A high-performance, low-cost bio-based liquid natural rubber and its preparation method

By combining a mixer and a twin-screw extruder, the problems of complex processes and high costs in the preparation of liquid natural rubber have been solved, enabling the preparation of high-performance, low-cost bio-based liquid natural rubber and improving production efficiency and product quality.

CN117341178BActive Publication Date: 2024-11-12宿迁绿金人橡塑机械有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202311335238.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-16
Publication Date
2024-11-12
Estimated Expiration
2043-10-16

AI Technical Summary

Technical Problem

Existing methods for preparing liquid natural rubber suffer from problems such as complex processes, high costs, low production efficiency, unstable product performance, and high impurity content.

Method used

By combining internal mixer plasticizing and twin-screw extruder, and controlling temperature and shear action, the molecular chains of natural rubber are broken down to prepare high-performance, low-cost bio-based liquid natural rubber.

Benefits of technology

This technology enables the efficient preparation of liquid natural rubber, reduces production costs, improves production efficiency, ensures stable product performance, and reduces impurity content.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a high-performance, low-cost bio-based liquid natural rubber and a preparation method thereof, the method comprising: adding a natural rubber material and an antioxidant into an internal mixer for plastication, transferring the plasticated natural rubber material to a first twin-screw extruder, controlling the temperature of the first screw extruder, breaking the molecular chain of the plasticated natural rubber material and transferring it to a second twin-screw extruder, and extruding the liquid natural rubber after temperature control and cooling. The present invention transports the natural rubber plasticated by the internal mixer to the first twin-screw extruder, utilizes the good heat transfer capacity of the barrel wall and the screw mandrel and the high shearing effect of the screw, realizes the breaking of the natural rubber molecular chain at low temperature, and the rubber material enters the second twin-screw extruder, and also utilizes the good heat transfer effect of the co-rotating twin-screw equipment to complete the cooling and conveying process of the natural rubber, and finally obtains a liquid natural rubber with a number average molecular weight Mn of 6000 to 25000 and a molecular weight distribution of 2 to 4.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical materials, and in particular to a high-performance, low-cost bio-based liquid natural rubber and a preparation method thereof. Background Art

[0002] Liquid natural rubber is a transparent viscous liquid with a certain fluidity at room temperature. It has a low relative molecular mass, so it is easy to process and shape. It has a wide range of uses in industrial production. It can be used as a rubber plasticizer, a resin toughening agent, an asphalt modifier, etc.

[0003] Liquid natural rubber is a medium molecular weight polymer, and its molecular weight is between small molecule monomers and solid rubber macromolecules. Therefore, there are two main preparation methods at present, namely small molecule monomer polymerization method and solid macromolecular rubber degradation method.

[0004] The small molecule monomer polymerization method is to achieve the transformation of small molecules into long-chain polymers through methods such as anionic polymerization, coordination polymerization and free radical polymerization. Liao Shuangquan et al. (CN 101942042B Method for preparing liquid natural rubber) proposed a method for preparing liquid natural rubber, by adding an appropriate amount of free radical initiator and carbonyl compound to purified latex, reacting for 20 to 26 hours under 50 to 80°C water bath conditions. The process of this method is simple and has little pollution, but it still needs to be coagulated with acetone, and the product needs to be soaked in water for 24 hours and washed, and dried in a vacuum at room temperature. The operation is cumbersome, time-consuming, and the cost of industrial production is high.

[0005] The solid macromolecular rubber degradation method is to break the main chain of the solid macromolecular rubber by various methods to obtain a medium molecular weight liquid rubber, mainly including photochemical degradation, chemical catalytic degradation, microbial degradation, etc. Liao Shuangquan et al. (CN 101921348 B Method for preparing epoxidized liquid natural rubber) added 0.5 parts by mass of periodic acid to epoxidized natural rubber latex with a dry rubber content of 20% to 50%, reacted at 30°C for 2 to 21 hours, precipitated in methanol, and vacuum dried at room temperature to prepare bright yellow epoxidized liquid natural rubber. This method requires a long preparation time, uses a large amount of chemical additives, and has a complicated process flow. There is no report on industrial production yet.

