A smelting method for improving the castability of low-carbon, low-silicon cathode flat steel.
By controlling the converter's final temperature and oxygen activity, combined with RH decarburization and LF refining processes, and employing stepwise slag making and calcium wire feeding, the cleanliness problem of low-carbon and low-silicon cathode flat steel molten steel was solved, enabling continuous casting and stable production, and improving the quality of the cast billet.
Patent Information
- Application Number
- CN202311407049.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-10-26
AI Technical Summary
In the current technology for smelting low-carbon, low-silicon cathode flat steel, it is difficult to guarantee the cleanliness of the molten steel, which leads to subcutaneous bubble defects and nodule flocculation problems in the cast billet, affecting the stability and quality of continuous production.
By controlling the converter's final temperature and oxygen activity, combined with RH decarburization and LF refining processes, and employing stepwise slag making and calcium wire feeding, the oxygen activity and slag phase composition of the molten steel are controlled, and with the aid of argon protection, continuous casting of molten steel is achieved.
It effectively improves the continuous casting capability of low-carbon and low-silicon molten steel, solves the problems of subcutaneous bubble defects and nodule turbulence in the billet, ensures the quality of the billet and the stability of production, and reduces the difficulty of controlling non-metallic inclusions.
Smart Images

Figure CN117431369B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metallurgical technology, and in particular to a smelting method for improving the castability of molten steel for low-carbon, low-silicon cathode flat steel. Background Technology
[0002] Electrolytic aluminum is a high-energy-consuming basic industry in my country's industrial production, with electricity costs dominating, accounting for over 40%. Currently, the average direct energy consumption per ton of aluminum in my country is about 13,000 kWh, while the theoretical direct energy consumption per ton of aluminum is about 6,300 kWh, resulting in an energy utilization rate of about 48%, indicating a huge potential for energy conservation and consumption reduction. Cathode flat steel, as an important component of the cathode in aluminum electrolytic cells, plays a role in evenly distributing current and improving the horizontal current of the molten aluminum. To achieve lower resistivity control of the cathode flat steel, elements with significant resistivity effects, such as carbon and silicon, are often kept at low levels. The process route of converter-RH-LF-continuous casting effectively avoids excessive levels of these elements.
[0003] However, due to limitations in chemical composition, the oxidizing properties of ladle slag after vacuum decarburization are high during production. Aluminum deoxidizers are often used to control the oxygen content in the molten steel. If the slag-forming process in the electric heating stage is improper, the acid-soluble aluminum in the molten steel is easily burned off, calcium treatment is ineffective, and the ladle slag's ability to adsorb non-metallic inclusions is weak, thus compromising the cleanliness of the molten steel. The control of silicon and manganese reversion in the reducing ladle slag should also be considered. Furthermore, when the acid-soluble aluminum content in the molten steel is low, continuous oxygen diffusion into the molten steel can cause subsurface bubble defects in the billet, and surface cracks appear on the cathode flat steel after rolling, rendering it unusable. When the acid-soluble aluminum content is high, after the CCM continuous casting machine starts casting, Al2O3 inclusions formed by the burning off of acid-soluble aluminum continuously accumulate at the long nozzle, causing nodule formation, turbulence, or even casting interruption, failing to meet the requirements for billet quality control and continuous production.
[0004] Therefore, when using the RH+LF process for refining, controlling the composition of ladle slag and the acid-soluble aluminum content in molten steel is key to improving the cleanliness of molten steel and ensuring continuous casting capability.
[0005] In view of this, improvements should be made to the existing technology. Summary of the Invention
[0006] The main objective of this invention is to provide a smelting method for improving the castability of molten steel for low-carbon and low-silicon cathode flat steel. By controlling the oxygen activity of molten steel during the converter-RH-LF-continuous casting process and formulating and implementing the LF slag-forming process, the continuous casting capability of molten steel is effectively improved, and the problems of subsurface bubble defects and nodule turbulence in the billet are solved, achieving continuous and stable production.
