A polyvinylidene fluoride-polyvinylpyrrolidone block copolymer, its preparation method and application
By preparing polyvinylidene fluoride-polyvinylpyrrolidone block copolymer as a binder, the problem of poor dispersion of lithium battery cathode materials was solved, achieving uniform dispersion and high-strength bonding of the slurry, thus improving the performance of lithium batteries.
Patent Information
- Application Number
- CN202311141952.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-06
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-09-06
AI Technical Summary
Existing lithium battery cathode materials are difficult to disperse evenly during the slurry process, resulting in excessively high slurry viscosity or excessively low solid content, which affects coating and battery performance.
Polyvinylidene fluoride-polyvinylpyrrolidone block copolymers were used as binders to prepare polyvinylidene fluoride blocks and polyvinylpyrrolidone blocks containing polar functional groups via iodine transfer radical polymerization, thereby improving dispersibility and adhesion properties.
It significantly improves the dispersibility and stability of lithium battery slurry, reduces slurry viscosity, increases slurry peel strength and bonding strength, and enhances the overall performance of the battery.
Smart Images

Figure CN117362554B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer materials, specifically relating to a polyvinylidene fluoride-polyvinylpyrrolidone block copolymer, its preparation method, and its application. Background Technology
[0002] Polyvinylidene fluoride (PVDF) resin is a high-performance polymer material with excellent high and low temperature resistance, weather resistance, low flammability, and chemical stability, making it widely used in various fields. In recent years, due to the rapid development of new energy vehicles and energy storage equipment, the demand for lithium batteries has been increasing, highlighting the growing importance of PVDF resin as a binder, a key material. Currently, major fluorochemical companies focus their research on improving the adhesion of PVDF resin, often neglecting other requirements such as dispersibility.
[0003] Because lithium-ion battery cathode materials such as LiFePO4 have small particle sizes and large specific surface areas, it is difficult to uniformly disperse the cathode material, binder PVDF, and conductive agents (SP, CNT, etc.) during the slurry preparation process. This results in excessively high viscosity or excessively low solid content in the slurry, leading to coating difficulties. Furthermore, the uneven distribution of conductive agents, cathode materials, and binders significantly affects the overall performance of the battery. Currently, the most common method is to add the dispersant polyvinylpyrrolidone (PVP) to improve the slurry's dispersibility. PVP's molecular structure contains strongly polar lactam hydrophilic groups and CC long-chain lipophilic groups, making it compatible with various solvents. It can also coat the surface of microparticles, forming a good dispersion effect through steric hindrance. Adding an appropriate amount of PVP to the lithium-ion battery cathode slurry can significantly improve its dispersibility, transforming the slurry from a Newtonian fluid to a non-Newtonian fluid, stabilizing the slurry viscosity to a lower level, ultimately helping to reduce the cathode impedance and improve battery performance.
[0004] For example, CN101679563A discloses a linear semi-crystalline copolymer comprising repeating units derived from vinylidene fluoride monomers and at least one hydrophilic (meth)acrylic acid monomer. The polymer comprises 0.05-10% (molar) of repeating units derived from hydrophilic (meth)acrylic acid monomers, with the hydrophilic (meth)acrylic acid monomers containing at least 40% random distribution. By introducing hydrophilic groups (such as carboxyl groups) and controlling the polymerization conditions, the comonomers tend to be more randomly distributed during polymerization. This invention significantly improves the adhesion of PVDF resin. Researchers have found that during slurry preparation, the slurry is prone to agglomeration (or gelation), resulting in uneven dispersion and high viscosity. This is speculated to be due to hydrogen bonding between polar functional groups of polar monomers and complexation between polar groups and active materials. In addition, the active materials have very small particle sizes, which inherently present difficulties in dispersion. These factors combined lead to poor slurry dispersibility.
