Preparation method of high light transmittance and high haze polyimide substrate

By synthesizing olefin-terminated amide monomers and Grubbs II catalyst through ternary copolymerization, a polyimide substrate with high transmittance and high haze was prepared, solving the problem of low transmittance of polyimide films and meeting the requirements of flexible electronic devices for high transmittance and haze.

CN117487214BActive Publication Date: 2024-11-01SUMII TECH (SHENZHEN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311268421.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-28
Publication Date
2024-11-01
Estimated Expiration
2043-09-28

AI Technical Summary

Technical Problem

Existing polyimide films have low transmittance due to backscattering, which cannot meet the requirements of flexible electronic devices for high transmittance and low haze.

Method used

Polyimide polymers were prepared by synthesizing olefin-terminated amide monomers, and ternary copolymerization was carried out using Grubbs II catalyst to disrupt the symmetry of the polymer chains. A high-transmittance, high-haze substrate was formed by combining a polyimide film and a polyimide nanomaterial in a bilayer composite.

Benefits of technology

This improved the transparency and haze of the substrate, solved the problem of low light transmittance of polyimide films caused by backscattering, and realized a polyimide substrate material with high light transmittance and high haze.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117487214B_ABST
    Figure CN117487214B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a high-transmittance and high-haze polyimide substrate, which specifically comprises the following steps: step 1, synthesizing an olefin terminal amide monomer; step 2, preparing a polyimide polymer; step 3, preparing a polyimide film according to the polyimide polymer prepared in step 2; and step 4, preparing a polyimide substrate according to the polyimide film prepared in step 3. The present invention solves the problem of light transmittance of a polyimide film caused by backscattering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials and relates to a method for preparing a high-light-transmittance and high-haze polyimide substrate. Background Art

[0002] Flexible electronic devices such as flexible display screens and flexible solar cells are developing rapidly. Substrate flexibility is the key to achieving device flexibility. Since flexible display screens and flexible solar cell technologies have higher requirements for substrate light transmittance, they play an important role in the efficiency of light-to-electricity or electricity-to-light.

[0003] Polyimide has good application prospects in the field of electronic devices due to its good water and oxygen isolation and heat resistance. The existing polyimide film has low transmittance due to backscattering; in addition, haze materials, as new light management materials, can effectively improve the optoelectronic performance of devices. Therefore, how to improve the transmittance and haze of substrate materials has become an urgent problem to be solved in this field. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a high-transmittance and high-haze polyimide substrate, which solves the problem of low light transmittance of a polyimide film caused by backscattering.

[0005] The technical solution adopted by the present invention is a method for preparing a high-transmittance, high-haze polyimide substrate, which specifically comprises the following steps:

[0006] Step 1, synthesizing olefin terminal amide monomer;

[0007] Step 2, preparing a polyimide polymer;

[0008] Step 3, preparing a polyimide film according to the polyimide polymer prepared in step 2;

[0009] Step 4: prepare a polyimide substrate based on the polyimide film prepared in step 3.

[0010] The present invention is also characterized in that:

[0011] The specific process of step 1 is:

[0012] Step 1.1, preparing a diaminoamide compound;

[0013] Step 1.2, 2.91 g to 5.82 g of the diaminoamide compound, 2.29 g to 4.58 g of 4-vinyl iodobenzene, 0.31 g to 0.62 g of copper powder, and 0.24 g to 0.48 g of sodium hydride are dispersed in 100 mL to 200 mL of m-cresol solution, purged with nitrogen for 30 min to 60 min, and then heated at 60 o C-90 oC for 1h-2h, and then raise the temperature to 130 o C-160 o C. After the reaction is completed, the temperature is cooled, the insoluble matter is removed by filtration, and the olefin terminal amide monomer is purified by column separation.