[0007] According to one aspect of the present invention, a smelting method for improving the castability of molten low-carbon, low-silicon cathode flat steel is provided, comprising the following steps:
[0008] S1, BOF smelting: control the converter end temperature to 1640℃~1680℃, α[O] range to 500ppm~600ppm, slag blocking during steel tapping, and manganese alloying.
[0009] S2, shallow deoxidation on small platform: add aluminum wire for shallow deoxidation according to the oxygen activity at the end of the converter, control the range of α[O] to 400ppm~500ppm, argon blowing throughout the process, and control the outlet temperature to 1600℃~1640℃.
[0010] S3, RH decarbonization: Control the C content at the outlet to 0.01% to 0.02%, remove the remaining oxygen by adding aluminum pellets, homogenize after deoxidation, and control the Al content to 0.04% to 0.06% by mass percentage. Add the first calcium-containing line 600m to 800m for the first time at the outlet.
[0011] S4, LF refining: Add 3.0-4.0 kg / (t·Fe) steel refining slag conditioner, 4.0-5.0 kg / (t·Fe) high basicity refining slag, and sprinkle 40-80 kg of aluminum shot on the slag surface. Heat the slag for ≥10 min, measure the temperature and take a slag sample. Then, according to the oxidizing properties of the slag, add 3.0-4.5 kg / (t·Fe) high basicity refining slag and 10-30 kg of aluminum shot. According to the fluidity of the steel slag, add 0-1.0 kg / (t·Fe) fluorite slag conditioner to create white slag. Add the second calcium-containing line according to the Al content.
[0012] S5. Large billet continuous casting: 360mm×450mm cross-section continuous casting is adopted. The tundish is purged with argon before pouring and the long nozzle is protected with argon.
[0013] According to one embodiment of the present invention, in step S1, 3.5 to 4.2 kg / (t·Fe) of active lime is added to the ladle during the tapping process.
[0014] According to one embodiment of the present invention, the steel refining slag conditioner comprises the following components by mass percentage: 15.0% ≤ CaO ≤ 30.0%, 45.0% ≤ Al2O3 ≤ 60.0%, 6.0% ≤ MAl ≤ 10.0%, and SiO2 ≤ 6.0%, with a product particle size ≤ 8 mm, wherein the content of the product with a particle size ≤ 5 mm is > 90%.
[0015] According to one embodiment of the present invention, the high-alkalinity refining slag comprises the following components by mass percentage: CaO ≥ 70%, Al2O3 ≤ 5.0%, SiO2 ≤ 5.0%, and product particle size ≤ 15 mm, wherein the product with a particle size < 3 mm ≤ 10%.
[0016] According to an embodiment of the present invention, in step S3, the first calcium-containing wire is an iron-calcium wire.
[0017] According to one embodiment of the present invention, in step S4, 400-600 μm of a second calcium-containing wire is added according to the Al content, wherein the second calcium-containing wire is a silicon-calcium wire.
[0018] According to one embodiment of the present invention, in step S4, the content of Als is controlled to be 0.020-0.035%, the content of Si at the outlet is controlled to be 0.03%-0.06%, and the outlet temperature is controlled to be 1595℃-1605℃.
[0019] According to one embodiment of the present invention, step S5 further includes controlling the overheating of the tundish at 20-40°C and the stretching speed at 0.40-0.50 m / min.
[0020] According to one embodiment of the present invention, step S4 further includes determining the degree of oxidation of the slag based on its color.
[0021] According to one embodiment of the present invention, in step S3, the homogenization time after deoxygenation is ≥3 min.
[0022] According to an embodiment of the present invention, a smelting method for improving the castability of low-carbon and low-silicon cathode flat steel includes the following process flow: BOF smelting—small platform shallow deoxidation—RH decarburization—LF refining—large billet continuous casting. The present invention effectively improves the continuous casting capability and billet quality of low-carbon and low-silicon molten steel by controlling the oxygen activity of molten steel and formulating and practicing the LF slag-forming process. The problems of subcutaneous bubble defects and nodule turbulence in the billet are solved. Attached Figure Description
[0023] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some implementation examples of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0024] Figure 1 A process flow diagram of a smelting method for improving the castability of molten steel for low-carbon, low-silicon cathode flat steel according to the present invention is shown. Detailed Implementation
[0025] To make the objectives, technical solutions, and advantages of the present invention clearer, the embodiments of the present invention will be further described in detail below with reference to specific examples and the accompanying drawings.
