A method for preventing intergranular stress corrosion and stress corrosion cracking in the shell of a hot blast stove

By using Q345R steel plates on the hot blast stove shell, scientific calculations, and multi-layer anti-corrosion treatment, the problem of stress corrosion cracking of the furnace shell under high pressure and high blast temperature was solved, resulting in a significant improvement in the lifespan and stability of the furnace shell.

CN117487988BActive Publication Date: 2026-11-17ZHENGZHOU YUXING HOT STOVE TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311410216.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-27
Publication Date
2026-11-17
Estimated Expiration
2043-10-27

AI Technical Summary

Technical Problem

Due to improper material selection and insufficient design calculations, the existing hot blast stove shell is prone to stress corrosion cracking under high pressure and high temperature conditions, and traditional anti-corrosion measures cannot effectively prevent cracking.

Method used

Using Q345R steel plates, the thickness of the furnace shell is determined by scientific calculation. The weld seams are then coated with acid-resistant high-temperature paint or sprayed with ceramic glaze to form a ceramic layer structure. This is then covered with stainless steel plates or ceramic materials to seal the corrosive medium. Finally, an acid-resistant coating is sprayed to form a multi-layer protective layer.

Benefits of technology

It effectively isolates corrosive media, increases the lifespan of the furnace shell by 3-10 times, solves the problem of stress corrosion cracking, and ensures stable operation of the furnace shell under high-pressure and high-temperature conditions, with a service life of over 30 years.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to a method for preventing intergranular stress corrosion and stress corrosion cracking in hot blast stove shells. It effectively solves the problem of furnace shell cracking, completely isolates the direct penetration corrosion of acidic corrosive media, and allows for safe, efficient, energy-saving, environmentally friendly, and low-cost use at high blast temperatures. The technical solution includes the following steps: 1) Selection of furnace shell material; 2) Scientific calculation and pre-fabrication design of the furnace shell; 3) Rolling, installation, and welding of the furnace shell; 4) Cleaning weld slag and grinding the weld seams; 5) Covering and inlaying or welding the weld seams; 6) Acid-proof treatment; 7) Sealing treatment; 8) Spraying protective treatment. This invention is simple, novel, unique, and easy to implement. The method is simple and easy to implement, with an extremely short manufacturing and processing period. It completely solves the problems of furnace shell cracking and stress corrosion cracking, increasing the overall lifespan of the furnace shell by 3-10 times. It is an innovation in methods for preventing intergranular stress corrosion and stress corrosion cracking in hot blast stove shells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to hot blast stoves, and in particular to a method for preventing intergranular stress corrosion and stress corrosion cracking of the furnace shell. Background Technology

[0002] Currently, the high-pressure (5MPa) and high-temperature (1300 degrees Celsius) top-fired hot blast stoves that are equipped with extra-large blast furnaces in my country are distributed in 32 hot blast stoves of 8 blast furnaces, including Jingtang Iron and Steel Company 3X5500, Baosteel Zhanjiang Company 3X5050, Angang Company 4747, and Taiyuan Iron and Steel Company 4800. Since the top-fired hot blast stoves used in the previous design were all hot blast stoves with ordinary blast temperature (1200-1250 degrees Celsius) and ordinary pressure (0.4MPa-0.45MPa), the steel shell material used for both high-pressure high-temperature hot blast stoves and ordinary hot blast stoves is Q345C low-alloy high-strength structural steel as the outer shell material of the hot blast stove.