[0005] For example, CN113224305A discloses a method for preparing modified polyvinylidene fluoride (PVDF) for lithium-ion batteries. The method includes adding graphene oxide to N,N-dimethylformamide, ultrasonically dispersing it, then adding itaconic acid and azobisisobutyronitrile (AIBN), heating to 60-70°C under a nitrogen atmosphere, magnetically stirring for 6-10 hours, cooling, filtering, and drying to obtain modified graphene oxide. The obtained modified graphene oxide is then added to N,N-dimethylacetamide, ultrasonically dispersed for 5-8 hours, followed by the addition of tin dichloride, raising the temperature to 60-70°C, stirring for 2-3 hours, adding PVDF and polyvinylpyrrolidone (PVDF), continuing magnetic stirring at this temperature for 10-16 hours, cooling, vacuum drying, and then grinding in a ball mill for 2-3 hours to obtain the binder. This invention first uses itaconic acid to modify graphene oxide, then uses the modified graphene oxide and tin dichloride to modify PVDF, and then simultaneously adds polyvinylpyrrolidone to increase adhesion. This invention actually obtains a composite adhesive by chemically modifying and solution blending PVDF. The addition of polyvinylpyrrolidone (PVDF) increases its adhesiveness through physical blending (solution blending). The invention does not mention any improvement in the dispersibility of the composite adhesive due to the addition of PVDF (possibly due to an inappropriate choice of PVDF molecular weight). Furthermore, since PVDF exists in an independent form in the adhesive, it may have issues with electrolyte resistance.
[0006] For example, CN111029585A discloses a method for preparing a highly dispersible composite binder for lithium-ion battery cathodes. It involves mixing polyvinylpyrrolidone-grafted modified conductive carbon material with polyvinylidene fluoride (PVDF) to obtain the highly dispersible composite binder. This patent, which grafts conductive carbon black with polyvinylpyrrolidone and then mixes it with PVDF to form a composite binder, still relies on a physical blending method, resulting in a complex composition. Furthermore, the applicability of this PVP-modified carbon black to different slurry systems is questionable. In addition, the preparation process of PVP-modified carbon black is overly complex and lacks operability, primarily addressing the dispersibility of conductive carbon black without significantly improving the adhesion and dispersibility of PVDF. Summary of the Invention
[0007] The purpose of this invention is to provide a polyvinylidene fluoride-polyvinylpyrrolidone block copolymer, its preparation method and application. The copolymer contains polar functional groups and polyvinylpyrrolidone blocks, and has excellent bonding properties while also having excellent dispersing properties for battery slurries, making it very suitable as a lithium battery binder.
[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows: a polyvinylidene fluoride-polyvinylpyrrolidone block copolymer, wherein the copolymer is a diblock copolymer of polyvinylidene fluoride blocks and polyvinylpyrrolidone blocks, wherein the polyvinylidene fluoride blocks are modified blocks containing polar monomers; and the content of the polyvinylpyrrolidone blocks in the copolymer is 3.3-16.7 wt%.
[0009] In a preferred embodiment of the present invention, the polar monomer content is 0.2-2 mol% of the polyvinylidene fluoride block.
[0010] In a preferred embodiment of the present invention, the weight-average molecular weight of the polyvinylidene fluoride block is 500,000 to 2,000,000.
[0011] The present invention also provides a method for preparing the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer, comprising the following steps:
[0012] (1) Add deionized water, 5-15wt% polar monomer, dispersant and chain transfer agent to the reactor. After deoxygenating the polymerization reactor with nitrogen vacuum, heat it to 40-60℃. Introduce vinylidene fluoride monomer to the reactor until the pressure is 8.0-14.0MPa. Add initiator to carry out polymerization reaction. During the polymerization process, maintain the polymerization pressure by adding vinylidene fluoride monomer. At the same time, continuously add the remaining polar monomer. When the mass ratio of the added amount of vinylidene fluoride monomer to the chain transfer agent is 200-450:1, stop adding. Cool down to recover the unreacted VDF monomer and discharge the material. After coagulation, washing and drying, obtain iodine-terminated polyvinylidene fluoride resin.
[0013] (2) The iodine-terminated polyvinylidene fluoride resin, N-vinylpyrrolidone (NVP) monomer and initiator prepared in step (1) are polymerized in an organic solvent. The polymerization reaction is carried out at a temperature of 50-90℃ and for a time of 10-20h. After the reaction is completed, the reaction solution is precipitated, washed and dried to obtain the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer product.
[0014] As a preferred embodiment of the present invention, the mass ratio of deionized water, polar monomer, dispersant, initiator and chain transfer agent in step (1) is 1000-1500: 5-10: 0.2-0.4: 0.3-0.6: 1.