[0006] Xu Jiming et al. (CN 109822776 A Low-molecular-weight liquid rubber preparation device) proposed a low-molecular-weight liquid rubber preparation device, which first crushes the rubber into small particles, and then heats and softens it in a heating chamber through an extrusion screw, extrudes and heats it to the degradation temperature at the degradation shaft section and degrades it into low-molecular-weight liquid rubber with a molecular weight of 4,000 to 20,000 and a brown color. In the actual processing and production process, on the one hand, due to the high viscoelasticity of the original rubber, it is difficult to crush it into particles by mechanical shearing. On the other hand, the elastic modulus of rubber is high, and after simple mechanical shearing, it enters the screw extruder, which will cause great torque and load on the screw, and the processing and manufacturing of the screw is difficult. In addition, rubber itself is a poor conductor of heat and has poor heat transfer performance. Thermal degradation of rubber is only carried out through heat conduction. On the one hand, in order to achieve the state of liquid rubber, the temperature of the degradation stage is too high (greater than 350°C). In addition, the rubber is heated unevenly inside and outside. The thermal decomposition reaction of the rubber will be accompanied by many complex side reactions, thereby producing a large number of low-molecular products. The final liquid rubber has a wide molecular weight distribution range and a high impurity content, which affects its performance. Summary of the invention

[0007] The present invention provides a high-performance, low-cost bio-based liquid natural rubber and a preparation method thereof, so as to solve or at least alleviate at least one problem existing in the prior art.

[0008] The present invention provides a method for preparing high-performance and low-cost bio-based liquid natural rubber, the method comprising:

[0009] The natural rubber and the antioxidant are added into an internal mixer for plasticizing, and the plasticized natural rubber is transferred to a first twin-screw extruder. The temperature of the first screw extruder is controlled, and the molecular chain of the plasticized natural rubber is broken and then transferred to a second twin-screw extruder. Liquid natural rubber is extruded after temperature-controlled cooling.

[0010] As a preferred embodiment of the present invention, transferring the plasticized natural rubber material to the first twin-screw extruder comprises: transferring the plasticized natural rubber material to the first twin-screw extruder via a continuous feeding device.

[0011] As a preferred embodiment of the present invention, the molecular chains of the plasticized natural rubber are broken and then transferred to the second twin-screw extruder, including: the molecular chains of the plasticized natural rubber are broken and then transferred to the second twin-screw extruder via a conveying device.

[0012] As a preferred embodiment of the present invention, the rotor speed of the internal mixer is 50-100 r / min, the filling factor is 0.5-0.8, and the mixing time is 180-450 s.

[0013] In the present invention, natural rubber and antioxidant are added into an internal mixer for plasticization to obtain a plasticized natural rubber with a temperature of 60-160° C. and a Mooney viscosity of 25-60.

[0014] As a preferred embodiment of the present invention, the antioxidant includes at least one of antioxidant MB, antioxidant SP-C, antioxidant 264 and antioxidant 2246.

[0015] As a preferred embodiment of the present invention, the mass ratio of the natural rubber to the antioxidant is 100:(0.2-2).

[0016] As a preferred embodiment of the present invention, the temperature of the first screw extruder is controlled, and the molecular chains of the plasticized natural rubber material are broken and then transferred to the second twin-screw extruder, comprising:

[0017] The temperature of the first screw extruder is controlled at 180-260° C., and after 2-6 minutes, the natural rubber material with broken molecular chains is transferred to the second twin-screw extruder.

[0018] As a preferred embodiment of the present invention, the temperature of the conveying section of the first twin-screw extruder is 180-220°C, the temperature of the shearing section is 230-260°C, and the temperature of the cooling section is 180-200°C.

[0019] As a preferred embodiment of the present invention, the temperature-controlled cooling followed by extrusion to obtain liquid natural rubber comprises: controlling the temperature of the barrel and the mandrel of the second twin-screw extruder to 8-50° C., cooling for 1-5 minutes, and then extruding to obtain the liquid natural rubber.

[0020] As a preferred embodiment of the present invention, the first screw extruder is a co-rotating twin-screw extruder, wherein the aspect ratio of the screw is (40-60):1, and the screw speed is 150-300 r / min.

[0021] As a preferred embodiment of the present invention, the second screw extruder is a co-rotating or counter-rotating twin-screw extruder, wherein the aspect ratio of the screw is (36-54):1, and the screw speed is 40-100 r / min.

