A MEMS micro-hotplate and preparation method thereof
By using the structure of silicon substrate, porous silicon insulation layer and silicon oxide-silicon nitride-silicon oxide composite insulation layer in the MEMS micro-hot plate, the problems of difficulty in manufacturing and low mechanical strength of the micro-hot plate are solved, and a more stable and efficient heating performance, and reduces electromagnetic interference and signal loss.
Patent Information
- Application Number
- CN202311365959.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-20
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-10-20
AI Technical Summary
Existing micro-hot plates are difficult to manufacture and have low mechanical strength, making them unable to meet actual needs.
It adopts the structure of silicon substrate, porous silicon thermal insulation layer, silicon oxide-silicon nitride-silicon oxide composite insulation layer, coplanar heating electrode and test electrode, and silicon nitride isolation ring. Through electrochemical etching, chemical vapor deposition and photolithography The MEMS micro-hot plate is prepared by process to improve the mechanical strength and stability.
It reduces the manufacturing difficulty of the micro-hot plate, enhances the structural stability and mechanical strength, avoids the process of suspended heating zone, and improves the device's resistance to cold and hot shock and electromagnetic interference performance.
Smart Images

Figure CN117401643B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of micro-electro-mechanical systems (MEMS) sensors, and in particular to a MEMS micro-hotplate and a preparation method thereof. Background Art
[0002] The rapid development of science and technology has brought many conveniences to people, but it is also accompanied by problems such as resources and the environment. In particular, the irregular treatment and emission of some polluted gases have seriously affected the air quality and affected our health at all times. In some indoor operating environments, the space is small and the gas is not easy to disperse, so it is more necessary to pay attention to the concentration of harmful substances in the air. Gas sensors can effectively detect and prevent air environment, and are widely used in environmental monitoring, disaster prevention and alarm, chemical industry and other fields. They have become an indispensable part of daily production and life.
[0003] Traditional gas sensors are large in size, high in power consumption, and low in circuit integration. MEMS gas sensors have the advantages of micro-nanostructure, low power consumption, high integration, and good repeatability, and have become a research hotspot in portable and distributed monitoring applications. Metal oxide semiconductor gas sensors based on silicon wafers have high sensitivity, good response and stability, and are currently the most widely used type of gas sensors. The micro-hotplate is the core structure of the MEMS gas sensor, which is used to heat the gas-sensitive material (metal oxide semiconductor) coated on the sensor to reach the operating temperature and improve its gas-sensitive response.
[0004] Conventional micro-hotplates are mostly suspended structures. The suspended micro-hotplates use several cantilever beams as mechanical supports to connect the heating platform and the insulating layer and suspend them through a front-side bulk silicon process or a sacrificial layer process. They are difficult to manufacture and have low mechanical strength, making them difficult to meet actual needs. Summary of the invention
[0005] The present application provides a MEMS micro-hotplate and a preparation method thereof, thereby solving the problems of high difficulty in manufacturing and low mechanical strength of conventional micro-hotplates in the prior art, reducing the difficulty in manufacturing the micro-hotplate and improving the mechanical strength of the micro-hotplate.
[0006] The embodiment of the present application provides a MEMS micro-hotplate, comprising:
[0007] Silicon substrate;
[0008] A heat-insulating layer is arranged on the upper part of the silicon substrate, and the heat-insulating layer is made of porous silicon;
[0009] An insulating layer, disposed above the thermal insulation layer, the insulating layer comprising, from bottom to top, a first silicon oxide layer, a silicon nitride layer, and a second silicon oxide layer;
[0010] A metal layer is arranged above the insulating layer, and the metal layer comprises a coplanar heating electrode and a testing electrode, the testing electrode is surrounded by the heating electrode, and an isolation ring is arranged between the testing electrode and the heating electrode.