[0015] In a preferred embodiment of the present invention, the initiator in step (1) is one of diisopropyl peroxydicarbonate and tert-butyl peroxypentanoate; the dispersant is methylcellulose; and the chain transfer agent is perfluoroiodoethane.
[0016] As a preferred embodiment of the present invention, the polar monomer mentioned in step (1) is at least one of acryloyloxyethyl succinate, monomethyl maleate, and methacrylic acid.
[0017] In a preferred embodiment of the present invention, the initiator in step (2) is azobisisobutyronitrile (AIBN); and the organic solvent is N,N-dimethylformamide.
[0018] In a preferred embodiment of the present invention, the drying temperature in step (2) is 80-120°C and the drying time is 20-30h.
[0019] The present invention also provides the application of the aforementioned polyvinylidene fluoride-polyvinylpyrrolidone block copolymer as a battery binder.
[0020] The polyvinylidene fluoride-polyvinylpyrrolidone block copolymer of the present invention contains polar-modified polyvinylidene fluoride blocks and polyvinylpyrrolidone blocks, and is prepared by iodine transfer polymerization. The polar-modified polyvinylidene fluoride blocks in this block copolymer impart excellent bonding properties, while the polyvinylpyrrolidone blocks impart excellent dispersibility. It is highly suitable as a battery binder material, and when used as a battery binder, it can significantly improve the dispersibility of the slurry, effectively reduce the slurry viscosity, and enhance the slurry stability.
[0021] In the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer of the present invention, the polyvinylidene fluoride block is a modified block containing a polar monomer. The polar monomer of the polyvinylidene fluoride block can be a monomer containing polar groups such as carboxyl, amino, hydroxyl, ester, and nitrile groups. Preferably, the polar monomer is a carboxyl-containing polar monomer, such as acrylic acid, methacrylic acid, monomethyl maleate, itaconic acid, 2-carboxyethyl acrylate, 2-carboxyethyl methacrylate, acryloyloxyethyl succinate, methacryloyloxyethyl succinate, ethyl acryloyloxyphthalate, ethyl methacryloyloxyphthalate, trifluoroacrylic acid, trifluoromethylacrylic acid, etc. It should be further noted that, as a carboxyl-containing monomer, one can be used alone or a mixture of two or more monomers during the polymerization reaction. More preferably, the polar monomer is at least one selected from acryloyloxyethyl succinate, monomethyl maleate, and methacrylic acid. The preferred content of the polar monomer is 0.2-2 mol of polyvinylidene fluoride block, more preferably 0.5-1.8 mol, and most preferably 1-1.5 mol.
[0022] In the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer of the present invention, the weight-average molecular weight of the polyvinylidene fluoride block is preferably 500,000 to 2,000,000, more preferably 600,000 to 1,500,000, and most preferably 800,000 to 1,200,000. The content of the polyvinylpyrrolidone block in the polymer is preferably 3.3 to 16.7 wt%, more preferably 4.8 to 14.3%, and most preferably 6.2 to 11.7%.
[0023] The polyvinylidene fluoride block of the present invention may also include at least one conventional monomer that can copolymerize with vinylidene fluoride, such as vinyl fluoride, trifluoroethylene, hexafluoropropylene, trifluorochloroethylene, tetrafluoroethylene, perfluoroalkyl vinyl ether, etc. Preferably, the proportion of vinylidene fluoride in the polyvinylidene fluoride block is at least 90%, so as not to affect its chemical properties.
[0024] The preparation method of the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer of the present invention is iodine transfer radical polymerization. Specifically, the method involves first preparing an iodine-terminated polyvinylidene fluoride macromolecular chain transfer agent by free radical polymerization, and then introducing polyvinylpyrrolidone segments through iodine transfer polymerization.