[0026] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," and "counterclockwise," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.
[0027] like Figure 1 As shown, the present invention provides a smelting method for improving the castability of low-carbon, low-silicon cathode flat steel, which includes the following steps:
[0028] S1, BOF smelting: control the converter end temperature to 1640℃~1680℃, α[O] range to 500ppm~600ppm, slag blocking during steel tapping, and manganese alloying.
[0029] S2, shallow deoxidation on small platform: add aluminum wire for shallow deoxidation according to the oxygen activity at the end of the converter, control the range of α[O] to 400ppm~500ppm, argon blowing throughout the process, and control the outlet temperature to 1600℃~1640℃.
[0030] S3, RH decarbonization: By mass percentage, control the C content at the outlet to be 0.01% to 0.02%, remove the remaining oxygen by adding aluminum pellets, homogenize after deoxidation, control the Al content to be 0.04% to 0.06%, and add the first calcium-containing line 600m to 800m at the outlet for the first time;
[0031] S4, LF refining: Add 3.0-4.0 kg / (t·Fe) steel refining slag conditioner, 4.0-5.0 kg / (t·Fe) high basicity refining slag, and sprinkle 40-80 kg of aluminum shot on the slag surface. Heat the slag for ≥10 min, measure the temperature and take a slag sample. Then, according to the oxidizing properties of the slag, add 3.0-4.5 kg / (t·Fe) high basicity refining slag and 10-30 kg of aluminum shot. According to the fluidity of the steel slag, add 0-1.0 kg / (t·Fe) fluorite slag conditioner to create white slag. Add the second calcium-containing line according to the Al content.
[0032] S5. Large billet continuous casting: 360mm×450mm cross-section continuous casting is adopted. The tundish is purged with argon before pouring and the long nozzle is protected with argon.
[0033] In the smelting method for improving the castability of low-carbon and low-silicon cathode flat steel according to an embodiment of the present invention, the continuous casting capacity and billet quality of low-carbon and low-silicon molten steel are effectively improved by controlling the oxygen activity of molten steel and formulating and practicing the LF slag-forming process. The problems of subcutaneous bubble defects and nodule turbulence in the billet are solved.
[0034] The production process of this invention is as follows: BOF smelting—small platform shallow deoxidation—RH decarburization—LF refining—large billet continuous casting, wherein:
[0035] In step S1, during the tapping process, 3.5 to 4.2 kg / (t·Fe) of active lime is added to the ladle to protect the molten steel.
[0036] The steel refining slag conditioner comprises the following components by mass percentage: 15.0% ≤ CaO ≤ 30.0%, 45.0% ≤ Al2O3 ≤ 60.0%, 6.0% ≤ MAl ≤ 10.0%, and SiO2 ≤ 6.0%, with a product particle size ≤ 8 mm, of which the content of the product with a particle size ≤ 5 mm is > 90%.
[0037] By mass percentage, the high-alkalinity refining slag comprises the following components: CaO ≥ 70%, Al2O3 ≤ 5.0%, SiO2 ≤ 5.0%, and product particle size ≤ 15 mm, of which product with particle size < 3 mm ≤ 10%.
[0038] In step S3, the [C]-[O] balance condition under vacuum is used to control the C output from the station to be 0.01% to 0.02%.
[0039] In step S3, the first calcium-containing wire is an iron-calcium wire.
[0040] In step S4, 400-600 μm of a second calcium-containing wire is added according to the Al content. The second calcium-containing wire is a silicon-calcium wire.