[0003] The contents of harmful components sulfur and phosphorus in Q345C low-alloy high-strength structural steel are relatively high. In particular, the adoption of Q345C as the material for the shell of high-pressure and high-wind-temperature hot-blast stoves exerts a significant impact on both the structure and service life of the furnace shell. Correspondingly, obvious full-scale cracking phenomena have occurred during the application of such shells in high-pressure and high-wind-temperature hot-blast stoves. As specified in relevant steel grade descriptions, sulfur and phosphorus cause hot brittleness, cold brittleness, pores and welding defects, and combined with comprehensive factors such as residual stress and poorer welding quality, stress cracking is relatively common in furnace shell plates, which is a potential cracking factor. Since the cracking textures are small and fine and cannot be observed with the naked eye, and with the gradual popularization and prevalence of top-fired hot-blast stoves, rolling, processing and welding have become relatively common processes. Therefore, users, manufacturers and installers have not adequately considered the damage caused by such factors, leaving hidden dangers for the subsequent continuous accelerated cracking of the furnace shell. Second, through comparison of the design of the furnace body structure and the manufacturing and installation drawings of the furnace shell for the top-fired hot-blast stoves supporting the 3X2500 of China Railway Equipment and the 4747m³ blast furnace of Angang, it is found that the regenerative heat exchange capacity of the furnace body structure and the furnace shell thickness of the hot-blast stoves under the two different working conditions are the same, while the pressure and wind temperature differ greatly, which indicates that there are errors in the design calculation of the furnace shell. The calculation formula for the furnace shell found in the national furnace shell design specification is t=2.2OD+2 (t - furnace shell thickness, 2.2 -- empirical modulus, D - diameter of the hot-blast stove, 2 - correction value). This calculation formula has been used for ordinary hot-blast stoves for at least more than 20 years, but the newly built high-pressure and high-wind-temperature hot-blast stoves in China are different from hot-blast stoves with ordinary pressure and wind temperature. At present, this part is designed by the Russian company Kalugin, and the furnace shell design calculation formulas seen are exactly the calculation formulas for ordinary hot-blast stoves in China's furnace shell design specifications, which leads to the lack of a valid basis for the design calculation of the furnace shells of high-pressure and high-wind-temperature hot-blast stoves. We have also developed a calculation formula for high-pressure and high-wind-temperature furnace shells in production practice. This calculation formula is slightly more complex, incorporating the explosion load, weld coefficient, corrosion coefficient, included angle coefficient, load-bearing coefficient and pressure into the calculation formula. The furnace shell calculated through this formula has been used in the catenary top-fired hot-blast stove supporting the 1860m³ blast furnace of Shanxi Tongcai for 11 years so far, with a designed wind temperature of 1320°C, and it has once achieved China's highest wind temperature of 1314.The historical record of 7 degrees Celsius monthly average wind temperature has not been broken to this day. Therefore, we believe that the first reason for using the calculation formula of ordinary hot blast stoves to calculate the furnace shell of high-pressure, high-temperature hot blast stoves is that the ultra-thin furnace shell is not suitable for the current high-pressure, high-temperature operating conditions, resulting in stress corrosion cracking. The second reason is that when the wind temperature is designed to be used at 1300 degrees Celsius, the nitrogen oxides of the burner are not very high, only 20-150 ppm, and the highest is only 200 ppm. Industry experts and conferences have consistently pointed out that the corrosive medium of harmful gases in flue gas such as nitrogen oxides, sulfides, and oxides leads to stress corrosion cracking of the furnace shell welds. Regarding the cracking issue, our research suggests that this is inaccurate. Our calculations show that nitrogen oxide generation during the air supply and pressurization periods is 2500 ppm at an air temperature of 1260 degrees Celsius, with an average of 850 ppm during the air supply period. We estimate that at an air temperature of 1300 degrees Celsius, it should be above 3000 ppm, with an average air supply volume above 1000 ppm. Since both the gas and air at high temperatures contain moisture, this moisture combines with nitrogen oxides to form acidic water droplets that adhere to the furnace shell wall. This is particularly problematic for weld defects and stress-induced structural damage during manufacturing, accelerating furnace shell cracking through corrosion penetration. This is a significant factor. Therefore, in addition to selecting furnace shell materials suitable for the operating conditions, it is essential to scientifically calculate the thickness of the furnace shell to withstand blind flange forces. Furthermore, corrosion protection treatment of the furnace shell material is crucial. Common methods include applying high-temperature acid-resistant paint and acid-resistant spray coatings. However, these traditional methods cannot prevent stress corrosion cracking. Taiyuan Iron & Steel (TISCO) and Jingtang Steel adopted a method of lining the newly installed furnace shells with 3mm thick 904L acid-resistant and corrosion-resistant stainless steel after the furnace shells were cut. This method played a certain role, but the forming and rolling processes are quite complex. For example, TISCO uses an explosive process to combine stainless steel plates with ordinary steel plates, while Jingtang uses a rolling process to combine stainless steel and steel plates. These processes are too complex, have higher welding requirements, and require greater investment. However, even with these methods, cracking still occurred at TISCO. Therefore, such anti-corrosion measures cannot completely prevent cracking.