[0025] In this invention, the preparation method of the iodine-terminated polyvinylidene fluoride macromolecular chain transfer agent preferably uses a polymerization temperature of 40-60℃, more preferably 43-57℃, and most preferably 46-54℃; a polymerization pressure preferably of 8.0-14.0 MPa, more preferably 9.0-13.0 MPa, and most preferably 10.0-12.0 MPa; the initiator can be an organic peroxide, such as diisopropyl peroxide (IPP) and diisopropyl peroxide... The chain transfer agent can be one of the following: n-propyl ester, dibutyl peroxydicarbonate, diethyl peroxydicarbonate, tert-butyl peroxypentanoate (TBPV), tert-amyl peroxypentanoate, etc.; the initiator is preferably one of diisopropyl peroxydicarbonate or tert-butyl peroxypentanoate; the chain transfer agent can be a perfluoroalkyl iodide, such as perfluorobutyl iodide, perfluorohexyl iodide, perfluorooctyl iodide, perfluorodecyl iodide, perfluoroalkyl iodide, perfluorobutyl ethyl iodide, perfluorohexyl ethyl iodide, perfluorooctyl ethyl iodide, perfluoroalkyl ethyl iodide, etc.; perfluoroiodoethane is preferred as the chain transfer agent.
[0026] In this invention, during the process of introducing iodine into the polyvinylpyrrolidone block, the preferred reaction temperature is 50-90°C, a more preferred reaction temperature is 60-85°C, and the most preferred reaction temperature is 65-80°C. The organic solvent is primarily a good solvent for PVDF resin, and examples include acetone, N,N-dimethylformamide (DMF), N,N-dimethylhexamethylene amide (DMAc), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO), with DMF being the most preferred.
[0027] In this invention, after the iodine transfer reaction to introduce polyvinylidene fluoride (PVDF) into the polyvinylidene fluoride block copolymer is completed, the reaction solution is precipitated, washed, and dried to obtain the PVDF-PVDF block copolymer product. For example, a crude PVDF-PVDF block copolymer can be obtained by precipitation with deionized water, followed by washing with deionized water to remove residual initiator, unreacted N-vinylpyrrolidone monomer, and the generated homopolymer PVDF copolymer. Finally, the product is dried to obtain the final product.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. The polyvinylidene fluoride-polyvinylpyrrolidone block copolymer of the present invention contains polar groups, which can improve the bonding strength between the copolymer and the metal electrode. In addition, the block polyvinylpyrrolidone is a hydrophilic group, which also improves the bonding between the copolymer and the metal electrode to a certain extent. The slurry prepared using the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer of the present invention has a rebound ratio of less than 120.1%.
[0030] 2. The polyvinylidene fluoride-polyvinylpyrrolidone block copolymer of the present invention contains polyvinylpyrrolidone blocks, which can significantly improve the dispersibility of battery slurry. At the same time, with the help of the excellent dispersibility of polyvinylpyrrolidone blocks, polyvinylidene fluoride blocks can also be uniformly dispersed in battery slurry, thus playing a better binding role. The slurry prepared using the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer of the present invention has a peel strength of 28.5 N / m or more at 180°. Attached Figure Description
[0031] Figure 1 The 1H NMR spectrum of the PVDF block in Example 1;
[0032] Figure 2 The PVDF block NMR fluorine spectrum in Example 1;
[0033] Figure 3 The 1H NMR spectrum of the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer in Example 1;
[0034] Figure 4 The NMR fluorine spectrum of the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer in Example 1 is shown. Detailed Implementation
[0035] The present invention will be further illustrated below with reference to specific embodiments, but these embodiments are only used to explain the present invention and are not intended to limit the scope of the present invention.
[0036] Example 1
[0037] Preparation of polar monomer-modified PVDF blocks: 3000g of deionized water, 0.8g of methylcellulose, 3.0g of perfluoroiodoethane, and 3.0g of acryloyloxyethyl succinate were added to a 5L vertical reactor equipped with a tilting paddle. After deoxygenation under alternating nitrogen vacuum, the reactor temperature was raised to 46℃, and VDF monomer was added to a pressure of 10.0MPa. 1.0g of IPP initiator was added to the polymerization reactor to initiate the reaction. During the reaction, the polymerization pressure was maintained by continuously adding VDF monomer, while simultaneously adding 200g of an aqueous solution containing 27g of acryloyloxyethyl succinate at the same rate. Addition of VDF monomer was stopped when the added amount reached 800g. After cooling and recovery of the VDF monomer, the product was discharged. After coagulation, washing, and drying, 840g of PVDF resin was obtained. The test results of the PVDF resin are shown in Table 1.