[0011] The beneficial effects of the above embodiments are as follows: compared with the suspended structure, the MEMS micro-hotplate has good structural stability, and does not require a suspended heating zone process, and has low manufacturing difficulty, thereby enhancing the stability and practicality of the MEMS micro-hotplate; the insulating layer of the MEMS micro-hotplate selects a composite structure of silicon oxide-silicon nitride-silicon oxide, and the power consumption required for silicon oxide to maintain a steady state is small, but the temperature distribution fluctuates greatly; the power consumption required for silicon nitride to maintain a steady state is large, but the temperature distribution is more uniform, the first silicon oxide layer acts as a contact layer to protect the silicon substrate at the same time, and the silicon nitride layer acts as a filling layer to make the temperature distribution more uniform The second silicon oxide layer is used as a protective layer. The thermal conductivity of silicon oxide is small, so the temperature in the heating area can be higher to prevent the temperature from diffusing to the edge. While protecting the lower structure, it is close to the metal layer to improve the thermal response of the micro-hotplate. This composite structure improves the mechanical strength and resistance to thermal shock of the device, and also has good electrical insulation and impurity blocking ability. In addition, the heating electrode and the test electrode of the MEMS micro-hotplate adopt a coplanar structure to avoid the influence of parasitic parameters on the device. At the same time, the heating area and the test area are independent of each other to avoid short circuit when the gas-sensitive material is coated.
[0012] Based on the above embodiments, the present application can be further improved as follows:
[0013] In one embodiment of the present application, the silicon substrate has a resistivity of 0.01-0.02 Ω.cm, a thickness of 380-420 μm, and a crystal orientation of <100> P-type silicon.
[0014] In one embodiment of the present application, the porosity of the porous silicon is 65% to 70%. The abundant holes in the porous silicon can absorb air, so the thermal conductivity is low, but since the silicon substrate and the insulating layer of the micro-hotplate are connected by an insulating layer, the porous silicon here needs to take into account the supporting function, and too high a porosity leads to too low a mechanical strength, so the porosity of the porous silicon cannot be higher than 70%.
[0015] In one embodiment of the present application, the thickness of the insulating layer is 11000Å, and the thickness ratio of the first silicon oxide layer, the silicon nitride layer, and the second silicon oxide layer is 3:5:3. The mechanical strength of the device is improved while the device's ability to resist thermal shock is improved.
[0016] In one embodiment of the present application, the heating electrode adopts a serpentine structure to surround the test electrode, the test electrode adopts a symmetrical comb-shaped interdigitated electrode structure, and the bending angle of the test electrode and the connecting section of the Pad end is 135°. If the test electrode is arranged at a right angle or an acute angle, a strong charge edge will be generated, and the edge will be in a concentrated energy state, causing electromagnetic interference; the bending angle of the test electrode is 135 degrees, which will make the edge distribution more uniform, the current smoother, and the signal reflection less; the symmetrical distribution of the electrodes will offset the magnetic field generated by the lead-in electricity, so the symmetrically designed test electrodes and the connecting sections in the micro-hotplate are bent at 135°, thereby reducing electromagnetic interference and signal loss to the test signal.
[0017] In one embodiment of the present application, the width of the connection between the end of the test electrode and the pad end gradually increases. The end of the test electrode adopts an extended design and is connected to the side of the pad end to increase the contact with the pad end and fix the electrode.
[0018] In one embodiment of the present application, the isolation ring is made of silicon nitride. Silicon nitride has certain thermal conductivity, low thermal expansion coefficient, good stability, and is a good insulating material. Silicon nitride is used as an isolation layer to prevent the heating area and the test area from short-circuiting when the conductive gas-sensitive material is coated, which affects the normal operation of the device.
[0019] In one embodiment of the present application, a passivation layer is disposed under the silicon substrate, and the passivation layer is silicon oxide, which is used to protect the silicon substrate.