[0014] The specific process of step 1.1 is:

[0015] Step 1.1.1, add 4.00 g-8.00 g of 4,4'-diaminodiphenyl ether and 10 mL-20 mL of m-cresol into a reaction flask, purge with nitrogen for 10 min-30 min to remove air, then heat to 100°C-110°C and stir for 10 min-25 min to dissolve all the 4,4'-diaminodiphenyl ether;

[0016] Step 1.1.2, dissolve 2.18g-4.36g of pyromellitic anhydride and 0.3g-0.6g of isoquinoline in 10mL-20mL of m-cresol, and then add dropwise to the 4,4'-diaminodiphenyl ether solution for 0.3h-1h. The temperature is maintained at 100℃-120℃ during the addition. After the addition is completed, the temperature of the reaction system is raised to 200℃-220℃ for 3-6 hours. After the reaction is completed, the reaction solution is cooled to room temperature and separated by a column to purify the diaminoamide compound.

[0017] The specific process of step 2 is as follows: 0.39g-0.79g of olefin terminal amide monomer, 0.23g-0.92g of 1,4-diallyl-2,3,5,6-tetrafluorobenzene, and 0.19g-0.76g of 1,4-bis(allyloxy)benzene are dissolved in 10mL-20mL of m-cresol solution, purged with nitrogen for 30min-60min, 50mg-100mg of Grubbs II catalyst is added, and the mixture is heated for 45min-50min. o C for 12h-24h, then add 50mg-100mg of Grubbs II catalyst and continue the reaction for 12h-24h. The solution after the reaction is introduced into industrial alcohol for sedimentation to obtain a filter cake of 45 o C vacuum dried for later use.

[0018] The specific process of step 3 is:

[0019] Take 30 mg-50 mg of polyimide polymer and dissolve it in 10 mL-15 mL of m-cresol solution, pour it into a polytetrafluoroethylene mold, put it into a constant temperature drying oven to dry, and obtain a polyimide film material film.

[0020] The specific process of step 4 is:

[0021] Step 4.1, dissolve 20 mg to 30 mg of polyimide polymer in 5 mL to 10 mL of m-cresol solution, and let the solution stand overnight;

[0022] Step 4.2, adding the solution prepared in step 4.1 dropwise into 100 mL to 200 mL of industrial alcohol to obtain a nanoparticle dispersion, and concentrating the dispersion to 50 mL;

[0023] Step 4.3, take a polyimide film of 2cmx2cm, spin-coat the dispersion prepared in step 4.2 onto the polyimide film, spin-coating for 5 to 15 times, and finally put the polyimide film into a constant temperature drying oven to dry, to obtain a polyimide substrate.

[0024] The beneficial effects of the present invention are as follows:

[0025] The present invention prepares a novel polyimide film and polyimide nanomaterial, further heat-presses and composites them to form a double-layer structure, obtains a high-transmittance-high-haze substrate, realizes the introduction of F atoms in the polymer chain in any proportion, and simultaneously utilizes the ternary copolymerization catalyzed by Grubbs II to destroy the symmetry of the polymer chain, thereby improving the transparency of the substrate. 2. The present invention utilizes a polyimide film and a polyimide nanomaterial having the same molecular structure to composite and prepare a double-layer high-transmittance-high-haze substrate material. The problem of light transmittance of polyimide film caused by backscattering is solved. The preparation of polyimide polymer adopts Grubbs II catalytic polymerization to realize the effective regulation of F content. At the same time, the long-range disorder of the ternary copolymer polymer chain under the Grubbs II catalytic condition is conducive to the improvement of the transparency of the substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a comparison chart of light transmittance test of substrates prepared in Example 1 of the method for preparing a high-transmittance, high-haze polyimide substrate of the present invention and in Comparative Examples 1 to 3;

[0027] Figure 2 This is a comparison chart of the haze of substrates prepared in Example 1 of the method for preparing a high-light-transmittance, high-haze polyimide substrate of the present invention and in Comparative Examples 1 to 3. DETAILED DESCRIPTION

[0028] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0029] The method for preparing a high light transmittance and high haze polyimide substrate of the present invention specifically comprises the following steps:

[0030] 1) Synthesis of olefin-terminated amide monomers

[0031] Add 4,4'-diaminodiphenyl ether (4.00-8.00 g) and m-cresol (10-20 mL) to a 100 mL reaction bottle, purge with nitrogen for 10-30 min to remove air, then heat to 100-110°C and stir for 10-25 min to dissolve all 4,4'-diaminodiphenyl ether; further dissolve pyromellitic anhydride (2.18-4.36 g) and isoquinoline (0.3-0.6 g) in 10-20 mL m-cresol, then slowly drop them into the 4,4'-diaminodiphenyl ether solution for 0.3-1 h, and keep the temperature at 100-120°C during the dropwise addition. After the dropwise addition is completed, the temperature of the reaction system is gradually raised to 200-220°C for 3-6 hours. After the reaction was completed, the reaction solution was cooled to room temperature and purified by column separation (eluent was methanol:chloroform:n-hexane, with a volume ratio of 1:3:9) to obtain a diaminoamide compound.

[0032] Disperse the above diaminoamide compound (2.91-5.82 g), 4-vinyl iodobenzene (2.29-4.58 g), copper powder (0.31-0.62 g), and sodium hydride (0.24-0.48 g) in 100-200 mL of m-cresol solution and purge with nitrogen for 30-60 min. o C for 1-2 hours, and then further increase the temperature to 130-160 o C. After the reaction is completed, the temperature is cooled and the insoluble matter is removed by filtration. Column separation (eluent is methanol: ethyl acetate: n-hexane, the volume ratio is 1:5:15) is used to purify the olefin terminal amide monomer.

[0033] 2) Preparation of polyimide polymer

[0034] Take olefin terminal amide monomer (0.39-0.79g), 1,4-diallyl-2,3,5,6-tetrafluorobenzene (0.23-0.92), 1,4-bis(allyloxy)benzene (0.19-0.76g) and dissolve them in m-cresol (10-20 mL) solution, and purge with nitrogen for 30-60 min. Add 50-100mg of Grubbs II catalyst, 45 o C for 12-24 hours, then add 50-100 mg of Grubbs II catalyst and continue the reaction for 12-24 hours. The solution after the reaction is introduced into industrial alcohol for sedimentation to obtain a filter cake of 45 o C vacuum dried for later use.

[0035] Polyimide polymer material, the synthesis route is as follows:

[0036]

[0037] 3) Preparation of polyimide film

[0038] Take 30-50 mg of polyimide polymer and dissolve it in 10-15 mL of m-cresol solution, pour it into a polytetrafluoroethylene mold with a diameter of 8 cm, put it in a constant temperature drying oven and dry it for 7 days to obtain a polyimide film material film.

[0039] 4) High light transmittance, high haze polyimide substrate

[0040] Take 20-30 mg of polyimide polymer and dissolve it in 5-10 mL of m-cresol solution. Let the solution stand overnight. Then slowly add the solution to 100-200 mL of industrial alcohol (addition time is 20-40 min) to obtain nanoparticle dispersion. Concentrate the dispersion to 50 mL. Take a polyimide film 2x2 cm and spin coat the white dispersion onto the polyimide film. Spin coat for 5-15 times. Finally, place the film in a 45 o The polyimide substrate was dried in a constant temperature drying oven at C.

[0041] Example 1 (3 equivalents of 1,4-diallyl-2,3,5,6-tetrafluorobenzene are added during the preparation of polyimide polymer, and the substrate is colorless)

[0042] Step 1, add 4.00 g of 4,4'-diaminodiphenyl ether and 10 mL of m-cresol into a 100 mL reaction bottle, purge with nitrogen for 10 min to remove air, then heat to 100°C and stir for 10 min to dissolve all 4,4'-diaminodiphenyl ether; further dissolve 2.18 g of pyromellitic anhydride and 0.3 g of isoquinoline in 10 mL of m-cresol, then slowly drop them into the 4,4'-diaminodiphenyl ether solution, the drop time is 0.3 h, and the temperature is maintained at 100°C during the drop process. After the drop addition is completed, the temperature of the reaction system is gradually raised to 200°C for 3 hours. After the reaction is completed, the reaction solution is cooled to room temperature and separated by column (the eluent is methanol: chloroform: n-hexane, the volume ratio is 1:3:9) to purify the diaminoamide compound.