[0038] Preparation of polyvinylidene fluoride-polyvinylpyrrolidone block copolymer: 50g of the above-mentioned PVDF resin was added to a 2L reactor containing 1200ml of DMF, 10g of N-vinylpyrrolidone monomer was added, and then 0.2g of AIBN initiator was added to the reactor. Under nitrogen protection, the polymerization reaction was carried out at 65℃ for 20h. The reaction was stopped by cooling, and the solution in the reactor was collected. After precipitation with deionized water, crude polyvinylidene fluoride-polyvinylpyrrolidone block copolymer was obtained. It was then washed with deionized water at 100℃ and dried at 100℃ for 24h to obtain the final product. The product test results are shown in Table 1, and the battery slurry performance test results are shown in Table 2.
[0039] Example 2
[0040] Preparation of polar monomer-modified PVDF blocks: 3000g of deionized water, 0.8g of methylcellulose, 2.5g of perfluoroiodoethane, and 2.2g of monomethyl maleate were added to a 5L vertical reactor equipped with a tilting paddle. After deoxygenation under alternating nitrogen vacuum, the reactor temperature was raised to 50℃, and VDF monomer was added to a pressure of 11.0MPa. 1.5g of TBPV initiator was added to the polymerization reactor to initiate the reaction. During the reaction, the polymerization pressure was maintained by continuously adding VDF monomer, while simultaneously adding 200g of an aqueous solution containing 19.8g of methacrylic acid at the same rate. Addition was stopped when the VDF monomer addition reached 800g. After cooling and recovery of the VDF monomer, the product was discharged. After coagulation, washing, and drying, 830g of PVDF resin was obtained. The test results of the PVDF resin are shown in Table 1.
[0041] Preparation of polyvinylidene fluoride-polyvinylpyrrolidone block copolymer: 50g of the above-mentioned PVDF resin was added to a 2L reactor containing 1200ml of DMF, along with 7g of N-vinylpyrrolidone monomer and 0.15g of AIBN initiator. Under nitrogen protection, the polymerization reaction was carried out at 72℃ for 16h. The reaction was stopped by cooling, and the solution in the reactor was collected. Crude polyvinylidene fluoride-polyvinylpyrrolidone block copolymer was obtained by precipitation with deionized water. The copolymer was then washed with deionized water at 90℃ and dried at 110℃ for 20h to obtain the final product. The test results are shown in Table 1, and the battery slurry performance test results are shown in Table 2.
[0042] Example 3
[0043] Preparation of polar monomer-modified PVDF blocks: 3000g of deionized water, 0.8g of methylcellulose, 2.0g of perfluoroiodoethane, and 2.0g of methacrylic acid were added to a 5L vertical reactor equipped with a tilting paddle. After deoxygenation under alternating nitrogen vacuum, the reactor temperature was raised to 54℃, and VDF monomer was added to a pressure of 12.0MPa. 0.6g of IPP initiator was added to the polymerization reactor to initiate the reaction. During the reaction, the polymerization pressure was maintained by continuously adding VDF monomer, while simultaneously adding 200g of an aqueous solution containing 19g of methacrylic acid at the same rate. Addition of VDF monomer was stopped when the added amount reached 800g. After cooling and recovery of the VDF monomer, the product was discharged. After coagulation, washing, and drying, 825g of PVDF resin was obtained. The test results of the PVDF resin are shown in Table 1.
[0044] Preparation of polyvinylidene fluoride-polyvinylpyrrolidone block copolymer: 50g of the above-mentioned PVDF resin was added to a 2L reactor containing 1200ml of DMF, along with 5g of N-vinylpyrrolidone monomer and 0.1g of AIBN initiator. Under nitrogen protection, the polymerization reaction was carried out at 80℃ for 10h. The reaction was stopped by cooling, and the solution in the reactor was collected. Crude polyvinylidene fluoride-polyvinylpyrrolidone block copolymer was obtained by precipitation with deionized water. The copolymer was then washed with deionized water at 70℃ and dried at 90℃ for 28h to obtain the final product. Product test results are shown in Table 1, and battery slurry performance tests are shown in Table 2.
