A Low-Cost RH Ultra-Low Carbon Silicon Steel Smelting Method

By controlling the converter tapping conditions and the timing of alloy addition, combined with vacuum level and feeding speed, and adopting a low-cost alloy route, the high cost problem of smelting low-carbon steel and ultra-low-carbon steel in RH refining furnace was solved, and high-quality, low-cost low-carbon silicon steel production was achieved.

CN117467822BActive Publication Date: 2026-11-10INST OF RES OF IRON & STEEL JIANGSU PROVINCE +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311520297.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-15
Publication Date
2026-11-10
Estimated Expiration
2043-11-15

AI Technical Summary

Technical Problem

Existing RH refining furnaces face high alloy costs when smelting low-carbon steel and ultra-low-carbon steel, and there are risks of poor steel cleanliness, excessive carbon content, and impurity element control, making it difficult to achieve high-quality, low-cost production.

Method used

The process route of hot metal desulfurization pretreatment, converter smelting, RH vacuum furnace smelting and continuous casting is adopted. By controlling the converter tapping conditions, making reasonable use of inexpensive alloys, and combining vacuum degree and alloy addition timing, ferrosilicon alloys are added in batches and the charging speed and gas flow rate are controlled to ensure the recovery rate of alloy elements and the cleanliness of molten steel.

Benefits of technology

Significantly reduce alloy costs, improve the cleanliness of molten steel, and achieve the smelting of high-quality low-carbon or ultra-low-carbon steel, reducing alloy costs by 38.9%-20.9%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117467822B_ABST
    Figure CN117467822B_ABST
Patent Text Reader

Abstract

This invention discloses a low-cost RH ultra-low carbon silicon steel smelting method to solve the technical problem of high overall cost of RH low carbon steel or ultra-low carbon steel alloys. The process route is: hot metal desulfurization pretreatment → converter smelting → RH vacuum furnace smelting → continuous casting. During the RH vacuum treatment, ferrosilicon alloy is added in batches according to the product composition. When the target steel grade has Si ≤ 1.0% by mass, ordinary ferrosilicon is used instead of ultra-low carbon low sulfur ferrosilicon; when the target steel grade has Si > 1.0%, low carbon low sulfur ferrosilicon is used instead of ultra-low carbon low sulfur ferrosilicon. While adding the ferrosilicon alloy in batches, the timing and speed of feeding are controlled, and the gas flow rate is increased to remove carbon from the ordinary alloy and reduce the [O] content of the molten steel. This invention significantly reduces alloy costs while increasing the cleanliness of the molten steel and improving the overall competitiveness of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a low-cost RH ultra-low carbon silicon steel smelting method, belonging to the field of iron and steel smelting technology. Background Technology

[0002] In modern metallurgical industrial production, ladle refining technology is one of the most important process methods. Among them, the RH refining furnace has been developed with significant decarburization and degassing effects, and is a process equipment for producing high-quality steel products.

[0003] The RH refining furnace consists of an exhaust system, a charging system, a blowing system, a vacuum tank, a immersion tube, a ladle, and a ladle lifting system. The addition of alloy raw materials into the furnace involves a series of physicochemical phenomena, including oxygen lance blowing, vacuum chamber extraction, molten pool stirring, steel decarburization, and element oxidation, making it a relatively complex process. Therefore, precisely controlling the recovery rate of alloying elements and the removal of impurities in RH refining furnaces presents numerous challenges. Currently, when smelting low-carbon steel and ultra-low-carbon steel (C ≤ 0.0030% by mass percentage), the stringent requirements for C content and impurities such as S and P in steel products necessitate the use of high-grade alloys such as aluminum, manganese, and ultra-low-carbon, low-sulfur ferrosilicon to alloy the molten steel in order to balance steel decarburization efficiency, alloying element recovery, and impurity control. This alloying process is extremely expensive, leading to a significant increase in production costs and causing numerous disadvantages for enterprise development.

[0004] Patent application CN112553410A discloses a silicon deoxidation process for RH-grade steel, using ordinary ferrosilicon as the deoxidizing material. It utilizes the high oxygen content at the converter endpoint to react with the ferrosilicon alloy, reducing the initial oxygen content in the RH process and thus controlling costs. However, this method involves adding ordinary ferrosilicon alloy at the converter tapping stage. On one hand, this generates a large amount of non-metallic inclusions, causing significant pollution to the molten steel. Simultaneously, the large amount of alloy added causes a significant temperature drop in the molten steel, resulting in a low RH inlet temperature. On the other hand, the carbon introduced by ordinary ferrosilicon is unsuitable for ultra-low carbon steel production, and there is also a risk of exceeding the control limits for impurity elements such as sulfur and phosphorus. In summary, this not only leads to a low RH inlet temperature but also results in poor steel cleanliness, excessive carbon content, and exceeding impurity element limits. Therefore, this method is not suitable for ultra-low carbon high-quality steel. There is an urgent need to develop a low-cost smelting process for high-quality low-carbon or ultra-low carbon steels using the RH process. Summary of the Invention