[0043] Take 2.91 g of the above diaminoamide compound, 2.29 g of 4-vinyl iodobenzene, 0.31 g of copper powder, and 0.24 g of sodium hydride and disperse them in 100 mL of m-cresol solution. Purge with nitrogen for 30 min. Then, at 60 o C for 1 h, and then the temperature was further increased to 130 o C. After the reaction is completed, the temperature is cooled and the insoluble matter is removed by filtration. Column separation (eluent is methanol: ethyl acetate: n-hexane, the volume ratio is 1:5:15) is used to purify the olefin terminal amide monomer.

[0044] Step 2: Dissolve 0.39 g of olefin terminal amide monomer, 0.69 g of 1,4-diallyl-2,3,5,6-tetrafluorobenzene, and 0.19 g of 1,4-bis(allyloxy)benzene in 10 mL of m-cresol solution and purge with nitrogen for 30 min. Add 50 mg of Grubbs II catalyst and 45 o C for 12 h, then 50 mg of Grubbs II catalyst was added and the reaction was continued for 12 h. The solution after the reaction was introduced into industrial alcohol for sedimentation to obtain a filter cake of 45 o C is vacuum dried for later use. In Example 1, the molecular formula of the polyimide polymer material synthesis route is x:y:z=3:0.5:1. The result of gel permeation chromatography test shows that the molecular weight is 30,000-50,000 and the molecular weight distribution is 1.1-1.3.

[0045] Step 3, take 30 mg of polyimide polymer and dissolve it in 10 mL of m-cresol solution, pour it into a polytetrafluoroethylene mold with a diameter of 8 cm, put it in a constant temperature drying oven and dry it for 7 days to obtain a polyimide film material film.

[0046] Step 4, take 20 mg of polyimide polymer and dissolve it in 5 mL of m-cresol solution, and let the solution stand overnight. Then slowly add the solution to 100 mL of industrial alcohol (addition time is 20 min) to obtain nanoparticle dispersion, and concentrate the dispersion to 50 mL. Take a polyimide film 2x2 cm, spin-coat the white dispersion onto the polyimide film, spin-coat for 5 times, and finally put the film into 45 o The polyimide substrate was dried in a constant temperature drying oven at C.

[0047] Comparative Example 1 (nanoparticles are not spin-coated on the film surface, step 4 of Example 1 is missing, and the remaining steps are the same as Example 1)

[0048] Take 30 mg of polyimide polymer and dissolve it in 10 mL of m-cresol solution, pour it into a polytetrafluoroethylene mold with a diameter of 8 cm, put it in a constant temperature drying oven and dry it for 7 days to obtain a polyimide film material film.

[0049] Comparative Example 2 (1 equivalent of 1,4-diallyl-2,3,5,6-tetrafluorobenzene was added during the preparation of the polyimide polymer, the substrate was light yellow, and the rest of the process was the same as in Example 1)

[0050] Take 0.39 g of olefin terminal amide monomer, 0.23 g of 1,4-diallyl-2,3,5,6-tetrafluorobenzene, and 0.19 g of 1,4-bis(allyloxy)benzene and dissolve them in 10 mL of m-cresol solution. Purge with nitrogen for 30 min. Add 50 mg of Grubbs II catalyst and 45 oC for 12 h, then 50 mg of Grubbs II catalyst was added and the reaction was continued for 12 h. The solution after the reaction was introduced into industrial alcohol for sedimentation to obtain a filter cake of 45 o C vacuum dried for later use.

[0051] Take 30 mg of polyimide polymer and dissolve it in 10 mL of m-cresol solution, pour it into a polytetrafluoroethylene mold with a diameter of 8 cm, put it in a constant temperature drying oven and dry it for 7 days to obtain a polyimide film material film.

[0052] Take 20 mg of polyimide polymer and dissolve it in 5 mL of m-cresol solution. Let the solution stand overnight. Then slowly add the solution to 100 mL of industrial alcohol (addition time is 20 min) to obtain nanoparticle dispersion. Concentrate the dispersion to 50 mL. Take a 2x2 cm polyimide film and spin-coat the white dispersion onto the polyimide film for 5 times. Finally, place the film in a 45 o The polyimide substrate was dried in a constant temperature drying oven at C.

