Catalytic slurry for anti-shedding and water-resistant ceramic fiber filter tube, preparation method and application

By preparing a catalytic slurry that is resistant to shedding and water on a ceramic fiber filter tube, and using titanium-silicon composite sol and ultrasonic dispersion technology, the problem of uneven catalyst distribution and easy shedding is solved, the reaction activity and stability of the catalyst are improved, and the Production costs and energy consumption are significantly improved, and filter tube performance is significantly improved.

CN117427628BActive Publication Date: 2024-10-11HANGZHOU XIFU ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311320321.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-12
Publication Date
2024-10-11
Estimated Expiration
2043-10-12

AI Technical Summary

Technical Problem

The existing filter tube catalyst implantation technology has problems such as uneven catalyst distribution, easy falling off, high energy consumption, high production costs and environmental pollution. Especially in ceramic fiber filter tubes, the catalyst implantation and stability are insufficient, which affects denitrification. Efficiency and filter tube performance.

Method used

Use butyl titanate and oxalic acid aqueous solution to form an organic titanium precursor solution, add organic silane to form a titanium-silicon composite sol, and add a dispersant and a penetrating agent after ultrasonic dispersion to prepare a catalytic slurry that is resistant to shedding and water resistance, and is dried and activated in the A uniformly distributed catalyst-titanium-silicon composite is formed on the ceramic fiber filter tube to improve the reaction activity and stability of the catalyst.

Benefits of technology

It achieves uniform distribution and high reactivity of the catalyst, reduces shedding and moisture adsorption, improves the mechanical strength and water resistance of the filter tube, reduces production costs and energy consumption, and significantly improves the performance of the ceramic fiber filter tube.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004490776230000051
    Figure BDA0004490776230000051
  • Figure BDA0004490776230000061
    Figure BDA0004490776230000061
Patent Text Reader

Abstract

The present invention discloses a catalytic slurry for an anti-shedding and water-resistant ceramic fiber filter tube, a preparation method and an application. The steps of the method for preparing the catalytic slurry are as follows: S1: dissolving butyl titanate in an oxalic acid aqueous solution to form an organic titanium precursor solution; S2: adding an organic silane to the organic titanium precursor solution of S1 to prepare a titanium-silicon composite sol; S3: adding a dispersant and a penetrant to the titanium-silicon composite sol of S2, and then adding vanadium oxalate pentahydrate and ammonium heptamolybdate tetrahydrate, and obtaining a catalytic slurry after ultrasonic dispersion. The catalytic slurry of the present invention can also better bond with the ceramic fiber filter tube, improve the mechanical strength and stability of the catalyst, and make it not easy to fall off; at the same time, due to the low surface energy, it can prevent water molecules from being adsorbed on the catalyst surface, thereby improving the water resistance and stability of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to a catalytic slurry for an anti-shedding and water-resistant ceramic fiber filter tube, a preparation method and an application thereof. Background Art

[0002] SCR denitration catalyst is one of the most mature technologies for industrial flue gas treatment of nitrogen compounds. However, it is limited by the flue gas temperature, dust and heavy metals, which will affect the honeycomb catalyst. Denitration is done first and then dust removal, which will inevitably cause dust to block the catalyst. Dust removal is done first and then denitration. Traditionally, bag dust removal is used, but the flue gas temperature is low, which is not conducive to denitration. Ceramic fiber tubes can achieve high-temperature dust removal, ensuring that the flue gas is in the most suitable reaction temperature zone when passing through the catalyst. The ceramic fiber tube is porous inside, combined with catalyst implantation, which can achieve integrated dust removal and denitration.