[0005] To address the aforementioned problems, this invention discloses a simple, effective, rationally designed, and highly operable low-cost method for smelting RH ultra-low carbon silicon steel. The specific technical solution is as follows: A low-cost RH ultra-low carbon silicon steel smelting method, the process route is: hot metal desulfurization pretreatment → converter smelting → RH vacuum furnace smelting → continuous casting, the steps are as follows: Step 1: Desulfurization pretreatment of molten iron: Desulfurization pretreatment of molten iron is carried out using a desulfurization station; Step 2: Converter smelting: The pretreated molten iron is smelted by oxygen blowing and slag forming using a top and bottom blowing converter. Step 3: RH vacuum furnace smelting: The molten steel after the converter treatment is completed is hoisted to the RH treatment station, where it undergoes vacuum decarburization and alloying treatment. Step 4: Continuous casting: The molten steel after RH vacuum treatment is cast under full-process protection.

[0006] Furthermore, step 1, the desulfurization pretreatment of molten iron, includes the following steps: (1) Use KR desulfurization station to desulfurize molten iron: After the treatment is completed, the molten iron should meet the following requirements: S≤0.0015% and temperature≥1300℃.

[0007] (2) Slag removal after desulfurization: After slag removal, [slag area] / [molten iron surface area] ≤ 2.0%.

[0008] Furthermore, step 2, converter smelting, includes the following steps: (1) Using a top-and-bottom blown converter to smelt the desulfurized molten iron: using a supersonic oxygen lance to supply oxygen to the molten iron for smelting, in order to achieve decarburization, temperature increase, and oxidation of impurity elements; using lime, dolomite, and iron ore to form slag, in order to achieve desulfurization, dephosphorization, and adsorption of impurities. The final temperature of the converter should be controlled at 1645-1690℃, with a C content of 0.03-0.08% and an O content of 0.03-0.08% by mass percentage; (2) Converter tapping: Slag feeding is strictly prohibited during converter tapping. When the tapping volume is 20%-30%, lime is added at a rate of 1.5kg / t-3.5kg / t. After the converter tapping is completed, low-alumina slag surface deoxidizer is added to modify the slag at a rate of 1.0kg / t-2.0kg / t. Bottom blowing and stirring of the ladle are turned on throughout the tapping process. The bottom blowing flow rate is 1.5NL / (t·min)-4.0NL / (t·min). After stirring for more than 3 minutes, the ladle can be transported to the RH treatment station.

[0009] Furthermore, step 3, RH vacuum furnace smelting, includes the following steps: (1) RH molten steel entering the station with constant oxygen and temperature measurement: molten steel entering the station: temperature ≥1610℃, of which the temperature of the casting furnace should be ≥1615℃; C content is 0.025%-0.075%, O content is 0.025%-0.075%, and T.Fe in slag is ≤15%; (2) RH vacuum treatment: when the pressure of the RH vacuum chamber is ≤100mbar and the O content of the molten steel is ≤0.045% by mass percentage, ferrosilicon alloy is added in batches according to the product composition. The ferrosilicon alloy is ordinary ferrosilicon or low carbon and low sulfur ferrosilicon. When the target steel grade Si is ≤1.0%, ordinary ferrosilicon is used to replace ultra-low carbon and low sulfur ferrosilicon. When the target steel grade Si is >1.0%, low carbon and low sulfur ferrosilicon is used to replace ultra-low carbon and low sulfur ferrosilicon. Ferrosilicon alloy is added in batches: First batch alloy → net circulation → Second batch alloy → net circulation → Third batch alloy → net circulation until decarburization is complete. For the first two batches, 60% of the alloy is added at a rate of 100-300 kg / min, with a boosting gas flow rate of 0.3-0.6 NL·(t·min). During net circulation, the boosting gas flow rate is 1.0-1.3 NL·(t·min). The remaining alloy is added in the third batch, ensuring a net circulation time greater than 5 minutes until decarburization is complete. Specific control parameters for alloy addition are shown in Table 1. Table 1 Control parameters for the addition of ferrosilicon alloy

[0010] The composition of ordinary ferrosilicon, by mass percentage, includes: C: 0.10%-0.20%, Si: 70%-80%, P≤0.025%, S≤0.030%, Al: 1.80%-2.2%, with the remainder being iron and unavoidable impurities; the composition of low-carbon, low-sulfur ferrosilicon, by mass percentage, includes: C: 0.01%-0.03%, Si: 75%-85%, P≤0.020%, S≤0.020%, Al: 0.10%-0.30%, with the remainder being iron and unavoidable impurities. (3) After the steel liquid is decarburized, aluminum and manganese are added in sequence for alloying. During alloying, a special deoxidizer for low carbon steel slag surface is added to the slag surface at a rate of 1.5 kg / t to 2.5 kg / t. Then, a net circulation treatment is carried out, with a net circulation time of ≥6 min. Finally, the steel is discharged through the void, and the T.Fe content in the discharged slag is ≤5%. The aluminum alloy used in the alloying process comprises: Al≥99%, with the remainder being iron and unavoidable impurities; the ultra-low carbon and low sulfur ferrosilicon alloy comprises, by mass percentage: C: 0.007%-0.014%, Si: 80%-90%, P≤0.020%, S≤0.015%, Al: 0.05%-0.10%, with the remainder being iron and unavoidable impurities; the manganese alloy comprises, by mass percentage: Mn≥96%, C: 0.02%-0.08%, P≤0.015%, S≤0.015%, Al≤0.005%, with the remainder being iron and unavoidable impurities.