[0004] Regarding the use of Q345C+904L composite steel plates for the hot blast stove shell of the 4800m³ blast furnace, two measures were actually adopted. First, 3 mm of 904L stainless steel was added to the original steel plate calculation, which is equivalent to thickening the furnace shell. The benefit is that it changes the properties of the original material and enhances the load-bearing capacity of the furnace shell, but stress damage and weld defects in the processing of the external Q345C plate still exist. The second measure is to add stainless steel, which has high corrosion resistance. This measure changes the original design concept and provides strength and corrosion resistance, but weld defects, porosity, and cracks still exist, and the safety hazards are not completely eliminated. At the same time, the use of composite plate technology increases the difficulty of composite process and welding, and also increases investment.

[0005] The furnace shell of the hot stove for the 5500 m³ blast furnace adopts Q345R+904L composite steel plate (when Jingtang Iron and Steel Company cut the furnace shell to replace the cracked one, a team led by Zhang Fuming, a first-class scientist of Shougang Group, visited Yuxing Company for in-depth discussion on Yuxing's technical measures for furnace shell cracking. Yuxing clearly proposed that the hot stove supporting the 1860 m³ blast furnace of Shanxi Tongcai put into operation in 2012 was made of this material, i.e., Q345R, which is the second hot stove supporting a blast furnace adopting this material in China and even in the world so far). In fact, two sets of measures were also adopted: first, 3 mm of 904L stainless steel was added on the basis of the original steel plate calculation, which is equivalent to thickening the thickness of the furnace shell, and the furnace shell was made of high-quality Q345R steel plate with high grade that can reduce welding defects and pores, which not only changed the performance of the original material but also enhanced the resistance load of the furnace shell; the second measure adds the high corrosion resistance performance of stainless steel. This measure changed the original design concept, providing resistance strength and corrosion resistance, but the adoption of composite plate technology increased the difficulty of the composite process and welding, and also increased the investment. The result is not worth the candle.

[0006] Referring to the inspection results of the furnace shell at the weld and heat-affected zone and the base metal of the 5050 hot stove at Baosteel Zhanjiang and the 4747 m³ hot stove at Angang, it is found that there are no network cracks, craze cracks or linear cracks in the base metal, while network cracks and craze cracks exist in the weld and heat-affected zones. Therefore, the furnace shell cracking is stress corrosion cracking, and the cracking areas are all located in the weld and heat-affected zones. Therefore, the use of explosion-bonded composite plates and roll-bonded composite plates in the hot stove furnace shell leads to material waste, increased investment, increased working procedures, and complicated welding technology. Moreover, the stainless steel plate and the ordinary steel plate in the composite plate are integrated, while the weld and the heat-affected zone are the same parts. Therefore, judging from the local weld cracking of the composite plate adopted in the hot stove furnace shell of Taigang, this is not a perfect technical measure to solve the furnace shell cracking. Therefore, this kind of composite steel plate that is wasteful, complicated in working procedures, high in investment, meaningless to the base metal, and still has certain hidden dangers for the weld should be eliminated for making furnace shells.

[0007] Practice has shown that when achieving high blast temperatures, the formation of nitrogen oxides during the pressurization and blasting periods is the primary factor contributing to the corrosion of the furnace shell, leading to weld cracks and porosity. The damage from sulfur dioxide and chlorine oxides during combustion is secondary. However, without stress cracking caused by the manufacturing process, the probability of stress corrosion cracking would be significantly reduced. The conditions of the corrosive media generated by the high-pressure, high-temperature blast of the hot blast stove remain unchanged, as do the residual stress after stress relief during processing and the significantly reduced yield strength after welding. However, the furnace shell material can be improved, and weld defects, porosity, hot brittleness, and cold brittleness can be avoided by modifying the material. Cracking during manufacturing can also be prevented. The furnace shell thickness can be scientifically calculated to suit the operating conditions. For corrosion, certain technical measures can be taken to isolate the corrosive media from the steel plate during the pressurization and blasting periods, preventing contact between the corrosive media and the weak points in the weld with residual stress after the yield strength has decreased. This is a crucial technical means to prevent furnace shell cracking.

[0008] While using Q345C+904L and Q345R+904L composite steel plates can resist penetrating corrosion and improve weld quality to prevent cracking, the composite process is complex (for example, the composite plate for a 4800m³ blast furnace hot blast stove uses an explosive bonding process to firmly bond the two materials, while the composite plate for a 5500m³ blast furnace hot blast stove uses a rolling process). Using 3mm stainless steel machining and welding processes involves high investment costs and requires meticulous craftsmanship. Furthermore, due to the different yield strengths of the two materials, the yield strength at the weld is significantly reduced, and even slight oversights can lead to weld cracking. Therefore, these two methods are not suitable for the stable, long-life, high-temperature blast furnace conditions required for operation.