[0041] In step S4, the content of Als is controlled to be 0.020-0.035%, the content of Si at the outlet is controlled to be 0.03%-0.06%, and the outlet temperature is controlled to be 1595℃-1605℃.
[0042] Step S5 also includes controlling the overheating of the tundish at 20-40°C and the pulling speed at 0.40-0.50 m / min.
[0043] Step S4 also includes determining the degree of oxidation of the slag based on its color.
[0044] Specifically, the LF refining process involves slag adhesion operation, and the following operations are performed according to the color of the slag: (1) When the slag is black: add high-basicity refining slag and aluminum shot; (2) When the slag is light blackish-yellow: add a small amount of high-basicity refining slag and aluminum shot; (3) When the slag is white or milky white, deoxidation is complete.
[0045] The argon gas protection at the long nozzle can effectively prevent secondary oxidation of the molten steel.
[0046] In step S3, the homogenization time after deoxygenation is ≥3 min.
[0047] After implementing the technical solution of this invention, the castability of molten steel is improved, the number of consecutive castings is 8-10, the liquid level is stable during the process, no nodule formation or turbulence occurs, no subcutaneous bubble defects are observed in the billet, and non-metallic inclusions are well controlled, creating great economic benefits. It can be applied and promoted in the production of low-carbon and low-silicon cathode flat steel products or as a raw material for special steel products, and has good prospects for promotion and application.
[0048] The chemical composition (mass percentage) of the cathode flat steel is composed of the following elements: C 0.02%~0.04%, Si 0.03%~0.06%, Mn 0.28%~0.40%, P≤0.015%, S≤0.008%, Als 0.010%~0.020%, O≤28ppm, N≤60ppm, with the remainder being Fe and other unavoidable impurities.
[0049] Analysis of the ladle slag composition after the two slag-forming processes revealed the following: after the first slag-forming process, the ladle slag mainly consisted of CaO = 42%–51%, Al2O3 = 27%–37%, FeO+MnO = 3%–7%, MgO = 6%–8%, SiO2 = 4%–7%, and CaF = 3%–7%. The slag color observed during the process was light blackish-yellow. After the second slag-forming process, the main components of the ladle slag were: CaO = 51%–55%, Al2O3 = 32%–38%, FeO+MnO = 0.8%–1.7%, MgO = 5%–7%, SiO2 = 3%–5%, and CaF = 1%–2%. The oxidizing power of the ladle slag decreased, and the ladle slag exhibited high basicity and low melting point properties. The color of the ladle slag was milky white.
[0050] The non-metallic inclusions were inspected and statistically analyzed. The non-metallic inclusion grades of the cast billets were: Class A 0-0.5, Class B 0-1.5, Class C 0, Class D 0.5-1.0, and Class DS 0.5-1.5. The non-metallic inclusions were well controlled.
[0051] The following specific embodiments illustrate this solution.
[0052] Example 1
[0053] A company uses the technology of this invention to prepare a 360mm×450mm cross-section low carbon and low silicon steel billet, grade SAE1006. Its production process is as follows: BOF smelting—small platform shallow deoxidation—RH decarburization—LF refining—large billet continuous casting.
[0054] BOF smelting: The converter end temperature is controlled at 1640℃, α[O] = 500ppm, slag is blocked during tapping, and manganese is alloyed in this process. During tapping, 3.5kg / (t·Fe) of active lime is added to the ladle to protect the molten steel.
[0055] Small platform shallow deoxidation: Add aluminum wire for shallow deoxidation according to the oxygen activity at the converter endpoint, control α[O] = 400ppm, argon blowing throughout the process, and control the outlet temperature at 1600℃.
[0056] RH decarbonization: C at the outlet is 0.01%, and the remaining oxygen is removed by adding aluminum pellets. After deoxidation, the homogenization time is 6 minutes, and the Al content is controlled at 0.06%. 600m of iron-calcium line is added for the first time at the outlet.