[0011] Furthermore, step 4, which involves full-process protective casting of the molten steel after RH vacuum treatment, includes casting using a long ladle nozzle and argon seal, tundish covering agent, submerged entry nozzle, and mold protective slag to prevent oxidation of the molten steel and alloy components.

[0012] Furthermore, in the aforementioned low-cost RH ultra-low carbon silicon steel smelting method, the Si content of the smelted steel is 0.80%-3.10% by mass percentage. When the RH steel is tapped, the comprehensive recovery rate of Si element in the silicon alloy is greater than 90%, and the recovery rate of Mn element in the manganese alloy reaches more than 97%.

[0013] The principle of this invention is as follows: Firstly, by controlling the molten iron and converter tapping conditions, the impact of impurities such as sulfur (S) and phosphorus (P) can be minimized, preventing excessive addition of alloying elements that could lead to excessive S and P levels. Excessively low converter tapping temperatures can cause the RH oxygen blowing process to raise the temperature, resulting in increased oxygen content in the molten steel. Simultaneously, excessive oxidation during tapping also directly contributes to high oxygen content in the molten steel. Ultimately, this leads to low alloying element recovery, significant alloy loss, and poor molten steel cleanliness. Therefore, it is essential to control the converter's endpoint, combining this with slag modification to stabilize the RH inlet steel temperature and C / O conditions, ensuring appropriate RH vacuum treatment conditions.

[0014] Secondly, during RH treatment, inexpensive alloys are used to replace expensive high-grade alloys, while reducing the O content in the molten steel and minimizing alloying losses, thereby significantly reducing smelting costs.

[0015] By studying the C, Si, and O balance and reaction mechanism under high vacuum, the timing of adding ferrosilicon alloy was determined. Based on the variation law of vacuum chamber pressure and C content, it was determined that the vacuum degree when adding ferrosilicon alloy should be <100 mbar, and the [O] in molten steel should be <0.045% by mass percentage. At this time, the C in the ferrosilicon alloy can be removed by utilizing the residual [O] in the molten steel. On the one hand, this can directly reduce the impact of C introduced by ordinary alloys on low-carbon steel or ultra-low-carbon steel; on the other hand, it can reduce the residual [O] in the molten steel, thereby comprehensively reducing the loss during subsequent alloying and improving the cleanliness of the molten steel, achieving multiple benefits.

[0016] Meanwhile, to ensure complete removal of carbon introduced from the ferrosilicon alloy, it should be added in batches multiple times, with controlled addition speed and increased gas flow rate. Reducing the gas flow rate during alloy addition weakens the steel circulation, prolonging the time the ferrosilicon alloy remains in the vacuum chamber, ensuring that the carbon introduced by the alloy fully reacts with the residual [O] in the molten steel. Increasing the gas flow rate during net circulation promptly promotes steel displacement in the vacuum chamber, ensuring effective decarburization of subsequent alloys. Since the reaction between the molten steel and the carbon introduced by the alloy reduces residual oxygen in the vacuum chamber, the gas flow rate should be increased immediately after each batch of alloy addition to ensure effective decarburization of the next batch. Therefore, the timing and speed of ferrosilicon alloy addition must be carefully controlled.

[0017] Next, by studying the alloy oxidation sequence, the alloying sequence of aluminum → manganese was determined. When the target steel grade Si ≤ 1.0%, ordinary ferrosilicon was used instead of ultra-low carbon and low sulfur ferrosilicon. When the target steel grade Si > 1.0%, the alloy addition was large, and to prevent incomplete decarburization and excessive S and P impurities, low carbon and low sulfur ferrosilicon was used instead of ultra-low carbon and low sulfur ferrosilicon. After alloying the molten steel, a special slag surface deoxidizer for low carbon steel was added to prevent oxygen transfer from the slag, ensuring a net circulation time of ≥ 8 minutes to remove inclusions such as Al2O3, and finally, the steel was tapped through a vacuum process. Finally, continuous casting with full protection was used to prevent oxidation of the molten steel and alloying elements, ensuring product quality.

[0018] The beneficial effects of this invention are to significantly reduce alloy costs while increasing the cleanliness of molten steel. By replacing expensive high-grade alloys with ordinary alloys, the consumption of high-grade alloys for low-carbon or ultra-low-carbon steel is reduced, significantly lowering smelting costs. By adding ferrosilicon alloys in batches and effectively controlling the timing, speed, and gas flow rate of the addition, carbon is removed from the ordinary alloys, while simultaneously reducing the oxygen content in the molten steel, further reducing alloy consumption and improving the cleanliness of the molten steel. Attached Figure Description

[0019] Figure 1 This is a process flow diagram of the present invention.