[0045] Comparative Example 1
[0046] The adhesive was prepared using the method described in patent CN101679563A:
[0047] 3100g of deionized water, 1.0g of suspending agent, 1.3g of acrylic acid, and 1320g of vinylidene fluoride monomer were added to a 5L vertical polymerization reactor equipped with a propeller. Then, 3.75g of tert-amyl peroxypentanoate was added. The polymerization reactor was gradually heated to 52℃, which corresponds to a pressure of 12MPa. During the entire reaction process, 875ml of an aqueous solution containing 23g of acrylic acid was added. The reaction was stopped after 540 minutes. The resulting suspension was filtered, washed, and dried to obtain 1020g of vinylidene fluoride resin. The resin test results are shown in Table 1, and the battery slurry performance test results are shown in Table 2.
[0048] Comparative Example 2
[0049] A compound binder was prepared by blending Solef 5130 (a commercially available binder) and PVP (K30) in a 10:1 ratio. The battery slurry performance tests are shown in Table 2.
[0050] Comparative Example 3
[0051] The adhesive was prepared using the method described in patent CN113224305A:
[0052] (1) Graphene oxide was added to N,N-dimethylformamide and ultrasonically dispersed. Then itaconic acid and azobisisobutyronitrile were added. The mixture was heated to 60°C under a nitrogen atmosphere and magnetically stirred for 6 hours. After cooling, it was filtered and dried to obtain modified graphene oxide. The mass ratio of graphene oxide, itaconic acid and azobisisobutyronitrile was 1:0.46:0.24.
[0053] (2) The modified graphene oxide obtained in step (1) was added to N,N-dimethylacetamide, and then sonicated for 5 hours. Then, tin dichloride was added, and the temperature was raised to 60°C and stirred for 2 hours. Polyvinylidene fluoride (Mw = 1 million) and polyvinylpyrrolidone were added, and the mixture was magnetically stirred at this temperature for 10 hours. After cooling and vacuum drying, the mixture was placed in a ball mill and ground for 2 hours to obtain the binder. The mass-to-volume ratio of modified graphene oxide, N,N-dimethylacetamide, and tin dichloride was 0.69 g:30 mL:0.22 g, and the mass ratio of polyvinylidene fluoride to polyvinylpyrrolidone was 8:1.2. The battery slurry performance test results are shown in Table 2.
[0054] Comparative Example 4
[0055] The adhesive was prepared using the method described in patent CN111029585A.
[0056] The preparation of polyvinylpyrrolidone-grafted modified conductive carbon materials includes the following steps:
[0057] (1) Weigh 10g of multi-walled carbon nanotubes and disperse them in 200g of mixed acid (a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1) for 1 hour by ultrasonic dispersion. Then add them to a three-necked flask and cool and reflux them in a constant temperature cold bath at 70℃ for 8 hours to obtain carboxylated carbon nanotubes. Then wash the carboxylated carbon nanotubes until neutral.
[0058] (2) After drying the product obtained in step (1), react it with excess thionyl chloride at 70°C for 24 h to activate the carboxyl group and convert it into an acyl chloride group.
[0059] (3) The product obtained in step (2) is dispersed in excess ethylene glycol to obtain hydroxylated conductive carbon material;
[0060] (4) Using 2-bromoisobutyryl bromide as the brominating agent, the hydroxyl groups on the conductive carbon material are condensed by bromine and hydroxylation, with triethylamine as the acid-binding agent and dimethylaminopyridine as the catalyst. The reaction is carried out at room temperature for 24 hours to remove hydrogen bromide and obtain the brominated carbon material. The mass ratio of hydroxylated conductive carbon material, brominating agent and acid-binding agent is 1.2:1:1; the mass ratio of acid-binding agent and catalyst is 10:1.
[0061] (5) The dried product of step (4) is mixed with pentamethyldiethylenetriamine and N,N-dimethylformamide in an amount of 10:1.2:1. After nitrogen purging, 0.2g of vinylpyrrolidone is injected and the mixture is stirred at 80°C for 24-48h. The resulting solution is diluted with anhydrous ethanol, filtered, and repeatedly washed to obtain polyvinylpyrrolidone grafted and modified conductive carbon material.