[0003] At present, the implantation of catalyst in filter tube mainly includes adding catalyst in the pulping process of filter tube preparation before filter tube is formed and implanting catalyst in various ways after filter tube is formed. In the former filter tube preparation process, when the filter tube is formed by using fiber slurry, the water in the slurry will be squeezed and sucked out and then dried to form. It is difficult to ensure the implantation amount and uniformity of the catalyst. In addition, the wastewater in the filter tube production process is difficult to reuse. Adding catalyst increases the difficulty of wastewater treatment and causes serious environmental pollution. The catalyst is implanted after the filter tube is formed. At present, the main method is to prepare catalytic powder first, then crush and grind the powder, and add various additives to the filter tube after pulping. The powder preparation process requires mixing, stirring and calcining, and then crushing and grinding. The filter tube is implanted after pulping. The whole process is complicated, the energy consumption is high, and the crushing and grinding requirements are high. The filter tube is mainly used to filter dust, and the pores are small. The slurry particle size is too large to penetrate into the filter tube and ensure uniform distribution. In addition, the implantation of large catalytic particles into the filter tube will block the pores of the filter tube, increase the resistance of the filter tube, and increase the operating cost of the catalyst filter tube. In addition, the prepared powders are mainly some inorganic oxides, which are difficult to crush and grind. At the same time, it is difficult to attach to the fibers when implanted in the filter tube, and it is inevitable that they will fall off during the flue gas circulation and backblowing process. There are also some slurries that are ground by adding molecular sieve matrix (or directly adding nano-titanium dioxide, treated or coated active nano-titanium carriers, and then adding active components to grind, slurry and then coat, and physically crush and mix the materials. The active components are difficult to contact evenly with the carrier to form a uniform catalytic slurry, and the denitrification activity is greatly reduced, and the production cost is relatively high. In addition, there are some schemes that treat the filter tube matrix, coat and bond multiple times, and implant catalytic carriers and active ingredients inside the filter tube. The entire catalytic filter tube production process is long, which affects production efficiency. Summary of the invention

[0004] Based on the technical problems existing in the background technology, the present invention proposes a catalytic slurry for an anti-shedding and water-resistant ceramic fiber filter tube, a preparation method and an application thereof, so as to improve the anti-shedding, water-resistant ability and reaction activity of the catalyst.

[0005] The method for preparing the catalytic slurry for the anti-shedding and water-resistant ceramic fiber filter tube proposed by the present invention comprises the following steps:

[0006] S1: dissolving butyl titanate in an oxalic acid aqueous solution to form an organic titanium precursor solution;

[0007] S2: adding organosilane to the organotitanium precursor solution of S1 to prepare a titanium-silicon composite sol;

[0008] S3: Add a dispersant and a penetrant to the titanium-silicon composite sol of S2, and then add vanadyl oxalate pentahydrate and ammonium heptamolybdate tetrahydrate, and obtain a catalytic slurry after ultrasonic dispersion.

[0009] Preferably, the mass ratio of butyl titanate, organosilane, dispersant, penetrant, vanadyl oxalate pentahydrate and ammonium heptamolybdate tetrahydrate is 100:15-20:3-5:1-3:30-50:8-12.

[0010] Preferably, the dispersant is P40 dispersant, and the penetrant is polysiloxane.

[0011] Preferably, the organosilane is a mixture of methyltriisopropenyloxysilane and diphenyldimethoxysilane in a mass ratio of 5:1-25.

[0012] Preferably, the frequency of ultrasound in S3 is 40 KHz, and the time of ultrasound is 40-80 min.

[0013] The invention provides a catalytic slurry for a ceramic fiber filter tube that is resistant to shedding and water-resistance and is prepared by the method mentioned above.

[0014] The present invention provides the application of the above catalytic slurry on ceramic fiber filter tubes.

[0015] Preferably, the catalytic slurry is diluted and coated on the inside and outside of the ceramic fiber filter tube, and then dried and activated.

[0016] Preferably, the drying temperature is 85-120° C. and the drying time is 5-10 h.

[0017] Preferably, the activation temperature is 320-380° C. and the activation time is 1-3 h.

[0018] Beneficial technical effects of the present invention:

[0019] (1) The present invention implants the catalyst by introducing a soluble active component into the titanium-silicon composite sol. When activated at high temperature, bonding occurs between the organic titanium source, the active component, and the organic silane, and a catalyst-titanium-silicon composite can be directly generated in situ on the surface of the filter tube fiber. The denitration catalyst is more evenly distributed, and the pressure difference is smaller after the catalyst is implanted in the catalytic filter tube. Compared with directly introducing titanium dioxide and active components, this method can make the active ingredients more evenly and tightly combined with titanium silicon to form an integrated composite, thereby improving the reaction activity of the catalyst.