[0020] Figure 2 This is a schematic diagram of carbon-silicon-aluminum-oxygen balance under different vacuum levels during the implementation of the technical solution of this invention.

[0021] Figure 3 This is a schematic diagram of local Si enrichment in steel during the implementation of the technical solution of the present invention.

[0022] Figure 4 This is a schematic diagram of silicon being reduced by aluminum during the implementation of the technical solution of the present invention.

[0023] Figure 5This is a schematic diagram showing the percentage content of SiO2 component in the inclusions during the implementation of the technical solution of this invention. Detailed Implementation

[0024] The present invention will be further illustrated below with reference to the accompanying drawings. It should be understood that the following specific embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Example

[0025] Example 1

[0026] A process route for smelting an ultra-low carbon silicon steel is as follows: KR desulfurization pretreatment → 180t top and bottom blowing converter → RH vacuum furnace → slab continuous casting. The RH alloying sequence using this invention is ordinary ferrosilicon → metallic aluminum → metallic manganese. The chemical composition of the finished product, by mass percentage, is: C≤0.0030%, Si: 0.87%-1.02%, Al: 0.23%-0.38%, Mn: 0.15%-0.25%, P≤0.025%, S≤0.0030%. The specific process parameters for a certain heat of smelting according to this invention are as follows: (1) KR desulfurization station pretreatment: The conditions of the molten iron entering the station are S: ≤0.0400% and the temperature of the molten iron is ≥1350℃. After the desulfurization pretreatment is completed, the molten iron has S: 0.0015% and the temperature is 1307℃.

[0027] (2) Converter smelting: The 180t converter is decarburized and dephosphorized by top and bottom blowing. The converter end temperature is 1687℃. The C content is 0.033% and the O content is 0.080% by mass percentage. When the converter output is 40t, 420kg of high-quality lime is added. The bottom blowing flow rate of the ladle during the tapping process is 330NL·min. -1 After tapping, add 300 kg of low-alumina slag surface deoxidizer, stir for 4 minutes, and then transport to RH treatment. (3) RH Vacuum Treatment: The temperature of the molten steel entering the RH station was 1625℃, the C content was 0.031%, the O content was 0.073%, and the T.Fe content in the slag was 15%. Since the amount of ferrosilicon alloy added to this steel grade was relatively small (target Si ≤ 1.0%), ordinary ferrosilicon was used instead of ultra-low carbon and low sulfur ferrosilicon. After the ladle was lifted to the treatment station, vacuuming began. When the vacuum chamber pressure dropped to 100 mbar, the O content of the molten steel was measured to be 0.045%, and a total of 2452 kg of ordinary ferrosilicon was added. The first batch added was 750 kg, and the gas flow rate was increased to 60 NL·min. -1 The feeding rate is 150 kg / min, and the gas flow rate at the end of feeding is set to 180 NL·min. -1 After a net circulation period of 2 minutes, the second batch of material is added; the amount of ordinary ferrosilicon added in the second batch is 750 kg, and the gas flow rate is increased to 70 NL·min. -1The feeding rate is 200 kg / min, and the gas flow rate at the end of feeding is set to 200 NL·min. -1 After a net circulation period of 1.5 minutes, the third batch of material is added; the amount of ordinary ferrosilicon added in the third batch is 952 kg, and the gas flow rate is increased by 80 NL·min. -1 The feeding rate is 300 kg / min, and the gas flow rate at the end of feeding is set to 290 NL·min. -1 After a net circulation of 3 minutes, 795 kg of metallic aluminum and 232 kg of metallic manganese are added sequentially for alloying. During RH alloying, 350 kg of low-carbon steel-specific slag surface deoxidizer is added to the slag surface. After alloying, the slag is circulated for 6 minutes to break the air and tap the steel. The T.Fe content in the RH tapped slag is 5%.

[0028] (4) Continuous casting: The casting process is protected by a long ladle nozzle and argon seal, tundish covering agent, submerged nozzle and mold protective slag.

[0029] The main components of ordinary ferrosilicon used in the RH vacuum furnace, by mass percentage, are: C: 0.12%, Si: 77%, P: 0.024%, S: 0.003%, Al: 1.94%, with the remainder being iron and unavoidable impurities. The price of ordinary ferrosilicon alloy is 8.7 yuan / kg. When this steel is smelted according to the process of this invention, the main chemical composition of the steel tapped from the RH furnace, by mass percentage, is: C: 0.0023%, Si: 0.96%, Al: 0.34%, Mn: 0.19%, P: 0.019%, S: 0.0027%, as well as Fe and other trace elements. The overall recovery rate of Si is 91.6%, the recovery rate of Al is 77.7%, and the recovery rate of Mn is 98.2%. The cost of ordinary ferrosilicon is approximately 118.4 yuan / t, the cost of metallic aluminum is approximately 91.9 yuan / t, and the cost of metallic manganese is approximately 27.7 yuan / t, for a total alloy cost of approximately 238.0 yuan / t.