[0022] The present invention provides a high-performance, low-cost bio-based liquid natural rubber, which is prepared by the preparation method of the high-performance, low-cost bio-based liquid natural rubber provided by the present invention.

[0023] The temperature of the liquid natural rubber prepared by the method for preparing high-performance and low-cost bio-based liquid natural rubber in the present invention is below 50° C., the number average molecular weight Mn is 6000-25000, and the molecular weight distribution is 2-4.

[0024] Compared with the prior art, the present invention has at least the following beneficial effects:

[0025] Since natural rubber has poor heat transfer performance and high viscoelasticity, it is not conducive to direct processing. Therefore, it is first placed in an internal mixer for plastication to reduce its Mooney viscosity, which is convenient for subsequent screw extruders to eat and shear. Adding a certain amount of antioxidant in the internal mixer can prevent excessive oxygen from participating in the breakage of rubber molecular chains, and also help control the molecular weight distribution of the product. During the plastication process, the temperature of the rubber will rise, and the movement of the internal molecular chains will become active, which is conducive to thermal shearing in the subsequent twin-screw extruder. When the material enters the first twin-screw extruder, under the combined effects of temperature, additives, and shear, according to the thermal weight loss curve of natural rubber and its heat transfer characteristics, the breakage of the natural rubber molecular chain can be achieved under process conditions below 260°C. It not only avoids excessive decomposition of rubber at too high a temperature to produce a large number of low-molecular products, thereby affecting the performance of the product, but also reduces production energy consumption and costs. After entering the second screw extruder, the high-temperature material will continue to undergo a molecular chain rupture reaction under the action of weak shear, and the molecular weight and Mooney viscosity of the material will be further reduced. The cooling temperature is reasonably set and the residence time is matched to achieve material cooling and ensure smooth extrusion of the material. In the present invention, only an antioxidant is added, and the molecular chain of the natural rubber is ruptured by the internal mixing of the internal mixer, the high shearing action of the screw extruder, and the heating of the barrel, thereby achieving the transformation of the rubber from a solid state to a liquid state.

[0026] While being based on the current status of the industry, the present invention reasonably connects and connects the plasticization, molecular chain degradation and cooling of natural rubber, adds the natural rubber plasticized in the internal mixer to the twin-screw extruder for further degradation, and gives full play to the characteristics of the twin-screw extruder screw, which has flexible and changeable arrangement of the threaded elements and multiple shear meshing areas, so that the material forms multiple changes in flow direction and flow rate, and can form an efficient shearing effect on the material. Based on the analysis and calculation of finite elements, the calculation of the dynamic friction coefficient between the material and the screw, etc., through the reasonable configuration and design of the power, torque, wear, etc. of the twin-screw extruder, the continuous industrial preparation of liquid natural rubber is realized. Compared with the previous preparation method, the production efficiency is greatly improved, the preparation cost is significantly reduced, and the impurities of the product are reduced and the performance is stable. DETAILED DESCRIPTION

[0027] Exemplary embodiments of the present invention will be described in more detail below. The present invention provides exemplary embodiments, but it should be appreciated that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to be able to more thoroughly understand the present invention, and the scope of the present invention can be fully communicated to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0028] Example 1

[0029] 100 parts of natural rubber and 0.2 parts of antioxidant MB were added to the internal mixer for internal mixing. The rotor speed was 50r / min, the filling factor was 0.5, and the mixing time was 180s. The material with a temperature of 60°C and a Mooney viscosity value of 25 was obtained. Then it entered the first twin-screw extruder through a continuous feeding device. The aspect ratio of the screw was 60:1, the screw speed was 150r / min, the temperature of the conveying section of the screw extruder was controlled at 180°C, the temperature of the shearing section was 260°C, and the temperature of the cooling section was 200°C. The molecular chain was broken within 2min, and it entered the second twin-screw extruder through the conveying device. The aspect ratio of the screw was 36:1, the screw speed was 40r / min, and the temperature of the barrel and the mandrel of the screw extruder was controlled at 8°C. After cooling for 1min, the liquid natural rubber with a temperature below 50°C, a number average molecular weight Mn of 6716, and a molecular weight distribution of 2.5 was obtained by extrusion.