[0057] LF refining: Slag formation is carried out in two large-volume steps. The first step involves adding 3.0 kg / (t·Fe) of steel refining slag conditioner, 5.0 kg / (t·Fe) of high-basicity refining slag, and 40 kg of aluminum shot sprinkled onto the slag surface. After heating and slag formation for 10 minutes, temperature is measured and slag samples are taken. The second slag formation involves adding 4.5 kg / (t·Fe) of high-basicity refining slag and 20 kg of aluminum shot, along with 0.5 kg / (t·Fe) of fluorite for slag conditioning, resulting in white slag. The outlet Als is 0.020%. 400 m of silicon-calcium wire is added, resulting in an outlet Si of 0.03% and an outlet temperature of 1595℃.
[0058] Large billet continuous casting: 360mm×450mm cross section continuous casting is adopted. Before pouring, the tundish is purged with argon gas and the long nozzle is protected with argon gas to prevent secondary oxidation of molten steel. The superheat of the tundish is controlled at 20℃ and the casting speed is 0.40m / min.
[0059] After the ladle was opened for casting, the above method was used continuously, and the number of consecutive heats cast in a single ladle was 9. The liquid level was stable during the process, no nodules or turbulence occurred, no subcutaneous bubble defects were found in the billet, and the non-metallic inclusions were well controlled.
[0060] The final slag from the ladle was milky white in color, with the following composition: CaO = 51%, Al₂O₃ = 35%, FeO + MnO = 0.8%, MgO = 7%, SiO₂ = 5%, CaF = 1%, and other components were not tested. The longitudinal non-metallic inclusions at the diagonal 1 / 4 mark of the cast billet were graded as follows: Class A 0, Class B 0.5, Class C 0, Class D 0.5, and Class DS 0.5, indicating good control of non-metallic inclusions.
[0061] Example 2
[0062] A company uses the technology of this invention to prepare a 360mm×450mm cross-section low carbon and low silicon steel billet, grade SAE1006. Its production process is as follows: BOF smelting—small platform shallow deoxidation—RH decarburization—LF refining—large billet continuous casting.
[0063] BOF smelting: The converter end temperature is controlled at 1680℃, α[O] = 600ppm, slag is blocked during tapping, and manganese is alloyed in this process. During tapping, 4.2kg / (t·Fe) of active lime is added to the ladle to protect the molten steel.
[0064] Small platform shallow deoxidation: Add aluminum wire for shallow deoxidation according to the oxygen activity at the converter endpoint, control α[O] = 450ppm, argon blowing throughout the process, and control the outlet temperature at 1640℃.
[0065] RH decarbonization: C at the outlet is 0.02%, and the remaining oxygen is removed by adding aluminum pellets. After deoxidation, the homogenization time is 3 minutes, and the Al content is controlled at 0.04%. 800m of iron-calcium line is added for the first time at the outlet.
[0066] LF refining: Slag formation is carried out in two large-volume steps. The first step involves adding 4.0 kg / (t·Fe) of steel refining slag conditioner, 4.0 kg / (t·Fe) of high-basicity refining slag, and 80 kg of aluminum shot sprinkled onto the slag surface. After heating and slag formation for 10 minutes, temperature is measured and slag samples are taken. The second slag formation involves adding 4.5 kg / (t·Fe) of high-basicity refining slag and 30 kg of aluminum shot, along with 1.0 kg / (t·Fe) of fluorite for slag conditioning, resulting in white slag. The outlet Als is 0.035%. 600 m of silicon-calcium wire is added, resulting in an outlet Si of 0.06% and an outlet temperature of 1605℃.
[0067] Large billet continuous casting: 360mm×450mm cross section continuous casting is adopted. Before pouring, the tundish is purged with argon gas and the long nozzle is protected with argon gas to prevent secondary oxidation of molten steel. The superheat of the tundish is controlled at 40℃ and the casting speed is 0.45m / min.
[0068] After the ladle was opened for casting, the above method was used continuously, and the number of consecutive heats cast in a single ladle was 9. The liquid level was stable during the process, no nodules or turbulence occurred, no subcutaneous bubble defects were found in the billet, and the non-metallic inclusions were well controlled.