[0053] Comparative Example 3 (1,4-diallyl-2,3,5,6-tetrafluorobenzene is not added during the preparation of the polyimide polymer, and the substrate is yellow)

[0054] Take 0.39 g of olefin terminal amide monomer and 0.19 g of 1,4-bis(allyloxy)benzene and dissolve them in 10 mL of m-cresol solution. Purge with nitrogen for 30 min. Add 50 mg of Grubbs II catalyst and 45 o C for 12 h, then 50 mg of Grubbs II catalyst was added and the reaction was continued for 12 h. The solution after the reaction was introduced into industrial alcohol for sedimentation to obtain a filter cake of 45 o C vacuum dried for later use.

[0055] Take 30 mg of polyimide polymer and dissolve it in 10 mL of m-cresol solution, pour it into a polytetrafluoroethylene mold with a diameter of 8 cm, put it in a constant temperature drying oven and dry it for 7 days to obtain a polyimide film material film.

[0056] Take 20 mg of polyimide polymer and dissolve it in 5 mL of m-cresol solution. Let the solution stand overnight. Then slowly add the solution to 100 mL of industrial alcohol (addition time is 20 min) to obtain nanoparticle dispersion. Concentrate the dispersion to 50 mL. Take a 2x2 cm polyimide film and spin-coat the white dispersion onto the polyimide film. Spin-coat 5 times and finally place the film in a 45 o The polyimide substrate was dried in a constant temperature drying oven at C.

[0057] Results and Discussion

[0058] Through the surface roughness test, it was found that the surface roughness of Example 1 was about 20 nm, while the surface roughness of Comparative Example 1 was about 0.5 nm. The main reason was that a layer of polyimide nanomaterial was spin-coated on the surface of Example 1.

[0059] like Figure 1 As shown, the substrate transmittance test shows that Example 1 has the highest transmittance at 550nm; this is mainly due to the spin coating of a layer of polyimide nanomaterial on its surface, which plays a role in anti-reflection; secondly, the GrubbsII multi-catalytic assembly is used to destroy the symmetry of the molecular structure. Comparative Examples 2-3 all have light absorption between 380-500, causing the substrate to present its complementary color. Among them, the absorption of Comparative Example 3 between 380-500 is significantly stronger than that of Comparative Example 2, so Comparative Example 2 presents a light yellow color; while Comparative Example 3 is darker in color and presents a color change.

[0060] like Figure 2 As shown, Example 1 and Comparative Examples 2-3 all have a relatively high haze (14-17%), which is due to the polyimide nanomaterials being spin-coated on the surface. In contrast, Comparative Example 1 is not spin-coated with nanomaterials, and its surface is relatively smooth, resulting in a relatively low haze value of only 1.4%.

[0061] Example 2

[0062] Step 1, add 6.00 g of 4,4'-diaminodiphenyl ether and 15 mL of m-cresol into a 100 mL reaction bottle, purge with nitrogen for 20 min to remove air, then heat to 105°C and stir for 15 min to dissolve all 4,4'-diaminodiphenyl ether; further dissolve 2.35 g of pyromellitic anhydride and 0.4 g of isoquinoline in 15 mL of m-cresol, and then slowly drop them into the 4,4'-diaminodiphenyl ether solution, the drop time is 0.8 h, and the temperature is maintained at 110°C during the drop process. After the drop addition is completed, the temperature of the reaction system is raised to 210°C for 5 h. After the reaction is completed, the reaction solution is cooled to room temperature and separated by column (the eluent is methanol: chloroform: n-hexane, the volume ratio is 1:3:9) to purify the diaminoamide compound.