[0020] The present application embodiment provides a method for preparing the above-mentioned MEMS micro-hotplate, comprising the following steps:
[0021] S1: preparing a P-type silicon substrate;
[0022] S2: preparing porous silicon by electrochemical etching on the surface of the silicon substrate to form the thermal insulation layer;
[0023] S3: Depositing the insulating layer on the thermal insulation layer using a chemical vapor deposition method;
[0024] S4: patterning the photoresist by photolithography combined with etching, and depositing the metal on the insulating layer by magnetron sputtering to form the metal layer;
[0025] S5: depositing silicon nitride on the metal layer, and after photolithography and etching, forming the isolation ring between the heating electrode and the test electrode of the metal layer;
[0026] S6: Using PVD sputtering to thicken the electrode at the Pad on the metal layer.
[0027] In one embodiment of the present application, in step S2, the porous silicon preparation method is as follows: at a current density of 60 mA / cm 2 Under the condition of , the silicon wafer is etched in a mixture of hydrofluoric acid and ethanol for 30 minutes. In the mixture of hydrofluoric acid and ethanol, a certain current density is applied to the silicon wafer to obtain porous silicon, and the excess porous silicon can be etched by KOH solution.
[0028] In one embodiment of the present application, the silicon oxide in the insulating layer is prepared by LPCVD, the silicon nitride in the insulating layer is prepared by PECVD, and the silicon nitride of the isolation ring is prepared by PECVD. Silicon oxide has good insulation performance and low thermal expansion coefficient, and the silicon nitride structure is more compact and has strong resistance to thermal shock. Silicon nitride is prepared by PECVD, and the preparation temperature meets the temperature that the MEMS micro-hotplate can withstand after metallization.
[0029] One or more technical solutions provided in the embodiments of the present application have at least the following technical effects or advantages:
[0030] 1. Compared with the suspended structure, the MEMS micro-hotplate has good structural stability, does not require the suspended heating zone process, and has low manufacturing difficulty, thereby enhancing the stability and practicality of the MEMS micro-hotplate;
[0031] 2. The insulating layer of the MEMS micro-hotplate is a composite structure of silicon oxide-silicon nitride-silicon oxide, which improves the mechanical strength and thermal shock resistance of the device;
[0032] 3. The heating electrode and the test electrode of the MEMS micro-hotplate adopt a coplanar structure to avoid the influence of parasitic parameters on the device; at the same time, the heating area and the test area are independent of each other to avoid short circuit when the gas-sensitive material is coated;
[0033] 4. The micro-hotplate uses symmetrically designed test electrodes and a 135° bend in the connecting section, thereby reducing electromagnetic interference and signal loss to the test signal. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.
[0035] Figure 1 This is a schematic diagram of a cross-sectional structure of a MEMS micro-hotplate in an embodiment of the present invention;
[0036] Figure 2 Schematic diagram of the distribution of heating electrodes and test electrodes in an embodiment of the present invention;
[0037] Figure 3 This is a schematic diagram of the connection between the test electrode and the Pad end in an embodiment of the present invention;
[0038] Figure 4 A flowchart of a method for preparing a MEMS micro-hotplate according to an embodiment of the present invention;
[0039] Among them, 1. silicon substrate, 2. thermal insulation layer, 3. insulating layer, 31. first silicon oxide layer, 32. silicon nitride layer, 33. second silicon oxide layer, 4. metal layer, 41. heating electrode, 42. test electrode, 5. isolation ring, 6. pad end, 7. passivation layer. DETAILED DESCRIPTION
[0040] The present invention is further explained below in conjunction with specific implementation methods. It should be understood that these implementation methods are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.
[0041] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0042] In the description of the present invention, it should be noted that the orientation or positional relationship indicated by the terms "vertical", "peripheral surface", etc. is based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the invented product is usually placed when in use, which is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. In addition, the terms "first", "second", "third", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0043] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0044] In the description of the present invention, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in the present invention and the features of different embodiments or examples without contradiction.