[0062] A highly dispersible composite binder was prepared by mixing polyvinylpyrrolidone-grafted modified conductive carbon material with polyvinylidene fluoride (Dongyue DS202) at a mass ratio of 1:1 and ball milling the mixture at 200 rpm for 2 hours.
[0063] The composite binder is used at a dosage of 4% in the slurry preparation, without the need for additional conductive carbon black. The battery slurry performance test results are shown in Table 2.
[0064] The test method described in this invention is as follows:
[0065] (1) Determination of modified monomer content
[0066] PVDF resin was dissolved in deuterated acetone, and the content of modified monomers was calculated by measuring the 1H NMR spectrum of the resin using a nuclear magnetic resonance spectrometer and the ratio of peak areas. Alternatively, the content of modified monomers could be determined by potentiometric titration.
[0067] (2) Calculation of polyvinylpyrrolidone block content
[0068] The mass of the polyvinylidene fluoride block copolymer is obtained by subtracting the mass of the polyvinylidene fluoride block from the total weight of the prepared polyvinylidene fluoride-polyvinylpyrrolidone block copolymer. Dividing this mass by the total weight of the block copolymer gives the content of the polyvinylpyrrolidone block.
[0069] (3) Determination of weight-average molecular weight (polyvinylidene fluoride block)
[0070] Accurately weigh (0.0200±0.0001) g of sample into a 25 mL capped glass vial, transfer it into 10.0 mL of LDM solution using a pipette, heat and stir magnetically at 60 °C (600 r / min) in a metal bath for 4 h, and after cooling, filter the sample solution through a disposable organic phase syringe filter to obtain the test solution.
[0071] Based on the different retention times of substances with different molecular weights in gel permeation chromatography columns, a series of polymers with known molecular weights were used as standards to plot a calibration curve of retention volume versus molecular weight, and the relative molecular weight of the samples was calculated.
[0072] (4) Preparation of battery slurry
[0073] The battery slurry is prepared according to the proportions in the table below. Using a dual planetary stirrer, NMP and PVDF are first added to the stirrer at a ratio of NMP:PVDF = 10:1 to prepare PVDF slurry. The mixture is stirred and dissolved for 120 hours. Then, SP and CNT solutions are added and dispersed for 120 minutes. Finally, LFP and the remaining NMP are added in 2-3 batches, with each batch dispersed for 5 minutes. After all the additions are completed, the mixture is dispersed for 180 minutes. Finally, the mixture is degassed under vacuum for 30 minutes to obtain the battery slurry.
[0074]
[0075] (5) Evaluation of slurry dispersibility
[0076] The dispersibility of the slurry is evaluated by its viscosity and stability. The viscosity of the slurry is tested using a rotational rheometer (25℃). For the same solid content, a lower viscosity indicates better dispersibility, and vice versa. In addition, the stability is evaluated by comparing the viscosity change (viscosity ratio) of the slurry before and after standing for 24 hours.
[0077] Slurry viscosity testing: The slurry viscosity was tested using a rotational viscometer.
[0078] (6) Determination of peel strength
[0079] The electrode paste from method (4) above was applied to a 10 μm thick aluminum foil using a rod coater and dried at 110°C for 30 minutes to produce a single-sided unit area weight of 80-100 g / m². 2 Single-sided coated electrode.
[0080] The single-sided coated electrode was cut into pieces 50 mm long and 20 mm wide, and then subjected to a pressure of 0.8 t / cm at room temperature. 2 The test piece was made by planar pressing.
[0081] Adhesive tape was pasted onto the coated electrode surface of the test piece, and aluminum foil was used as the "flexible adhesive material". According to GB / T2792-2014, a tensile testing machine was used to conduct a 180-degree peel test at a tensile speed of 200 mm / min to determine the peel strength.