[0063] Take 4.68 g of the above diaminoamide compound, 3.35 g of 4-vinyl iodobenzene, 0.48 g of copper powder, and 0.36 g of sodium hydride and disperse them in 150 mL of m-cresol solution. Purge with nitrogen for 50 min. Then, at 80 o C for 1.5 h, and then the temperature was raised to 150 o C. After the reaction is completed, the temperature is cooled and the insoluble matter is removed by filtration. Column separation (eluent is methanol: ethyl acetate: n-hexane, the volume ratio is 1:5:15) is used to purify the olefin terminal amide monomer.

[0064] Step 2: Dissolve 0.68 g of olefin terminal amide monomer, 0.23 g of 1,4-diallyl-2,3,5,6-tetrafluorobenzene, and 0.48 g of 1,4-bis(allyloxy)benzene in 15 mL of m-cresol solution and purge with nitrogen for 45 min. Add 80 mg of Grubbs II catalyst and 45 o C for 20 h, then 80 mg of Grubbs II catalyst was added and the reaction was continued for 20 h. The solution after the reaction was introduced into industrial alcohol for sedimentation to obtain a filter cake of 45 o C vacuum dried for later use.

[0065] Step 3, take 40 mg of polyimide polymer and dissolve it in 12 mL of m-cresol solution, pour it into a polytetrafluoroethylene mold with a diameter of 8 cm, put it in a constant temperature drying oven and dry it for 7 days to obtain a polyimide film material film.

[0066] Step 4: Dissolve 25 mg of polyimide polymer in 8 mL of m-cresol solution and let the solution stand overnight. Slowly add the solution to 150 mL of industrial alcohol (addition time is 30 min) to obtain nanoparticle dispersion, and concentrate the dispersion to 50 mL. Take a 2x2 cm polyimide film and spin-coat the white dispersion onto the polyimide film. Spin-coat 10 times and place the film in a 45 o The polyimide substrate was dried in a constant temperature drying oven at C.

[0067] Example 3

[0068] Step 1, add 8.00 g of 4,4'-diaminodiphenyl ether and 20 mL of m-cresol into a 100 mL reaction bottle, purge with nitrogen for 30 min to remove air, then heat to 110°C and stir for 25 min to dissolve all 4,4'-diaminodiphenyl ether; further dissolve 4.36 g of pyromellitic anhydride and 0.6 g of isoquinoline in 20 mL of m-cresol, and then slowly drop them into the 4,4'-diaminodiphenyl ether solution for 1 h, and keep the temperature at 120°C during the dropwise addition. After the dropwise addition is completed, the temperature of the reaction system is gradually raised to 220°C for 6 h. After the reaction is completed, the reaction solution is cooled to room temperature and separated by column (the eluent is methanol: chloroform: n-hexane, the volume ratio is 1:3:9) to purify the diaminoamide compound.

[0069] Take 5.82 g of the above diaminoamide compound, 4.58 g of 4-vinyl iodobenzene, 0.62 g of copper powder, and 0.48 g of sodium hydride and disperse them in 200 mL of m-cresol solution. Purge with nitrogen for 60 min. Then, at 90 o C for 2 h, and then the temperature was further increased to 160o C. After the reaction is completed, the temperature is cooled and the insoluble matter is removed by filtration. Column separation (eluent is methanol: ethyl acetate: n-hexane, the volume ratio is 1:5:15) is used to purify the olefin terminal amide monomer.

[0070] Step 2: Dissolve 0.79 g of olefin terminal amide monomer, 0.92 g of 1,4-diallyl-2,3,5,6-tetrafluorobenzene, and 0.76 g of 1,4-bis(allyloxy)benzene in 20 mL of m-cresol solution and purge with nitrogen for 60 min. Add 100 mg of Grubbs II catalyst and 45 o C for 24 h, then 100 mg of Grubbs II catalyst was added and the reaction was continued for 24 h. The solution after the reaction was introduced into industrial alcohol for sedimentation to obtain a filter cake of 45 o C vacuum dried for later use.

[0071] Step 3, take 50 mg of polyimide polymer and dissolve it in 15 mL of m-cresol solution, pour it into a polytetrafluoroethylene mold with a diameter of 8 cm, put it in a constant temperature drying oven and dry it for 7 days to obtain a polyimide film material film.