[0009] In the high-temperature zone of the hot blast stove and the pre-combustion chamber, temperature fluctuations are common. Furthermore, the combustion gas and combustion air introduced into the hot blast stove during combustion and air supply introduce moisture that easily adheres to the furnace shell. Due to the significant difference in yield strength between the weld and the base material, residual stress is prone to occur during processing and installation. Even with timely stress relief, residual stress remains, and the stress and yield strength of the weld and heat-affected zone vary considerably, easily leading to microscopic cracks. These cracks are more noticeable and more severe when the furnace shell material is of a lower grade. While higher-grade materials also exhibit corrosion, their higher grade, lower levels of harmful elements, better welding quality, and fewer hot / cold brittleness and porosity defects mean that even when corrosion penetrates into the micro-cracked areas, it does not cause greater damage or cracking. Nevertheless, necessary measures should still be taken for effective treatment.

[0010] At present, the hot blast stove supporting the 1860m³ blast furnace of Shanxi Tongcai of Yuxing Company adopts Q345R material for the first time. Its pressure is similar to that of the hot blast stove of the 4747m³ blast furnace of Angang, and a practical comparison shows that its air temperature is higher than that of the hot blast stove of the 4747m³ blast furnace of Angang. This proves that it is correct to use Q345R for high-temperature hot blast stoves, the scientific calculation is correct, and the furnace shell can be free from cracking for 11 years. At the same time, in order to completely avoid the stress corrosion cracking of the furnace shell, it is imperative to invent a method for preventing intergranular stress corrosion and stress corrosion cracking of the hot blast stove shell. Contents of the Invention

[0011] In view of the above situation and to overcome the defects of the prior art, the purpose of the present invention is to provide a method for preventing intergranular stress corrosion and stress corrosion cracking of a hot blast stove shell, which can effectively solve the problem of furnace shell cracking, completely isolate the direct penetration corrosion effect of acid radical corrosive media, and realize the use of high air temperature in a safe, efficient, energy-saving, environmentally friendly and low-cost manner.

[0012] The technical solution adopted by the present invention comprises the following steps: 1) Selection of furnace shell material Select Q345R material or a steel plate with good weldability, high flexibility, and no cracking tendency during processing and production as the furnace shell plate; 2) Scientific calculation of the furnace shell and design before production Determine the resistance, pressure resistance and load-bearing thickness of the furnace shell by using the national standard calculation formula for hot blast stove shells or a comprehensive scientific calculation formula derived from pressure, weld coefficient, corrosion coefficient, included angle coefficient, explosion load and load-bearing capacity, so as to adapt to the high-pressure and high-air-temperature working conditions; 3) Rolling, installation and welding of the furnace shell After the calculation and determination in step 2), perform rolling according to the drawing design, then carry out installation and welding. Implement heating treatment before welding and annealing treatment after welding. Then brush acid-resistant high-temperature paint on the furnace shell in the high-temperature area of the hot blast stove, or the longitudinal and transverse welds and heat-affected zones (20 mm wide welds) of the furnace shell for rust prevention and anti-corrosion treatment. Then add a 0.01-3mm thick stainless steel plate on top by means of inlaying, welding or pasting, and then apply high-temperature acid-resistant paint to seal the gaps of this 0.01-3mm thick stainless steel isolation layer to isolate the corrosive media. Alternatively, spray corrosion-resistant and high-temperature resistant ceramic glaze on the furnace shell in the high-temperature area of the hot blast stove, or the longitudinal and transverse welds and heat-affected zones (20 mm wide welds) of the furnace shell, and use a 800-1000℃ high-temperature spray gun for porcelain firing while spraying, so as to form a ceramic body structure or ceramic layer liner structure inside the welds or the whole furnace shell, completely blocking the passage of corrosive media; 4) Cleaning weld slag corrosion and polishing the welds After welding, the surface oil and slag are treated, and the weld seam is cleaned with a hand-held angle grinder. The rust, dead skin, corrosion and loose material on the steel plate surface at both ends of the weld are cleaned and polished with a hand-held steel wool ball. 5) Cover or weld the weld seam. After applying acid-resistant high-temperature paint to the cleaned weld seam in step 4), cover and inlay or weld the weld seam with a stainless steel plate several times wider than the weld seam (or use a special medium to bond the stainless steel plate to the furnace shell); at the same time, double-wheel rolling is used to make the welded or bonded stainless steel with a special high-temperature medium tightly bonded to the furnace shell to achieve a completely sealed and gapless joint. 6) Acid-resistant treatment After uniform stress relief treatment of the furnace shell welds and inlaid stainless steel plates, the inlaid or welded (or covered with special media) stainless steel plates and edges are coated with a 10cm high-temperature resistant acid-resistant coating for acid prevention. 7) Sealing treatment The upper part of the anti-corrosion treatment zone is connected and welded to the anchor structure at both ends by bridging, so that the subsequent acid-resistant spray coating can firmly adhere to the furnace shell, while also protecting the tightness of the weld and the inlaid stainless steel. 8) Spray coating protection treatment The entire furnace interior is then coated with a 5-10cm layer of acid-resistant paint for protection.