[0069] The final slag from the ladle was milky white in color, with the following composition: CaO = 53%, Al₂O₃ = 32%, FeO + MnO = 1.7%, MgO = 7%, SiO₂ = 4%, CaF = 1%, and other components were not tested. The longitudinal non-metallic inclusions at the diagonal 1 / 4 mark of the billet were graded as follows: A: 0.5, B: 1.0, C: 0, D: 1.0, and DS: 1.5, indicating good control of non-metallic inclusions.
[0070] Example 3
[0071] A company uses the technology of this invention to prepare a 360mm×450mm cross-section low carbon and low silicon steel billet, grade SAE1006. Its production process is as follows: BOF smelting—small platform shallow deoxidation—RH decarburization—LF refining—large billet continuous casting.
[0072] BOF smelting: The converter end temperature is controlled at 1660℃, α[O] = 560ppm, slag is blocked during tapping, and manganese is alloyed in this process. During tapping, 3.8kg / (t·Fe) of active lime is added to the ladle to protect the molten steel.
[0073] Small platform shallow deoxidation: Add aluminum wire for shallow deoxidation according to the oxygen activity at the converter endpoint, control α[O] = 500ppm, purge argon throughout the process, and control the outlet temperature at 1610℃.
[0074] RH decarbonization: C at the outlet is 0.01%, and the remaining oxygen is removed by adding aluminum pellets. After deoxidation, the homogenization time is 4 minutes, and the Al content is controlled at 0.05%. 700m of iron-calcium line is added for the first time at the outlet.
[0075] LF refining: Slag formation is carried out in two large-volume steps. The first step involves adding 3.5 kg / (t·Fe) of steel refining slag conditioner, 4.5 kg / (t·Fe) of high-basicity refining slag, and 60 kg of aluminum shot to the slag surface. After heating and slag formation for 10 minutes, temperature is measured and slag samples are taken. The second slag formation involves adding 3.0 kg / (t·Fe) of high-basicity refining slag and 30 kg of aluminum shot, along with 1.0 kg / (t·Fe) of fluorite for slag conditioning, resulting in white slag. The outlet Als is 0.030%. 550 m of silicon-calcium wire is added, resulting in an outlet Si of 0.05% and an outlet temperature of 1602℃.
[0076] Large billet continuous casting: 360mm×450mm cross section continuous casting is adopted. Before pouring, the tundish is purged with argon gas and the long nozzle is protected with argon gas to prevent secondary oxidation of the molten steel. The superheat of the tundish is controlled at 20℃ and the casting speed is 0.50m / min.
[0077] The final slag from the ladle was milky white in color, with the following composition: CaO = 52%, Al₂O₃ = 38%, FeO + MnO = 1.0%, MgO = 7%, SiO₂ = 3%, CaF = 2%, and other components were not tested. The longitudinal non-metallic inclusions at the diagonal 1 / 4 of the billet were graded as follows: A (Grade 0), B (Grade 1.5), C (Grade 0), D (Grade 0.5), and DS (Grade 1.0), indicating good control of non-metallic inclusions.
[0078] Example 4
[0079] A company uses the technology of this invention to prepare a 360mm×450mm cross-section low carbon and low silicon steel billet, grade SAE1006. Its production process is as follows: BOF smelting—small platform shallow deoxidation—RH decarburization—LF refining—large billet continuous casting.
[0080] BOF smelting: The converter end temperature is controlled at 1670℃, α[O]=569ppm, slag is blocked during tapping, and manganese is alloyed in this process. During tapping, 4.0kg / (t·Fe) of active lime is added to the ladle to protect the molten steel.
[0081] Small platform shallow deoxidation: Add aluminum wire for shallow deoxidation according to the oxygen activity at the converter endpoint, control α[O] = 480ppm, argon blowing throughout the process, and control the outlet temperature at 1625℃.
[0082] RH decarbonization: C at the outlet is 0.02%, and the remaining oxygen is removed by adding aluminum pellets. After deoxidation, the homogenization time is 5 minutes, and the Al content is controlled at 0.06%. 800m of iron-calcium line is added for the first time at the outlet.