[0082] Table 1 Resin Test Results
[0083]
[0084] Table 2. Test results of battery slurry performance
[0085]
Claims
1. A polyvinylidene fluoride-polyvinylpyrrolidone block copolymer, characterized in that, The copolymer is a diblock copolymer of polyvinylidene fluoride (PVDF) blocks and polyvinylpyrrolidone (PVP) blocks, wherein the PVDF blocks are modified blocks containing polar monomers; the PVP blocks constitute 3.3-16.7 wt% of the copolymer; the polar monomers are at least one selected from acryloyloxyethyl succinate, monomethyl maleate, and methacrylic acid, and the content of the polar monomers is 0.2-2 mol% of the PVDF blocks. The preparation method of the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer includes the following steps: (1) Add deionized water, 5-15wt% polar monomer, dispersant and chain transfer agent to the reactor. After deoxygenating the polymerization reactor with nitrogen, heat it to 40-60℃. Introduce vinylidene fluoride monomer to the reactor until the pressure is 8.0-14.0MPa. Add initiator to carry out polymerization reaction. During the polymerization process, maintain the polymerization pressure by adding vinylidene fluoride monomer. At the same time, continuously add the remaining polar monomer. When the mass ratio of the added amount of vinylidene fluoride monomer to the chain transfer agent is 200-450:1, stop adding. Cool down to recover the unreacted VDF monomer and discharge the material. After coagulation, washing and drying, obtain iodine-terminated polyvinylidene fluoride resin. (2) The iodine-terminated polyvinylidene fluoride resin, N-vinylpyrrolidone monomer and initiator prepared in step (1) are polymerized in an organic solvent. The polymerization reaction is carried out at a temperature of 50-90℃ and a time of 10-20h. After the reaction is completed, the reaction solution is precipitated, washed and dried to obtain the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer product.
2. The polyvinylidene fluoride-polyvinylpyrrolidone block copolymer according to claim 1, characterized in that, The weight-average molecular weight of the polyvinylidene fluoride block is 500,000 to 2,000,000.
3. The method for preparing the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer according to claim 1, characterized in that, Includes the following steps: (1) Add deionized water, 5-15wt% polar monomer, dispersant and chain transfer agent to the reactor. After deoxygenating the polymerization reactor with nitrogen, heat it to 40-60℃. Introduce vinylidene fluoride monomer to the reactor until the pressure is 8.0-14.0MPa. Add initiator to carry out polymerization reaction. During the polymerization process, maintain the polymerization pressure by adding vinylidene fluoride monomer. At the same time, continuously add the remaining polar monomer. When the mass ratio of the added amount of vinylidene fluoride monomer to the chain transfer agent is 200-450:1, stop adding. Cool down to recover the unreacted VDF monomer and discharge the material. After coagulation, washing and drying, obtain iodine-terminated polyvinylidene fluoride resin. (2) The iodine-terminated polyvinylidene fluoride resin, N-vinylpyrrolidone monomer and initiator prepared in step (1) are polymerized in an organic solvent. The polymerization reaction is carried out at a temperature of 50-90℃ and a time of 10-20h. After the reaction is completed, the reaction solution is precipitated, washed and dried to obtain the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer product.
4. The method for preparing the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer according to claim 3, characterized in that, The mass ratio of deionized water, polar monomer, dispersant, initiator and chain transfer agent mentioned in step (1) is 1000-1500: 5-10: 0.2-0.4: 0.3-0.6:
1.
5. The method for preparing the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer according to claim 3, characterized in that, The initiator mentioned in step (1) is one of diisopropyl peroxydicarbonate and tert-butyl peroxypentanoate; the dispersant is methylcellulose; and the chain transfer agent is perfluoroiodoethane.
6. The method for preparing the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer according to claim 3, characterized in that, The initiator mentioned in step (2) is azobisisobutyronitrile; the organic solvent is N,N-dimethylformamide.
7. The method for preparing the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer according to claim 3, characterized in that, The drying temperature in step (2) is 80-120℃ and the time is 20-30h.
8. The use of the polyvinylidene fluoride-polyvinylpyrrolidone block copolymer according to any one of claims 1-2 as a battery binder.
Citation Information
Patent Citations
Vinylidene fluoride copolymers
CN101679563A
Preparation method of high-dispersity composite binder for cathode of lithium ion battery
CN111029585A
Preparation method of modified polyvinylidene fluoride in lithium ion battery
CN113224305A
Method for preparing pre-irradiated PVDF (Polyvinylidene Fluoride) grafted with NVP (N-Vinyl Pyrrolidinone) and prepared copolymer
CN102504116A
Preparation method of polyvinylidene fluoride-polyvinylpyrrolidone (PVDF-PVP) block copolymer
CN104558452A