test of PBCsC powder from 100 to 700°C (the holding time at each temperature is 1h), indicating that PBCsC oxide exhibits good phase structure stability and chemical stability at high temperatures. In the high-temperature in-situ XRD test of PBCsC oxide, as the test temperature increases, the main peak of PBCsC moves to a lower angle, which can be attributed to the lattice expansion caused by the increase in temperature.

[0081] 2. X-ray Photoelectron Spectroscopy (XPS) Characterization

[0082] According to the fitting data, after Cs partially replaces the Ba element in the A position of PBC, in order to maintain its own electrical neutrality, Pr( Figure 5 (a)) and Co( Figure 5 (b)) has further increased its high valence ratio. Figure 5 As shown in (a), Pr in PBC 4+ The content of Pr in PBCsC is 37.9%. 4+ The content of Co increased to 41.1%. The Co element also showed a similar trend, such as Figure 5 (b) As shown. In PBC, Co 3+ and Co 4+ The contents of Pr and Co in PBCsC were 36.7% and 35.0%, respectively, while in PBCsC, these contents increased to 41.8% and 43.5%, respectively. XPS results show that the incorporation of Cs in PBC leads to an increase in the content of high-valent cations of Pr and Co.

[0083] The corresponding O1s XPS fitting data of PBC and PBCsC are as follows: Figure 6 (a, b). The O1s of PBC and PBCsC can be divided into four subordinate peaks. The subordinate peaks at 528.3, 530.0, 531.4 and 533.4 eV are respectively related to the lattice oxygen (O lat ), high oxidizing oxygen (O - / O2 2- ), adsorbed oxygen (O ads ) and oxygen in the hydroxyl environment (OH - ) is related. Among them, O - / O2 2 and O lat The ratio of PBC to PBCsC reflects the content of oxygen vacancies, and the ratios of PBC to PBCsC are 1.49 and 2.03, respectively. - / O2 2- The proportion of is generally considered to play a key role in the ORR process.

[0084] 3. Relaxation characterization

[0085] Figure 7 The surface exchange coefficient k of PBCsC and PBC at the test temperature of 550-650℃ * chem and the bulk diffusion coefficient D * chem Among them, the surface exchange coefficient of PBCsC at the test temperature of 650℃ was calculated to be 7.98×10 -4 cm s-1 The surface exchange coefficient of PBC tested under the same conditions is higher than that of PBC (2.31×10 -4 cm s -1 ). * chem The increase in the value indicates that the PBCsC air electrode has faster oxygen surface exchange kinetics, thereby accelerating the ORR reaction process. * chem The results also showed a similar trend. Under the test conditions of 650℃, the D * chem The values ​​are 2.64×10 -5 and 9.01×10 -5 cm 2 s -1 . D of PBCS * chem The larger the value, the better the oxygen diffusion kinetics. In summary, the enhanced electrocatalytic activity of PBCsC air electrode may be due to the doping of A-site dopant (Cs), which produces more oxygen vacancies and improves the surface exchange kinetics.

[0086] 4. Electrochemical impedance and stability study

[0087] For the first time, the electrocatalytic activity of PBCsC air electrodes was studied by measuring the area specific resistance of symmetrical cells supported by BZCYYb1711 in humid air (3% H2O) at 700-500℃. Figure 8 As shown in (a), at 700, 650, 600, 550 and 500 °C, the surface resistivity of the PBCsC air electrode reaches 0.067, 0.184, 0.276, 0.575 and 1.588 Ωcm, respectively. 2 . Figure 8 (b) shows the electrocatalytic activity of the PBC air electrode. Under the same test conditions, the surface resistivity of the PBC air electrode reached 0.113, 0.258, 0.372, 0.977 and 2.443 Ωcm at 700, 650, 600, 550 and 500 °C, respectively. 2 Compared with the PBC air electrode, the PBCsC air electrode has higher electrocatalytic activity.

[0088] Fig. 9The stability of PBCsC and PBC in humid air (3% H2O). When exposed to humid air, the surface specific resistance value of the PBC air electrode increased significantly with the extension of the test time. On the contrary, under the same test conditions, the surface specific resistance value of the PBCsC air electrode showed better stability. Based on the above analysis, the symmetrical cell with the PBCsC air electrode has good stability and high electrocatalytic activity.

[0089] 7. Fourier transform infrared spectroscopy (FTIR) characterization

[0090] Fig.10 The Fourier transform infrared spectra of PBCsC and PBC air electrodes treated in humid air containing 30% water vapor at 600°C for 50 h are shown. FTIR measurement can identify the hydroxyl signal value in the oxide, and its characteristic peak appears at 3400-3800 cm -1 The test results show that the hydroxyl peak intensity of 30% water vapor treated PBCsC is slightly higher than that of PBC oxide, indicating that PBCsC exhibits better hydration behavior.