[0020] (2) The catalytic slurry of the present invention has a strong permeability and can better penetrate the inner and outer surfaces of the ceramic fiber filter tube, thereby improving the mechanical strength and stability of the catalyst and making it less likely to fall off; at the same time, due to its low surface energy, it can prevent water molecules from being adsorbed on the catalyst surface, thereby improving the water resistance and stability of the catalyst.

[0021] (3) The organic components in the organic silica gel form a porous structure during the activation process, which helps to load more effective components of the catalyst. At the same time, the SiO2 formed after the organic silica gel is activated has extremely strong hydrophobicity, which can improve the water resistance of the catalyst.

[0022] (4) The organosilane of the present invention is composed of methyltriisopropenyloxysilane and diphenyldimethoxysilane, which has a synergistic effect on improving the reaction activity, water resistance and sulfur resistance of the ceramic fiber filter tube, thereby significantly improving the performance of the prepared ceramic fiber filter tube.

[0023] (5) The valence state of vanadium after drying affects the color of the filter tube after drying, and the uniformity of the distribution of the vanadium source affects the surface color of the filter tube (the appearance of the finished product). The introduction of an organic vanadium source with a relatively high solubility, due to the excellent permeability of the slurry and the uniform distribution of the active ingredients, reduces the coating amount of a single filter tube from the common 13-15 kg on the market to 10-12 kg while ensuring a uniform appearance, which greatly reduces the heat consumption during the production and drying process, saves production costs and improves production efficiency. DETAILED DESCRIPTION

[0024] The present invention will be further explained below in conjunction with specific embodiments.

[0025] Example 1

[0026] The method steps for preparing the catalytic slurry proposed by the present invention are as follows:

[0027] S1: Add 35g of oxalic acid to 435g of aqueous solution, then add 333.6g of butyl titanate to the stirred oxalic acid aqueous solution to form an organic titanium precursor solution; then add 58g of organic silane, and perform high-speed dispersion for 30min at a dispersion speed of 800r / min to form a titanium-silicon composite sol; wherein the organic silane is a mixture of methyltriisopropenyloxysilane and diphenyldimethoxysilane in a mass ratio of 1:1.

[0028] S2: Add 14 g of P40 dispersant and 8.7 g of polysiloxane to the prepared titanium-silicon composite sol, then add 140.5 g of vanadyl oxalate pentahydrate and 32 g of ammonium heptamolybdate tetrahydrate, stir and dissolve, then subject the slurry to ultrasonic dispersion at 40 kHz for 60 min to prepare the target product.

[0029] When in use, stir the slurry evenly and add 1 times water to dilute it. After dilution, apply it on a small filter tube at a weight ratio of 1:1 (the whole filter tube weighs 10 kg), dry it at 105°C for 8 hours to simulate the filter tube coating and drying process, and then activate it at 350°C in a muffle furnace for 2 hours to simulate on-site yellow tube activation. Finally, the sample is tested for denitrification efficiency and other tests.

[0030] Example 2

[0031] The method steps for preparing the catalytic slurry proposed by the present invention are as follows:

[0032] S1: Add 35g of oxalic acid to 435g of aqueous solution, then add 333.6g of butyl titanate to the stirred oxalic acid aqueous solution to form an organic titanium precursor solution; then add 50g of organic silane, and perform high-speed dispersion for 30min at a dispersion speed of 800r / min to form a titanium-silicon composite sol; wherein the organic silane is a mixture of methyltriisopropenyloxysilane and diphenyldimethoxysilane in a mass ratio of 1:1.

[0033] S2: Add 10 g of P40 dispersant and 7.6 g of polysiloxane to the prepared titanium-silicon composite sol, then add 101 g of vanadyl oxalate pentahydrate and 27 g of ammonium heptamolybdate tetrahydrate, stir to dissolve, and then subject the slurry to ultrasonic dispersion at 40 kHz for 60 min to prepare the target product.