[0030] Comparative Example 1 The process route for smelting an ultra-low carbon silicon steel is as follows: KR desulfurization pretreatment → 180t top-and-bottom blowing converter → RH vacuum furnace → slab continuous casting. The RH alloying sequence is: aluminum → ultra-low carbon low-sulfur ferrosilicon → manganese. The chemical composition of the finished product, by mass percentage, is: C≤0.0030%, Si: 0.87%-1.02%, Al: 0.23%-0.38%, Mn: 0.15%-0.25%, P≤0.025%, S≤0.0030%. The specific process parameters for a certain heat are as follows: (1) KR desulfurization station pretreatment: The conditions of the molten iron entering the station are S: ≤0.0400% and the temperature of the molten iron is ≥1350℃. After the desulfurization pretreatment is completed, the S of the molten iron is 0.0014% and the temperature is 1305℃.

[0031] (2) Converter smelting: 180t converter top and bottom blowing decarburization and dephosphorization, converter final temperature 1669℃, C content 0.042% and O content 0.059% by mass percentage, ladle bottom blowing flow rate 350NL·min during tapping process. -1 After stirring for 5 minutes, transport to RH treatment; (3) RH vacuum treatment: The temperature of the molten steel entering the RH station was 1612℃, the C content was 0.040%, the O content was 0.056%, and the T.Fe content in the slag was 18%. After the ladle was lifted to the treatment station, vacuuming was started. When the vacuum degree of the vacuum chamber was <1.0mbar, the deep decarburization mode was entered until the decarburization was completed. The oxygen content of the molten steel after decarburization was measured to be 0.035%. Then, 897kg of metallic aluminum, 2366kg of ultra-low carbon and low sulfur ferrosilicon, and 246kg of metallic manganese were added in sequence for alloying. Finally, after a net circulation treatment of 5 minutes, the steel was discharged through the vacuum. The T.Fe content in the RH slag was 7.0%.

[0032] (4) Continuous casting: The casting process is protected by a long ladle nozzle and argon seal, tundish covering agent, submerged nozzle and mold protective slag.

[0033] The ultra-low carbon, low sulfur ferrosilicon used in the RH vacuum furnace has the following composition by mass percentage: C: 0.009%, Si: 81%, P: 0.018%, S: 0.0014%, Al: 0.06%, with the remainder being iron and unavoidable impurities. The price of the ultra-low carbon, low sulfur ferrosilicon alloy is 19.5 yuan / kg. The final RH tapped steel has the following main chemical composition by mass percentage: C: 0.0019%, Si: 1.03%, Al: 0.32%, Mn: 0.20%, P: 0.017%, S: 0.0019%, as well as Fe and other trace elements. The overall Si recovery rate is 96.7%, the Al recovery rate is 64.8%, and the Mn recovery rate is 98.6%. The cost of ultra-low carbon and low sulfur ferrosilicon is approximately RMB 256.3 / t, the cost of metallic aluminum is approximately RMB 103.7 / t, and the cost of metallic manganese is approximately RMB 29.4 / t, for a total alloy cost of approximately RMB 389.4 / t per ton of steel.

[0034] In Example 1, the cost of smelting this steel alloy using the present invention is only 238.0 yuan / t, which saves 151.4 yuan per ton of steel, significantly reducing the alloy cost by 38.9%.

[0035] Example 2

[0036] A high-grade ultra-low carbon silicon steel is smelted using the following process: KR desulfurization pretreatment → 180t top-and-bottom combined blowing converter → RH vacuum furnace → slab continuous casting. The RH alloying sequence using this invention is low-carbon, low-sulfur ferrosilicon → metallic aluminum → metallic manganese. The finished product's chemical composition, by mass percentage, is: C ≤ 0.0025%, Si: 1.85%-2.05%, Al: 0.25%-0.40%, Mn: 0.25%-0.40%, P ≤ 0.020%, S ≤ 0.0030%. The specific process parameters for a particular heat of smelting according to this invention are as follows: (1) KR desulfurization station pretreatment: The conditions of the molten iron entering the station are S: ≤0.0400% and the temperature of the molten iron is ≥1350℃. After the desulfurization pretreatment is completed, the S of the molten iron is 0.0014% and the temperature is 1311℃.