[0091] 8. Electrochemical performance test

[0092] The battery prepared in Example 2 was used to perform an electrochemical power density test in a fuel cell mode (FC mode) and a current density test in an electrolysis mode (EC mode). Fig.11 The full cell composed of the PBCsC air electrode of the present invention was tested in the fuel cell mode, with humidified hydrogen introduced into the anode side and air as the atmosphere on the air electrode side. The power density tested in the range of 650-500℃ was 1.66W cm -2 ,1.19W cm -2 ,0.72W cm -2 , and 0.41 W cm -2 .

[0093] Fig.12 The present invention relates to a single cell (Ni-BZCYYb1711||BZCYYb1711||PBCsC) prepared with PBCsC as the air electrode and Ni-BZCYYb1711 as the fuel electrode support, and the IV curve of the test in the EC mode (humidified hydrogen is introduced into the anode side and humidified air is introduced into the oxygen electrode side) in the range of 650-500°C. Among them, the electrolytic cell of the PBCsC air electrode also shows more excellent electrolytic performance, and the current density under the voltage condition of 1.3V at 650, 600, 550 and 500°C is -2.85Acm -2 , -1.48A cm -2 , -0.71A cm -2, and -0.31A cm -2 .

[0094] 9. Single cell stability and cycle test

[0095] Fig.13 The current density of the PBCsC air electrode at 650 °C is 0.5 A cm -2 The long-term stability of the cell running in FC mode for 170 h was demonstrated. In addition, due to the presence of humid air in the R-PCEC air electrode chamber, the air electrode's tolerance to steam is critical to the stability of the cell. The full cell with PBCsC air electrode showed good stability in the electrolysis mode using humid air (3% H2O) as the oxidant, at -0.5A cm -2 and 650℃ for 200h. -2 At 600℃, a cyclic test of FC and EC dual mode switching was carried out every 2h. Fig.14 ). The battery with PBCsC air electrode showed good stability during 80 h of reversible operation.

[0096] 10. Faradaic efficiency and hydrogen production rate test

[0097] The Faradaic efficiency is crucial for hydrogen production in the R-PCEC electrochemical process and is defined as the ratio of the actual H2 production rate (detected by gas chromatography equipment) to the theoretical H2 production rate (calculated by the applied current). Fig.15 and Fig.16 The Faradaic efficiency and hydrogen production rate at different current densities and 600 °C humid air (steam concentration is 30%) are shown. -2 When different current densities are applied, the Faradaic efficiency decreases from 85.37% to 60.86% and 48.88% as Fig.15 In addition, at -0.5, -0.75 and -1.0 A cm -2 At the current density, the corresponding H2 generation rate increased from 2.98 to 3.18 and 3.41. Fig.16 shown.

[0098] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. Application of double perovskite materials as air electrodes in reversible proton ceramic electrochemical cells, characterized in that: The expression of the double perovskite material is: PrBa 0.9 Cs 0.1 Co2O 6-δ ; Where δ is the oxygen vacancy content.

2. The use according to claim 1, characterized in that: The double perovskite material has a tetragonal layered perovskite structure.

3. The use according to claim 2, characterized in that: The lattice parameter a is b is c is 4. The use according to claim 1, characterized in that: The preparation method of the double perovskite material comprises the following steps: 1) dissolving praseodymium nitrate, barium nitrate, cesium nitrate and cobalt nitrate in water to obtain a mixed solution; then mixing the mixed solution, ethylenediaminetetraacetic acid, citric acid and ammonia water, and adjusting the pH to 7-8 to obtain a mixed solution; 2) heating the mixed solution to a gel state, performing high temperature treatment at 200-250° C. to obtain a precursor, and calcining the precursor.

5. The use according to claim 4, characterized in that: In step 1), the molar ratio of the metal element, ethylenediaminetetraacetic acid and citric acid is 0.5-1.5:0.5-1.5:1-2; wherein the metal element is the sum of Pr, Ba, Cs and Co.

6. The use according to claim 4 or 5, characterized in that: In step 2), the temperature of heating the mixed solution is 80-100° C.; and / or, the time of the high temperature treatment is 2-6 hours; and / or, the temperature of the calcination is 950-1050° C.; and the time of the calcination is 2-4 hours.

7. A reversible proton ceramic electrochemical cell, characterized in that: The reversible proton ceramic electrochemical cell comprises an anode support layer, an electrolyte and an air electrode connected in sequence; the air electrode is prepared from the double perovskite material in the application according to any one of claims 1 to 3.

8. The reversible proton ceramic electrochemical cell according to claim 7, characterized in that: The electrolyte material includes BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ , wherein δ is the oxygen vacancy content; and / or, The material of the anode support layer comprises NiO and BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ Among them, NiO and BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ The mass ratio of is 5.5-6.5:3.5-4.5; and / or, The reversible protonic ceramic electrochemical cell further includes a transition layer disposed between the anode support layer and the electrolyte.

9. The reversible proton ceramic electrochemical cell according to claim 8, characterized in that: The transition layer comprises NiO and BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ Among them, NiO and BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-δ The mass ratio is 5.5~6.5:3.5~4.5.

Citation Information

Cited By

  • A / B-site co-doped proton ceramic reversible battery perovskite air electrode material and preparation method thereof