[0034] Example 3

[0035] The method steps for preparing the catalytic slurry proposed by the present invention are as follows:

[0036] S1: Add 35g of oxalic acid to 435g of aqueous solution, then add 333.6g of butyl titanate to the stirred oxalic acid aqueous solution to form an organic titanium precursor solution; then add 66g of organic silane, and perform high-speed dispersion for 30min at a dispersion speed of 800r / min to form a titanium-silicon composite sol; wherein the organic silane is a mixture of methyltriisopropenyloxysilane and diphenyldimethoxysilane in a mass ratio of 1:1.

[0037] S2: Add 16 g of P40 dispersant and 10 g of polysiloxane to the prepared titanium-silicon composite sol, then add 162 g of vanadyl oxalate pentahydrate and 38 g of ammonium heptamolybdate tetrahydrate, stir and dissolve, then subject the slurry to ultrasonic dispersion at 40 kHz for 60 min to prepare the target product.

[0038] Comparative Example 1

[0039] The method steps for preparing the catalytic slurry proposed by the present invention are as follows:

[0040] S1: Add 67g of ammonium metavanadate and 174g of ammonium heptamolybdate tetrahydrate into 800g of pure water and heat to dissolve, then add 67g of titanium dioxide, continue heating and stirring to evaporate, and control the heating temperature at 90°C until the solution becomes viscous and cannot be stirred. Then dry it at 105°C overnight, take out the sample, calcine it at 500°C in an oxygen atmosphere for 4h, and then crush it to prepare a catalyst powder with the same proportion of active components as in Case 1.

[0041] S2: Take 87g of catalyst powder and add it into 413g of water, stir and disperse it, adjust the pH to below 2 with nitric acid, then add 7g of dispersant and 4.35g of polysiloxane, add it into a grinder and grind it until D50 is less than 100nm to obtain catalytic slurry, then add 488g of water to dilute it, apply it on a small filter tube in a 1:1 ratio, dry it at 105℃ for 8h, activate it at 350℃ for 2h, and finally test the sample.

[0042] Comparative Example 2

[0043] Dissolve 70.3g of vanadium oxalate pentahydrate and 16g of ammonium heptamolybdate tetrahydrate in 865g of water, take 47.8g of commercial nano titanium dioxide with a particle size of 0-100nm and stir and disperse it in the solution, add 7g of P40 dispersant and 4.35g of polysiloxane, and perform ultrasonic dispersion at 40KHz for 60min to prepare the target slurry. Apply it on a small filter tube in a ratio of 1:1, dry it at 105℃ for 8h, activate it at 350℃ for 2h, and finally test the sample.

[0044] Comparative Example 3

[0045] The organosilane in this solution is methyltriisopropyleneoxysilane, and the other conditions are the same as those in Example 1.

[0046] Comparative Example 4

[0047] The organosilane in this solution is diphenyldimethoxysilane, and the other conditions are the same as those in Example 1.

[0048] The performance of the ceramic fiber filter tubes of Example 1 and Comparative Examples 1-4 was tested, and the results are shown in Table 1.

[0049] in:

[0050] The catalytic slurry bonding strength test method is: after ultrasonic vibration of the calcined activated coated filter tube, the ratio before and after the coating falls off is: W = (M0-M1) / M0*100%, M0 is the weight before ultrasound, M1 is the weight after ultrasound, the ultrasonic frequency is 40KHz, and the ultrasonic time is 30min.

[0051] The denitrification rate test method is: punch a hole in the ceramic fiber filter tube and take a sample with a diameter of 30mm for denitrification test, and control the concentration of each gas (vol%) through a mass flow meter: NO: 500ppm, NH3: 500ppm, O2: 5%, H2O: 10%, N2 as the balance gas, and the filtration wind speed is 1m / min. The denitrification rate calculation formula is η=(C1-C2) / C1×100%, where C1 is NO x The inlet concentration of C2 is NO x The outlet concentration is obtained by flue gas analysis test.

[0052] The filter tube resistance test method is: connect the air inlet and outlet of the denitrification device reactor to a differential pressure transmitter, detect the resistance pressure difference caused by the filter tube under the test conditions, and compare the relative pressure difference between the samples.