[0030] Example 2

[0031] 100 parts of natural rubber and 0.6 parts of antioxidant 264 were added to the internal mixer for internal mixing. The rotor speed was 60r / min, the filling factor was 0.6, and the mixing time was 200s. The material with a temperature of 65°C and a Mooney viscosity value of 55 was obtained. Then it entered the first twin-screw extruder through a continuous feeding device. The aspect ratio of the screw was 48:1, the screw speed was 210r / min, the temperature of the conveying section of the screw extruder was controlled at 205°C, the temperature of the shearing section was 230°C, and the temperature of the cooling section was 180°C. The molecular chain was broken within 4 minutes. It entered the second twin-screw extruder through the conveying device. The aspect ratio of the screw was 42:1, the screw speed was 55r / min, and the temperature of the barrel and the mandrel of the screw extruder was controlled at 20°C. After cooling for 3 minutes, the liquid natural rubber with a temperature below 50°C, a number average molecular weight Mn of 9716, and a molecular weight distribution of 3.5 was obtained by extrusion.

[0032] Example 3

[0033] 100 parts of natural rubber and 1.2 parts of antioxidant 2246 were added to the internal mixer for internal mixing. The rotor speed was 70r / min, the filling factor was 0.65, and the mixing time was 280s. The material with a temperature of 80°C and a Mooney viscosity value of 47 was obtained. Then it entered the first twin-screw extruder through a continuous feeding device. The aspect ratio of the screw was 55:1, the screw speed was 250r / min, the temperature of the conveying section of the screw extruder was controlled at 195°C, the temperature of the shearing section was 255°C, and the temperature of the cooling section was 185°C. The molecular chain was broken within 6 minutes. It entered the second twin-screw extruder through the conveying device. The aspect ratio of the screw was 54:1, the screw speed was 75r / min, and the temperature of the barrel and the mandrel of the screw extruder was controlled at 38°C. After cooling for 4 minutes, the liquid natural rubber with a temperature below 50°C, a number average molecular weight Mn of 17635, and a molecular weight distribution of 3.9 was obtained by extrusion.

[0034] Example 4

[0035] 100 parts of natural rubber and 1.5 parts of antioxidant MB were added to the internal mixer for internal mixing. The rotor speed was 85r / min, the filling factor was 0.7, and the mixing time was 320s. The material with a temperature of 90°C and a Mooney viscosity value of 36 was obtained. Then it entered the first twin-screw extruder through a continuous feeding device. The aspect ratio of the screw was 40:1, the screw speed was 300r / min, the temperature of the conveying section of the screw extruder was controlled at 220°C, the temperature of the shearing section was 260°C, and the temperature of the cooling section was 200°C. The molecular chain was broken within 3min, and it entered the second twin-screw extruder through the conveying device. The aspect ratio of the screw was 50:1, the screw speed was 100r / min, and the temperature of the barrel and the mandrel of the screw extruder was controlled at 15°C. After cooling for 2min, the liquid natural rubber with a temperature below 50°C, a number average molecular weight Mn of 13325, and a molecular weight distribution of 3.2 was obtained by extrusion.

[0036] Example 5

[0037] 100 parts of natural rubber and 2 parts of antioxidant SP-C were added to the internal mixer for internal mixing. The rotor speed was 95r / min, the filling factor was 0.8, and the mixing time was 450s. The material with a temperature of 160°C and a Mooney viscosity value of 55 was obtained. Then it entered the first twin-screw extruder through a continuous feeding device. The aspect ratio of the screw was 58:1, the screw speed was 220r / min, the temperature of the conveying section of the screw extruder was controlled at 205°C, the temperature of the shearing section was 245°C, and the temperature of the cooling section was 195°C. The molecular chain was broken within 5min, and it entered the second twin-screw extruder through the conveying device. The aspect ratio of the screw was 44:1, the screw speed was 88r / min, and the temperature of the barrel and the mandrel of the screw extruder was controlled at 45°C. After cooling for 5min, the liquid natural rubber with a temperature below 50°C, a number average molecular weight Mn of 24325, and a molecular weight distribution of 3 was obtained.