[0083] LF refining: Slag formation is carried out in two large-volume steps. The first step involves adding 3.2 kg / (t·Fe) of steel refining slag conditioner, 5.0 kg / (t·Fe) of high-basicity refining slag, and 50 kg of aluminum shot sprinkled onto the slag surface. After heating and slag formation for 10 minutes, temperature is measured and slag samples are taken. The second slag formation involves adding 4.0 kg / (t·Fe) of high-basicity refining slag and 30 kg of aluminum shot, without adding fluorite, resulting in white slag. The outlet Als is 0.025%. Adding 500 m of silicon-calcium wire results in an outlet Si of 0.04% and an outlet temperature of 1598℃.
[0084] Large billet continuous casting: 360mm×450mm cross section continuous casting is adopted. Before pouring, the tundish is purged with argon gas and the long nozzle is protected with argon gas to prevent secondary oxidation of the molten steel. The superheat of the tundish is controlled at 30℃ and the casting speed is 0.45m / min.
[0085] The final slag from the ladle was milky white in color, with the following composition: CaO = 55%, Al₂O₃ = 32%, FeO + MnO = 1.4%, MgO = 5%, SiO₂ = 5%, CaF = 1%, and other components were not tested. The longitudinal non-metallic inclusions at the diagonal 1 / 4 mark of the billet were graded as follows: A: Grade 0, B: Grade 0, C: Grade 0, D: Grade 0.5, DS: Grade 1.0, indicating good control of non-metallic inclusions.
[0086] This invention proposes a smelting method for improving the castability of molten steel in low-carbon, low-silicon cathode flat steel, which has at least the following beneficial effects after implementation:
[0087] (1) The converter avoids excessively high steel temperature and oxygen activity fluctuations caused by deep blowing, and also avoids damage to the furnace body caused by slag splashing.
[0088] (2) The shallow deoxidation of the small platform ensures the smooth progress of vacuum decarburization on the one hand, and reduces the oxygen activity of the molten steel on the other hand, thus reducing the difficulty of controlling the oxygen activity of the molten steel in subsequent processes.
[0089] (3) Although the calcium wire fed into the RH process has a poor effect on the denaturation of inclusions, it reduces the oxidizing properties of ladle slag to a certain extent as a deoxidizer, which is beneficial to the stable control of LF white slag and Al content.
[0090] (4) The LF process implemented a step-by-step large-volume white slag production operation. The distributed white slag production effectively ensured the quality of the white slag, effectively reduced the oxidizing properties of the ladle slag, and facilitated the coordination of uncertain factors during on-site operations. The inclusions were treated with modified calcium again. Through weak argon blowing, the flotation and adsorption of non-metallic inclusions were improved, the cleanliness of the molten steel was improved, and the pourability of the molten steel was effectively guaranteed. The large-volume slag refining effectively prevented the high-oxidizing ladle slag from returning to silicon and manganese, mainly preventing silicon return and improving the hit rate of chemical composition.
[0091] (5) Continuous casting adopts protective casting, which reduces the amount of acid-soluble aluminum loss and realizes the continuous production of low carbon and low silicon steel billets.
[0092] The above are exemplary embodiments disclosed in this invention. The order of the disclosed embodiments is merely for descriptive purposes and does not represent the superiority or inferiority of the embodiments. However, it should be noted that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the disclosed embodiments of this invention (including the claims) is limited to these examples. Various changes and modifications can be made without departing from the scope defined by the claims. The functions, steps, and / or actions of the methods according to the disclosed embodiments described herein do not need to be performed in any particular order. Furthermore, although the elements disclosed in the embodiments of this invention may be described or claimed individually, they may be understood as multiple unless explicitly limited to a singular.
[0093] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention (including the claims) is limited to these examples. Within the framework of the invention, technical features of the above embodiments or different embodiments can be combined, and many other variations of the different aspects of the invention as described above exist, which are not provided in the details for the sake of brevity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the invention should be included within the protection scope of the invention.