[0045] The embodiment of the present application provides a MEMS micro-hotplate and a preparation method thereof, thereby solving the problem of high difficulty in manufacturing and low mechanical strength of conventional micro-hotplates in the prior art, reducing the difficulty in manufacturing the micro-hotplate and improving the mechanical strength of the micro-hotplate.
[0046] The technical solution in the embodiment of the present application is to solve the above problems, and the overall idea is as follows:
[0047] Embodiment 1:
[0048] like Figure 1-3 As shown, a MEMS micro-hotplate is applied to a gas sensor, comprising: a silicon substrate 1, a heat insulation layer 2, an insulating layer 3, a metal layer 4, an isolation ring 5, a pad end 6 and a passivation layer 7;
[0049] The silicon substrate 1 has a resistivity of 0.01-0.02Ω.cm, a thickness of 380-420μm, and a crystal orientation of <100> P-type silicon;
[0050] The heat insulation layer 2 is arranged on the upper part of the silicon substrate 1, and the material of the heat insulation layer 2 is porous silicon, and the porosity of the porous silicon is 65% to 70%;
[0051] The insulating layer 3 is disposed above the heat-insulating layer 2, and the insulating layer 3 includes, from bottom to top, a first silicon oxide layer 31, a silicon nitride layer 32, and a second silicon oxide layer 33;
[0052] The metal layer 4 is arranged above the insulating layer 3, and the metal layer 4 includes a coplanar heating electrode 41 and a test electrode 42. The heating electrode 41 adopts a serpentine structure to surround the test electrode 42. The test electrode 42 adopts a symmetrical comb-shaped interdigitated electrode structure, and the bending angle of the connecting section between the test electrode 42 and the pad end 6 is 135°. The width of the connecting section between the end of the test electrode 42 and the pad end 6 gradually increases. An isolation ring 5 is arranged between the test electrode 42 and the heating electrode 41, and the isolation ring 5 is made of silicon nitride.
[0053] The passivation layer 7 is disposed under the silicon substrate 1 .
[0054] The technical solutions in the above embodiments of the present application have at least the following technical effects or advantages:
[0055] 1. Compared with the suspended structure, the MEMS micro-hotplate has good structural stability, does not require the suspended heating zone process, and has low manufacturing difficulty, thereby enhancing the stability and practicality of the MEMS micro-hotplate;
[0056] 2. The insulating layer of the MEMS micro-hotplate is a composite structure of silicon oxide-silicon nitride-silicon oxide, which improves the mechanical strength and thermal shock resistance of the device;
[0057] 3. The heating electrode and the test electrode of the MEMS micro-hotplate adopt a coplanar structure to avoid the influence of parasitic parameters on the device; at the same time, the heating area and the test area are independent of each other to avoid short circuit when the gas-sensitive material is coated;
[0058] 4. The micro-hotplate uses symmetrically designed test electrodes and a 135° bend in the connecting section, thereby reducing electromagnetic interference and signal loss to the test signal.
[0059] Embodiment 2:
[0060] like Figure 4 As shown, a method for preparing the above-mentioned MEMS micro-hotplate comprises the following steps:
[0061] S1: Prepare P-type silicon substrate, crystal orientation <100> .
[0062] First, the silicon wafer is placed in a solution of concentrated H2SO4 and H2O2 for cleaning to remove organic pollutants on the surface; after rinsing with deionized water, it is further placed in a mixture of HF and deionized water to remove the surface oxide layer; after rinsing with deionized water, it is ultrasonically cleaned in acetone and ethanol solutions respectively; finally, it is placed in anhydrous ethanol for later use.
[0063] S2: Electrochemical etching is used to prepare porous silicon on the surface of the silicon substrate to form a thermal insulation layer.
[0064] In a mixture of hydrofluoric acid and ethanol, a certain current density is applied to the silicon wafer to obtain porous silicon. In this example, the current density is 60 mA / cm 2 Under the conditions, the corrosion lasts for 30 minutes, the corrosion depth is about 70μm, and the excess porous silicon can be corroded by KOH solution.