[0037] (2) Converter smelting: 180t converter top and bottom blowing decarburization and dephosphorization, converter final temperature 1669℃, C content 0.039% and O content 0.063% by mass percentage; when the converter tapping rate is 45t, 400kg of high-quality lime is added, and the bottom blowing flow rate of the ladle during the tapping process is 350NL·min -1 After tapping, add 280 kg of low-alumina slag surface deoxidizer, stir for 3 minutes, and then transport to RH treatment. (3) RH vacuum treatment: The temperature of the molten steel entering the RH station was 1612℃, the C content was 0.037%, the O content was 0.061%, and the T.Fe content in the slag was 15%. Due to the large amount of ferrosilicon alloy added to this steel grade (target Si > 1.0%), low-carbon and low-sulfur ferrosilicon was selected to replace ultra-low-carbon and low-sulfur ferrosilicon. After the ladle was lifted to the treatment position, vacuuming began. When the vacuum chamber pressure dropped to 100 mbar, the O content of the molten steel was measured to be 0.043%, and a total of 4923 kg of low-carbon and low-sulfur ferrosilicon was added. The first batch was 1480 kg, and the gas flow rate was increased to 90 NL·min. -1 The feeding rate is 200 kg / min, and the gas flow rate at the end of feeding is set to 200 NL·min. -1 After a net circulation period of 3 minutes, the second batch of material is added; the amount of ordinary ferrosilicon added in the second batch is 1480 kg, and the gas flow rate is increased by 100 NL·min. -1 The feeding rate is 300 kg / min, and the gas flow rate at the end of feeding is set to 230 NL·min. -1 After a net circulation period of 3 minutes, the third batch of material is added; the amount of ordinary ferrosilicon added in the third batch is 1963 kg, and the gas flow rate is increased by 110 NL·min. -1 The feeding rate is 300 kg / min, and the gas flow rate at the end of feeding is set to 320 NL·min. -1After a net circulation of 4 minutes, 867 kg of metallic aluminum and 415 kg of metallic manganese are added sequentially for alloying. During RH alloying, 300 kg of low-carbon steel-specific slag surface deoxidizer is added to the slag surface. After alloying, the slag is circulated for 7 minutes to break the air and tap the steel. The T.Fe content in the RH tapped slag is 5%.

[0038] (4) Continuous casting: The casting process is protected by a long ladle nozzle and argon seal, tundish covering agent, submerged nozzle and mold protective slag.

[0039] The main components of the low-carbon, low-sulfur ferrosilicon used in the RH vacuum furnace, by mass percentage, are: C: 0.014%, Si: 77%, P: 0.017%, S: 0.002%, Al: 0.09%, with the remainder being iron and unavoidable impurities. The price of the low-carbon, low-sulfur ferrosilicon alloy is 13.5 yuan / kg. When this steel is smelted according to the process of this invention, the main chemical components at the RH tapping stage, by mass percentage, are: C: 0.0015%, Si: 1.95%, Al: 0.32%, Mn: 0.29%, P: 0.016%, S: 0.0019%, as well as Fe and other trace elements. The overall recovery rate of Si is 92.6%, the recovery rate of Al is 67.1%, and the recovery rate of Mn is 97.8%. The cost of low-carbon, low-sulfur ferrosilicon is approximately 369.2 yuan / t, the cost of metallic aluminum is approximately 100.2 yuan / t, and the cost of metallic manganese is approximately 49.8 yuan / t, for a total alloy cost of approximately 519.2 yuan / t per ton of steel.

[0040] Comparative Example 2 The process route for smelting a high-grade ultra-low carbon silicon steel is as follows: KR desulfurization pretreatment → 180t top-and-bottom combined blowing converter → RH vacuum furnace → slab continuous casting. The RH alloying sequence is: aluminum → ultra-low carbon low-sulfur ferrosilicon → manganese. The chemical composition of the finished product, by mass percentage, is: C≤0.0025%, Si: 1.85%-2.05%, Al: 0.25%-0.40%, Mn: 0.25%-0.40%, P≤0.020%, S≤0.0030%. The specific process parameters for a certain heat are as follows: (1) KR desulfurization station pretreatment: The conditions of the molten iron entering the station are S: ≤0.0400% and the temperature of the molten iron is ≥1350℃. After the desulfurization pretreatment is completed, the molten iron has S: 0.0015% and the temperature is 1308℃.

[0041] (2) Converter smelting: 180t converter top and bottom blowing decarburization and dephosphorization, converter final temperature 1675℃, C content 0.037% and O content 0.066% by mass percentage, ladle bottom blowing flow rate during tapping is 260NL·min -1 After stirring for 4 minutes, it is transported to RH treatment; (3) RH vacuum treatment: The temperature of the molten steel entering the RH station was 1618℃, the C content was 0.035%, the O content was 0.065%, and the T.Fe content in the slag was 17% by mass percentage. After the ladle was lifted to the treatment station, vacuuming was started. When the vacuum degree of the vacuum chamber was <1.0mbar, the deep decarburization mode was entered until the decarburization was completed. The O content of the molten steel after decarburization was measured to be 0.034%. Then, 956kg of metallic aluminum, 4598kg of ultra-low carbon and low sulfur ferrosilicon, and 398kg of metallic manganese were added in sequence for alloying. Finally, after a net circulation treatment of 8 minutes, the steel was discharged through the vacuum. The T.Fe content in the RH slag was 8.0%.

[0042] (4) Continuous casting: The casting process is protected by a long ladle nozzle and argon seal, tundish covering agent, submerged nozzle and mold protective slag.