[0013] In step 8), the acid-resistant spray coating has a protective layer of 5-20cm.

[0014] The protective layer consists of absorbent, acid-resistant, and fire-resistant fiber cotton and various refractory bricks. A 65-230mm thick layer of fiber cotton is wrapped around the outside of the acid-resistant spray coating. Then, ordinary lightweight bricks with a density of 0.5-1.2 and a thickness of 114-230mm are laid sequentially for heat insulation, acid isolation, and thermal insulation; high-grade lightweight bricks with a density of 0.8-1.2 and a thickness of 114-230mm are laid for heat insulation, acid isolation, and thermal insulation; finally, a 300-450mm thick layer of high-temperature resistant and acid-resistant silica bricks is laid as an inner lining to comprehensively isolate the high-temperature combustion space from the entire acid-resistant protective layer.

[0015] The existing furnace shell preparation method is as follows: ordinary Q345C low alloy carbon steel is selected, rolled and shaped according to the design drawings, then installed and welded, and annealed. The thickness of the steel shell is calculated by multiplying the furnace shell diameter by an empirical modulus and adding a fixed correction value.

[0016] The calculation formula, which is based on a comprehensive scientific analysis of pressure, weld coefficient, corrosion coefficient, included angle coefficient, explosion load, and load-bearing capacity, is as follows: S = PDi / (2*[σt]*Φ-P) + C (straight section) S = PDi / (2*[σt]*Φ-P)*1 / cosα+C (Transition segment) Where Di is the inner diameter of the cylinder, in mm. [σ]t - Allowable stress of the container component material at the design temperature, MPa C - Wall thickness allowance, mm P - Design pressure (MPa) α - Half vertex angle ° The special medium is a high-temperature, high-strength adhesive.

[0017] This invention is simple, novel, unique, and easy to implement. The method is simple and easy to carry out, with an extremely short manufacturing and processing period. It completely solves the problems of furnace shell cracking and stress corrosion cracking, prevents furnace shell deformation and damage, and can adapt to high-pressure blast temperature conditions. It increases the overall lifespan of the furnace shell by 3-10 times, with a service life of more than 30 years without cracking or any obstacles. It is an innovation in the method of preventing intergranular stress corrosion and stress corrosion cracking of hot blast furnace shells. Detailed Implementation

[0018] The specific embodiments of the present invention will be further described in detail below with reference to examples. Example

[0019] In its specific implementation, this invention includes the following steps: 1) Selection of furnace shell material Select steel plates with good weldability, high flexibility, and resistance to cracking during processing for furnace shell plates; 2) Scientific calculations and pre-fabrication design of the furnace shell The compressive and load-bearing thickness of the furnace shell is determined using the calculation formula of the national hot blast stove shell specification in order to adapt to high pressure and high blast temperature working conditions. 3) Rolling, installation, and welding of the furnace shell After calculating and determining according to step 2), roll and manufacture according to the design drawings, then install and weld. Heat treatment is performed before welding, and annealing treatment is performed after welding. Then, apply acid-resistant high-temperature paint to the furnace shell or the longitudinal and transverse welds of the furnace shell and the heat-affected zone (20 mm wide weld) in the high-temperature zone of the hot blast stove for rust and corrosion prevention. Then, add a 0.01-3 mm stainless steel plate on top for inlay and welding, and then apply high-temperature acid-resistant paint to isolate the corrosive medium and seal the gaps of this 0.01-3 mm stainless steel isolation layer. 4) Clean the weld slag and grind the weld. After welding, the surface oil and slag are treated, and the weld seam is cleaned with a hand-held angle grinder. The rust, dead skin, corrosion and loose material on the steel plate surface at both ends of the weld are cleaned and polished with a hand-held steel wool ball. 5) Cover or weld the weld seam. After applying acid-resistant high-temperature paint to the cleaned weld seam in step 4), cover and inlay or weld the weld seam with a stainless steel plate several times wider than the weld seam width; at the same time, double-wheel rolling is used to press the welded or bonded stainless steel with special high-temperature media to make it tightly bonded to the furnace shell to achieve a completely sealed and gapless joint. 6) Acid-resistant treatment After uniform stress relief treatment of the furnace shell welds and inlaid stainless steel plates, the inlaid or welded stainless steel plates and edges are coated with high-temperature resistant acid-resistant paint for sealing and acid protection. 7) Sealing treatment The upper part of the anti-corrosion treatment zone is connected and welded to the anchor structure at both ends by bridging, so that the subsequent acid-resistant spray coating can firmly adhere to the furnace shell, while also protecting the tightness of the weld and the inlaid stainless steel. 8) Spray coating protection treatment The entire furnace interior is then coated with a 5cm layer of acid-resistant paint for protection. Example