[0065] S3: A chemical vapor deposition method is used to deposit an insulating layer on the thermal insulation layer, and a thermal oxidation method is used to generate a passivation layer on the back side of the silicon substrate.
[0066] The insulating layer is a composite structure of silicon oxide-silicon nitride-silicon oxide, wherein silicon oxide is prepared by LPCVD and silicon nitride is prepared by PECVD. The thickness of the composite structure of silicon oxide-silicon nitride-silicon oxide of the insulating layer is 11000Å, and the thickness ratio of each layer is 3:5:3.
[0067] S4: Photoresist is patterned by photolithography combined with etching, and then metal is deposited on the insulating layer by magnetron sputtering to form a metal layer.
[0068] The excess photoresist and metal are stripped off using solutions such as acetone; the metal layer includes a heating electrode and a test electrode, and the heating electrode and the test electrode are sputtered with metal Pt with a thickness of 3000±300Å.
[0069] S5: Silicon nitride is deposited on the metal layer, and after photolithography and etching, an isolation ring is formed between the heating electrode and the test electrode of the metal layer.
[0070] The thickness of the isolation ring is about 6000~8000Å and is prepared by PECVD.
[0071] S6: Form a thickened electrode at the pad of the metal layer using PVD sputtering.
[0072] A layer of metal thickened electrode (Au) is re-sputtered at the position of the pad as a pad, that is, the end of the pad contains the lower metal Pt and the upper metal Au. The thickness of the thickened electrode is 4000±400Å, and the sputtering method is magnetron sputtering.
[0073] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a MEMS micro-hotplate, characterized in that: The following steps are involved: S1: prepare silicon substrate; S2: directly preparing porous silicon by electrochemical etching on the surface of the silicon substrate to form a heat insulation layer; S3: depositing an insulating layer on the thermal insulation layer by a chemical vapor deposition method, wherein the insulating layer includes, from bottom to top, a first silicon oxide layer, a silicon nitride layer, and a second silicon oxide layer; S4: Patterning of the photoresist is formed by photolithography combined with etching, and metal is deposited on the insulating layer by magnetron sputtering to form a metal layer, wherein the metal layer includes a coplanar heating electrode and a test electrode, wherein the heating electrode adopts a serpentine structure to surround the test electrode, and the test electrode adopts a symmetrical comb-shaped interdigitated electrode structure, and the bending angle of the connecting section between the test electrode and the pad end is 135°, and the width of the connecting section between the end of the test electrode and the pad end gradually increases; S5: depositing silicon nitride on the metal layer, and after photolithography and etching, forming an isolation ring between the heating electrode and the test electrode of the metal layer; S6: Using PVD sputtering to thicken the electrode at the Pad on the metal layer.
2. The preparation method according to claim 1, characterized in that: In step S2, the porous silicon is prepared as follows: etching in a mixture of hydrofluoric acid and ethanol for 30 minutes at a current density of 60 mA / cm2.
3. The preparation method according to claim 1, characterized in that: The silicon substrate has a resistivity of 0.01 to 0.02 Ω.cm, a thickness of 380 to 420 μm, and a crystal orientation of <100> P-type silicon.
4. The preparation method according to claim 1, characterized in that: The porosity of the porous silicon is 65% to 70%.
5. The preparation method according to claim 1, characterized in that: The thickness of the insulating layer is The thickness ratio of the first silicon oxide layer, the silicon nitride layer, and the second silicon oxide layer is 3:5:
3.
6. The preparation method according to claim 1, characterized in that: The width of the connection between the end of the test electrode and the Pad end gradually increases.
7. The preparation method according to claim 1, characterized in that: The isolation ring is made of silicon nitride.
8. The preparation method according to claim 1, characterized in that: A passivation layer is arranged under the silicon substrate.