[0043] The ultra-low carbon and low sulfur ferrosilicon used in the RH vacuum furnace has the following composition by mass percentage: C: 0.009%, Si: 81%, P: 0.018%, S: 0.002%, Al: 0.06%, with the remainder being iron and unavoidable impurities. The price of the ultra-low carbon and low sulfur ferrosilicon alloy is 19.5 yuan / kg. The final RH tapped steel has the following main chemical composition by mass percentage: C: 0.0014%, Si: 1.99%, Al: 0.32%, Mn: 0.21%, P: 0.015%, S: 0.0017%, as well as Fe and other trace elements. The overall recovery rate of Si is 96.2%, Al is 60.9%, and Mn is 98.8%. The cost of ultra-low carbon and low sulfur ferrosilicon is approximately 498.1 yuan / t, the cost of aluminum is approximately 110.5 yuan / t, and the cost of manganese is approximately 47.5 yuan / t, for a total alloy cost of approximately 656.1 yuan / t.

[0044] In Example 2, the cost of smelting this steel alloy using the present invention is only 519.2 yuan / t, which saves 136.9 yuan per ton of steel, significantly reducing the alloy cost by 20.9%.

[0045] Figure 2The figure shows the carbon-silicon-aluminum-oxygen equilibrium under different vacuum levels. It can be seen that when the vacuum level is <500mbar and C <0.070%, the bonding ability between Si and [O] is stronger than that between C; when the vacuum level is <200mbar and C >0.020%, the bonding ability between C and [O] is stronger than that between Si; when the vacuum level is <100mbar and C >0.003%, the bonding ability between C and [O] is stronger than that between Si. If the ferrosilicon alloy is added too early, the RH vacuum chamber pressure is high (>500 mbar), the molten steel is highly oxidizing ([O]>0.050%), and the binding ability of Si with the residual [O] in the molten steel is stronger than that of C, resulting in a large amount of Si being oxidized and a decrease in element yield. If it is added too late, although the vacuum chamber pressure is low (<1.0 mbar), the high-speed decarburization period of the molten steel has passed, the oxygen content in the steel is low (<0.030%), the carbon-oxygen reaction is weakened, and a large amount of ferrosilicon alloy will cause carbon increase in the molten steel, resulting in incomplete decarburization and ultimately causing the C content to exceed the standard. Therefore, when the vacuum degree is less than 100 mbar, as the vacuum degree continues to decrease, the residual [O] in the molten steel can preferentially react with the C in the ordinary ferrosilicon alloy, thereby achieving the purpose of "decarburization and silicon preservation".

[0046] Figure 3 This is a schematic diagram of localized Si enrichment in steel. Controlling the addition rate and increasing the gas flow rate are to prevent the alloy from accumulating in large quantities, causing Si enrichment, increasing the local Si concentration, and ultimately leading to Si oxidation loss.

[0047] Figure 4 This is a schematic diagram of silicon being reduced by aluminum. Figure 5 This is a schematic diagram illustrating an example of silicon reduction by aluminum. Although the method of adding ferrosilicon alloy has been determined by controlling the vacuum level and residual [O] in the molten steel, due to the structural characteristics of the RH vacuum chamber, the oxidation of Si is inevitable during the addition process. Therefore, during alloying, metallic aluminum is added first. On the one hand, this further deoxidizes and purifies the molten steel; on the other hand, it reduces the previously oxidized Si, such as... Figure 4 as well as Figure 5 As shown, this comprehensively improves the yield of Si.

[0048] The technical means disclosed in this invention are not limited to those disclosed above, but also include technical solutions composed of any combination of the above technical features.

[0049] Based on the above-described preferred embodiments of the present invention, and through the foregoing description, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.

Claims

1. A low-cost RH ultra-low carbon silicon steel smelting method, characterized in that, The process route is: hot metal desulfurization pretreatment → converter smelting → RH vacuum furnace smelting → continuous casting, and the steps are as follows: Step 1: Desulfurization pretreatment of molten iron: Desulfurization pretreatment of molten iron is carried out using a desulfurization station; Step 2: Converter smelting: The pretreated molten iron is smelted by oxygen blowing and slag forming using a top and bottom blowing converter. Step 3: RH vacuum furnace smelting: The molten steel after the converter treatment is completed is hoisted to the RH treatment station, where it undergoes vacuum decarburization and alloying treatment. During the RH vacuum treatment process, ferrosilicon alloy is added in batches according to the product composition. When the target steel grade has Si ≤ 1.0%, ordinary ferrosilicon is used instead of ultra-low carbon and low sulfur ferrosilicon. When the target steel grade has Si > 1.0% by mass percentage, low carbon and low sulfur ferrosilicon is used instead of ultra-low carbon and low sulfur ferrosilicon. While adding ferrosilicon alloy in batches, the timing and speed of feeding are controlled, and the gas flow rate is increased to remove C from the ordinary alloy and reduce the [O] content of the molten steel. Step 4: Continuous casting: Casting the molten steel after RH vacuum treatment under full-process protection; In step 3, RH vacuum treatment is performed. When the pressure of the RH vacuum chamber is ≤100mbar and the O content of the molten steel is ≤0.045% by mass percentage, the ferrosilicon alloy is added in batches: first batch of alloy → net circulation → second batch of alloy → net circulation → third batch of alloy → net circulation until decarburization is completed. 60% of the alloy is added in the first two batches at a rate of 100-300kg / min. The remaining alloy is added in the third batch, ensuring that the net circulation time is greater than 5min until decarburization is completed. When adding the alloy, reduce the boost gas flow rate to 0.3-0.6 NL / (t·min); when increasing the net circulation, increase the boost gas flow rate to 1.0-1.3 NL / (t·min). The boost gas flow rate should be increased immediately after each batch of alloy is added.