[0053] The test conditions for water resistance are: changing the H2O content to 20% and 30% at 220°C, and testing the denitrification rate of the ceramic fiber filter tube;

[0054] The test conditions for sulfur resistance are: continuously introducing 100 ppm of SO2 at 250°C, and measuring the denitrification rate of the ceramic fiber filter tube after 24 hours and 168 hours.

[0055] Table 1 Ceramic fiber filter tube performance test results

[0056]

[0057]

[0058] It can be seen from the test results in Table 1 that the catalytic slurry of the present invention has high bonding strength with the filter tube, is not easy to fall off, and has good denitration, sulfur resistance and water resistance. It can be seen from the test results of Example 1 and Comparative Example 1 and Comparative Example 2 that the present invention implants the catalyst by introducing a soluble active component into the titanium-silicon composite sol. During high-temperature activation, bonding occurs between the organic titanium source, the active component and the organic silane, and a catalyst-titanium-silicon composite can be directly generated in situ on the surface of the filter tube fiber. The denitration catalyst is more evenly distributed, and the pressure difference is smaller after the catalytic filter tube is implanted with the catalyst. Compared with directly introducing titanium dioxide , active components, this method can make the active ingredients more evenly and tightly combined with titanium silicon to form an integrated complex, thereby improving the reaction activity of the catalyst; at the same time, due to the low surface energy, water molecules can be prevented from being adsorbed on the catalyst surface, thereby improving the water resistance and stability of the catalyst; from the test results of Example 1 and Comparative Example 3 and Comparative Example 4, it can be seen that the organosilane of the present invention is composed of methyltriisopropenyloxysilane and diphenyldimethoxysilane, and has a synergistic promoting effect on improving the reaction activity, water resistance and sulfur resistance of the ceramic fiber filter tube, thereby significantly improving the performance of the prepared ceramic fiber filter tube.

Claims

1. A method for preparing a catalytic slurry for an anti-shedding and water-resistant ceramic fiber filter tube, characterized in that: The steps are as follows: S1: dissolving butyl titanate in an oxalic acid aqueous solution to form an organic titanium precursor solution; S2: adding organosilane to the organotitanium precursor solution of S1 to prepare a titanium-silicon composite sol; S3: adding a dispersant and a penetrant to the titanium-silicon composite sol of S2, and then adding vanadyl oxalate pentahydrate and ammonium heptamolybdate tetrahydrate, stirring and dissolving, and obtaining a catalytic slurry after ultrasonic dispersion; The organic silane is prepared by mixing methyl triisopropenyloxysilane and diphenyl dimethoxysilane in a mass ratio of 5:1-25.

2. The method for preparing the catalytic slurry for the anti-shedding and water-resistant ceramic fiber filter tube according to claim 1, characterized in that: The mass ratio of butyl titanate, organic silane, dispersant, penetrant, vanadyl oxalate pentahydrate and ammonium heptamolybdate tetrahydrate is 100:15-20:3-5:1-3:30-50:8-12.

3. The method for preparing the catalytic slurry for the anti-shedding and water-resistant ceramic fiber filter tube according to claim 1, characterized in that: The dispersant is a nonionic P40 dispersant, and the penetrant is polysiloxane.

4. The method for preparing the catalytic slurry for the anti-shedding and water-resistant ceramic fiber filter tube according to claim 1, characterized in that: The frequency of ultrasound in S3 is 40 KHz, and the duration of ultrasound is 40-80 min.

5. Catalytic slurry for anti-shedding and water-resistant ceramic fiber filter tube prepared by the method according to any one of claims 1 to 4.

6. Use of the catalytic slurry as claimed in claim 5 on a ceramic fiber filter tube.

7. The use of the catalytic slurry on a ceramic fiber filter tube according to claim 6, characterized in that: The method comprises the following steps: diluting the catalytic slurry and coating it on the inside and outside of the ceramic fiber filter tube, and then performing drying and activation treatment.

8. The use of the catalytic slurry on a ceramic fiber filter tube according to claim 7, characterized in that: The drying temperature is 85-120°C and the drying time is 5-10h.