Claims
1. A smelting method for improving the castability of molten steel in low-carbon, low-silicon cathode flat steel, characterized in that, It includes the following steps: S1, BOF smelting: control the converter end temperature to 1640℃~1680℃, α[O] range to 500ppm~600ppm, slag blocking during steel tapping, and manganese alloying. S2, shallow deoxidation on small platform: add aluminum wire for shallow deoxidation according to the oxygen activity at the end of the converter, control the range of α[O] to 400ppm~500ppm, argon blowing throughout the process, and control the outlet temperature to 1600℃~1640℃. S3, RH decarbonization: By mass percentage, control the C content at the outlet to be 0.01%~0.02%, remove the remaining oxygen by adding aluminum pellets, homogenize after deoxidation, control the Al content to be 0.04%~0.06%, and add the first calcium-containing line 600m~800m for the first time at the outlet; S4, LF refining: Add 3.0~4.0 kg / (t•Fe) steel refining slag conditioner, 4.0~5.0 kg / (t•Fe) high basicity refining slag, and sprinkle 40-80 kg of aluminum shot on the slag surface. Heat the slag for ≥10 min, measure the temperature and take a slag sample. Then, according to the oxidizing properties of the slag, add 3.0~4.5 kg / (t•Fe) high basicity refining slag and 10~30 kg of aluminum shot. According to the fluidity of the steel slag, add 0~1.0 kg / (t•Fe) fluorite slag conditioner to create white slag. Add the second calcium-containing line according to the Al content. S5. Large billet continuous casting: 360mm×450mm cross section continuous casting is adopted. The tundish is purged with argon before pouring and the long nozzle is protected with argon. In step S3, the first calcium-containing wire is an iron-calcium wire; In step S4, 400-600 μm of a second calcium-containing wire is added according to the Al content. The second calcium-containing wire is a silicon-calcium wire. In step S4, the content of Als is controlled to be 0.020~0.035%, the content of Si at the outlet is controlled to be 0.03%~0.06%, and the outlet temperature is controlled to be 1595℃~1605℃.
2. The smelting method for improving the castability of low-carbon, low-silicon cathode flat steel according to claim 1, characterized in that, In step S1, 3.5~4.2 kg / (t•Fe) of active lime is added to the ladle during the tapping process.
3. The smelting method for improving the castability of low-carbon, low-silicon cathode flat steel according to claim 1, characterized in that, The steel refining slag conditioner comprises the following components by mass percentage: 15.0%≤CaO≤30.0%, 45.0%≤Al2O3≤60.0%, 6.0%≤MAl≤10.0%, SiO2≤6.0%, with a product particle size ≤8mm, of which the content of the product with a particle size ≤5mm is >90%.
4. The smelting method for improving the castability of low-carbon, low-silicon cathode flat steel according to claim 1, characterized in that, The high-alkalinity refining slag comprises the following components by mass percentage: CaO ≥ 70%, Al2O3 ≤ 5.0%, SiO2 ≤ 5.0%, and product particle size ≤ 15 mm, of which product with particle size < 3 mm ≤ 10%.
5. The smelting method for improving the castability of low-carbon, low-silicon cathode flat steel according to claim 1, characterized in that, Step S5 also includes controlling the overheating of the tundish at 20~40℃ and the pulling speed at 0.40~0.50m / min.
6. The smelting method for improving the castability of low-carbon, low-silicon cathode flat steel according to claim 1, characterized in that, Step S4 also includes determining the degree of oxidation of the slag based on its color.
7. The smelting method for improving the castability of low-carbon, low-silicon cathode flat steel according to claim 1, characterized in that, In step S3, the homogenization time after deoxygenation is ≥3 min.
Citation Information
Patent Citations
Method for manufacturing low-carbon and low-silicon steel
CN103627853A
Ultralow-carbon ultralow-silicon-manganese electrode flat steel as well as production method and application thereof
CN116083780A
Production method of electrode flat steel
CN116445686A