2. The low-cost RH ultra-low carbon silicon steel smelting method according to claim 1, characterized in that, After the desulfurization pretreatment process of molten iron in step 1 is completed, the molten iron should meet the following requirements: S≤0.0015%, temperature≥1300℃.

3. The low-cost RH ultra-low carbon silicon steel smelting method according to claim 2, characterized in that, After the desulfurization pretreatment process of molten iron is completed, the slag is removed, and the ratio of [slag area] to [molten iron surface area] after slag removal is ≤2.0%.

4. The low-cost RH ultra-low carbon silicon steel smelting method according to claim 1, characterized in that, In step 2, a top-and-bottom blown converter is used to smelt the desulfurized molten iron; a supersonic oxygen lance is used to supply oxygen to the molten iron for smelting; lime, dolomite, and iron ore are used to make slag; the final temperature of the converter is controlled at 1645-1690℃; and the C content is 0.03-0.08% and the O content is 0.03-0.08% by mass percentage.

5. The low-cost RH ultra-low carbon silicon steel smelting method according to claim 1, characterized in that, In step 2, slag feeding is strictly prohibited during converter tapping. Lime is added when the tapping rate is 20%-30%, with an addition amount of 1.5 kg / t-3.5 kg / t. After the converter tapping is completed, a low-alumina slag surface deoxidizer is added to modify the slag, with an addition amount of 1.0 kg / t-2.0 kg / t. Bottom blowing and stirring of the ladle are activated throughout the tapping process, with a bottom blowing flow rate of 1.5 NL / (t·min)-4.0 NL / (t·min) and a stirring time of >3 min.

6. The low-cost RH ultra-low carbon silicon steel smelting method according to claim 1, characterized in that, The molten steel hoisted to the RH treatment station in step 3 meets the following requirements: temperature ≥ 1610℃, of which the furnace opening temperature ≥ 1615℃; C content 0.025%-0.075% by mass percentage; O content 0.025%-0.075% by mass percentage; and T.Fe in slag ≤ 15%.

7. The low-cost RH ultra-low carbon silicon steel smelting method according to claim 1, characterized in that, In step 3, after the steel melt is decarburized, metallic aluminum and metallic manganese are added sequentially for alloying. During alloying, a low-carbon steel slag surface deoxidizer is added to the slag surface at a rate of 1.5 kg / t to 2.5 kg / t. Then, a net circulation process is performed with a net circulation time of ≥6 min. Finally, the steel is tapped through a hole, and the T.Fe content in the tapped slag is ≤5%.

8. The low-cost RH ultra-low carbon silicon steel smelting method according to claim 7, wherein the alloy composition used in the alloying treatment is: The aluminum composition, by mass percentage, includes: Al ≥ 99%, the remainder being iron and unavoidable impurities; The ultra-low carbon and low sulfur ferrosilicon composition, by mass percentage, includes: C: 0.007%-0.014%, Si: 80%-90%, P≤0.020%, S≤0.015%, Al: 0.05%-0.10%, with the remainder being iron and unavoidable impurities; the metallic manganese composition, by mass percentage, includes: Mn≥96%, C: 0.02%-0.08%, P≤0.015%, S≤0.015%, Al≤0.005%, with the remainder being iron and unavoidable impurities. The ferrosilicon alloy is ordinary ferrosilicon or low-carbon, low-sulfur ferrosilicon. The ordinary ferrosilicon composition, by mass percentage, includes: C: 0.10%-0.20%, Si: 70%-80%, P≤0.025%, S≤0.030%, Al: 1.80%-2.2%, with the remainder being iron and unavoidable impurities. The low-carbon, low-sulfur ferrosilicon composition, by mass percentage, includes: C: 0.01%-0.03%, Si: 75%-85%, P≤0.020%, S≤0.020%, Al: 0.10%-0.30%, with the remainder being iron and unavoidable impurities.

9. The low-cost RH ultra-low carbon silicon steel smelting method according to claim 1, characterized in that, Step 4 involves the following process for the protective casting of molten steel after RH vacuum treatment: casting is performed using a long ladle nozzle and argon seal, tundish covering agent, submerged entry nozzle, and mold protective slag.

Citation Information

Patent Citations

  • Method for synchronously desulphurizing molten steel and slag of non-oriented silicon steel RH vacuum oven

    CN107299196A

  • RH variety steel silicon deoxidation process