[0072] Step 4: Dissolve 30 mg of polyimide polymer in 10 mL of m-cresol solution and let the solution stand overnight. Slowly add the solution to 200 mL of industrial alcohol (addition time is 40 min) to obtain nanoparticle dispersion, and concentrate the dispersion to 50 mL. Take a 2x2 cm polyimide film and spin-coat the white dispersion onto the polyimide film for 15 spin-coating times. Finally, place the film in a 45 o The polyimide substrate was dried in a constant temperature drying oven at C.

Claims

1. A method for preparing a high light transmittance and high haze polyimide substrate, characterized in that: The specific steps include: Step 1, synthesizing olefin terminal amide monomer; The specific process of step 1 is as follows: Step 1.1, preparing a diaminoamide compound; The specific process of step 1.1 is as follows: Step 1.1.1, add 4.00 g-8.00 g of 4,4'-diaminodiphenyl ether and 10 mL-20 mL of m-cresol into a reaction flask, purge with nitrogen for 10 min-30 min to remove air, then heat to 100°C-110°C and stir for 10 min-25 min to dissolve all the 4,4'-diaminodiphenyl ether; Step 1.1.2, dissolving 2.18g-4.36g of pyromellitic anhydride and 0.3g-0.6g of isoquinoline in 10mL-20mL of m-cresol, and then adding dropwise to the 4,4'-diaminodiphenyl ether solution for 0.3h-1h. The temperature is maintained at 100℃-120℃ during the addition. After the addition is completed, the temperature of the reaction system is raised to 200℃-220℃ for 3-6 hours. After the reaction is completed, the reaction solution is cooled to room temperature, separated by a column, and purified to obtain a diaminoamide compound; Step 1.2, 2.91 g to 5.82 g of the diaminoamide compound, 2.29 g to 4.58 g of 4-vinyl iodobenzene, 0.31 g to 0.62 g of copper powder, and 0.24 g to 0.48 g of sodium hydride are dispersed in 100 mL to 200 mL of m-cresol solution, purged with nitrogen for 30 min to 60 min, and then stirred at 60 o C-90 o C for 1h-2h, and then raise the temperature to 130 o C-160 o C. After the reaction is completed, the temperature is cooled, the insoluble matter is removed by filtration, and the olefin terminal amide monomer is purified by column separation; Step 2, preparing a polyimide polymer; The specific process of step 2 is as follows: 0.39g-0.79g of olefin terminal amide monomer, 0.23g-0.92g of 1,4-diallyl-2,3,5,6-tetrafluorobenzene, and 0.19g-0.76g of 1,4-bis(allyloxy)benzene are dissolved in 10mL-20mL of m-cresol solution, purged with nitrogen for 30min-60min, 50mg-100mg of Grubbs II catalyst is added, and the mixture is heated to 45°C. o C for 12h-24h, then add 50mg-100mg of Grubbs II catalyst and continue the reaction for 12h-24h. The solution after the reaction is introduced into industrial alcohol for sedimentation to obtain a filter cake of 45 o C vacuum drying for later use; Step 3, preparing a polyimide film according to the polyimide polymer prepared in step 2; the specific process of step 3 is: Take 30 mg-50 mg of polyimide polymer and dissolve it in 10 mL-15 mL of m-cresol solution, pour it into a polytetrafluoroethylene mold, put it into a constant temperature drying oven for drying, and obtain a polyimide film material film; Step 4, preparing a polyimide substrate according to the polyimide film prepared in step 3; The specific process of step 4 is as follows: Step 4.1, dissolve 20 mg to 30 mg of polyimide polymer in 5 mL to 10 mL of m-cresol solution, and let the solution stand overnight; Step 4.2, adding the solution prepared in step 4.1 dropwise into 100 mL to 200 mL of industrial alcohol to obtain a nanoparticle dispersion, and concentrating the dispersion to 50 mL; Step 4.3, take a polyimide film of 2cmx2cm, spin-coat the dispersion prepared in step 4.2 onto the polyimide film, spin-coating for 5 to 15 times, and finally put the polyimide film into a constant temperature drying oven to dry, to obtain a polyimide substrate.