[0038] The present invention transports the natural rubber after plastication in the internal mixer to the first twin-screw extruder, utilizes the good heat transfer capacity of the barrel wall and the screw mandrel and the high shearing effect of the screw to achieve the breaking of the natural rubber molecular chain at low temperature, and the rubber enters the second twin-screw extruder, and also utilizes the good heat transfer effect of the co-rotating twin-screw equipment to complete the cooling and transportation process of the natural rubber, and finally obtains liquid natural rubber with a number average molecular weight Mn of 6000 to 25000 and a molecular weight distribution of 2 to 4. Compared with the traditional method for preparing liquid natural rubber, the method uses bio-based natural rubber as raw material, does not rely on petrochemical resources, has the advantages of low preparation cost, low carbon production process, simple equipment, etc., and the product produced has few impurities and stable performance.

[0039] It should be understood that in order to streamline the present invention and aid in understanding one or more of the various inventive aspects, in the above description of exemplary embodiments of the present invention, various features of the present invention are sometimes grouped together into a single embodiment or description thereof. However, this method of invention should not be interpreted as reflecting the intention that the claimed invention requires more features than those expressly recited in each claim. Rather, as reflected in the claims below, inventive aspects lie in less than all of the features of a single embodiment of the preceding invention. Therefore, the claims that follow the detailed description are hereby expressly incorporated into the detailed description, with each claim itself serving as a separate embodiment of the present invention.

[0040] In addition, those skilled in the art will appreciate that, although some embodiments described herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present invention and form different embodiments. For example, in the claims, any one of the claimed embodiments may be used in any combination.

[0041] The above description is only an illustrative embodiment of the present invention and is not intended to limit the present invention in any form or substance. It should be pointed out that, for ordinary technicians in this technical field, a number of improvements and supplements made without departing from the method of the present invention should also be regarded as the protection scope of the present invention; any equivalent changes, modifications and evolutions made by technicians familiar with this profession using the technical content disclosed above without departing from the spirit and scope of the present invention are all equivalent embodiments of the present invention; at the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention still fall within the protection scope of the present invention.

Claims

1. A method for preparing high-performance and low-cost bio-based liquid natural rubber, characterized in that: The method includes: Adding natural rubber and antioxidant into an internal mixer for plasticizing, transferring the plasticized natural rubber to a first twin-screw extruder, controlling the temperature of the first screw extruder, breaking the molecular chain of the plasticized natural rubber, and transferring it to a second twin-screw extruder, cooling it under temperature control, and extruding it to obtain liquid natural rubber; The rotor speed of the internal mixer is 50-100 r / min, the filling factor is 0.5-0.8, and the mixing time is 180-450 s; The antioxidant includes at least one of antioxidant MB, antioxidant SP-C, antioxidant 264 and antioxidant 2246; The mass ratio of the natural rubber to the antioxidant is 100:(0.2-2); The temperature of the first screw extruder is controlled to break the molecular chain of the plasticized natural rubber material and then transfer it to the second twin-screw extruder, including: controlling the temperature of the first screw extruder at 180-260° C., and transferring the natural rubber material with broken molecular chain to the second twin-screw extruder after 2-6 minutes; The temperature of the conveying section of the first twin-screw extruder is 180-220°C, the temperature of the shearing section is 230-260°C, and the temperature of the cooling section is 180-200°C.

2. The method for preparing high-performance and low-cost bio-based liquid natural rubber according to claim 1, characterized in that: The method of extruding the liquid natural rubber after temperature control and cooling comprises: controlling the temperature of the barrel and the core shaft of the second twin-screw extruder to be 8-50° C., cooling for 1-5 minutes and then extruding to obtain the liquid natural rubber.

3. The method for preparing high-performance and low-cost bio-based liquid natural rubber according to claim 1, characterized in that: The first screw extruder is a co-rotating twin-screw extruder, wherein the aspect ratio of the screw is (40-60):1, and the screw speed is 150-300 r / min.

4. The method for preparing high-performance and low-cost bio-based liquid natural rubber according to any one of claims 1 to 3, characterized in that: The second screw extruder is a co-rotating or counter-rotating twin-screw extruder, wherein the aspect ratio of the screw is (36-54):1, and the screw speed is 40-100 r / min.

5. A high-performance, low-cost bio-based liquid natural rubber, characterized in that: The high-performance, low-cost bio-based liquid natural rubber is prepared by the preparation method of high-performance, low-cost bio-based liquid natural rubber according to any one of claims 1 to 4.

Citation Information

Cited By

  • Preparation method and application of low-molecular-weight natural rubber

    CN121159737A