[0020] In its specific implementation, this invention includes the following steps: 1) Selection of furnace shell material Q345R material was selected as the furnace shell material; 2) Scientific calculations and pre-fabrication design of the furnace shell The compressive and load-bearing thickness of the furnace shell is determined by a calculation formula based on pressure, weld coefficient, corrosion coefficient, included angle coefficient, explosion load, and load-bearing comprehensive scientific factors, in order to adapt to high pressure and high wind temperature conditions. 3) Rolling, installation, and welding of the furnace shell After calculating and determining according to step 2), roll and manufacture according to the design drawings, then install and weld. Heat treatment is carried out before welding, and annealing treatment is carried out after welding. Then, corrosion-resistant and high-temperature resistant ceramic glaze is sprayed on the furnace shell or the longitudinal and transverse welds of the furnace shell and the heat-affected zone (20 mm wide weld). While spraying, a high-temperature spray gun at 800-1000℃ is used for vitrification and baking, so that a ceramic body structure or ceramic inner liner structure is formed at the weld or the entire furnace shell, completely isolating the passage of corrosive media. 4) Clean the weld slag and grind the weld. After welding, the surface oil and slag are treated, and the weld seam is cleaned with a hand-held angle grinder. The rust, dead skin, corrosion and loose material on the steel plate surface at both ends of the weld are cleaned and polished with a hand-held steel wool ball. 5) Cover or weld the weld seam. After applying acid-resistant high-temperature paint to the cleaned weld seam in step 4), cover and inlay or weld the weld seam with a stainless steel plate several times wider than the weld seam width; at the same time, double-wheel rolling is used to press the welded or bonded stainless steel with special high-temperature media to make it tightly bonded to the furnace shell to achieve a completely sealed and gapless joint. 6) Acid-resistant treatment After uniform stress relief treatment of the furnace shell welds and inlaid stainless steel plates, the stainless steel plates and edges that have been inlaid, welded or covered with special media are coated with high-temperature resistant acid-resistant paint for acid protection. 7) Sealing treatment The upper part of the anti-corrosion treatment zone is connected and welded to the anchor structure at both ends by bridging, so that the subsequent acid-resistant spray coating can firmly adhere to the furnace shell, while also protecting the tightness of the weld and the inlaid stainless steel. 8) Spray coating protection treatment The entire furnace interior is then coated with an 8cm layer of acid-resistant paint for protection. Example

[0021] In its specific implementation, this invention includes the following steps: 1) Selection of furnace shell material Q345R material was selected as the furnace shell plate. 2) Scientific calculations and pre-fabrication design of the furnace shell The compressive and load-bearing thickness of the furnace shell is determined using the calculation formula of the national hot blast stove shell specification in order to adapt to high pressure and high blast temperature working conditions. 3) Rolling, installation, and welding of the furnace shell After calculating and determining according to step 2), roll and manufacture according to the design drawings, then install and weld. Heat treatment is carried out before welding, and annealing treatment is carried out after welding. Then, corrosion-resistant and high-temperature resistant ceramic glaze is sprayed on the furnace shell or the longitudinal and transverse welds of the furnace shell and the heat-affected zone (20 mm wide weld). While spraying, a high-temperature spray gun at 800-1000℃ is used for vitrification and baking, so that a ceramic body structure or ceramic inner liner structure is formed at the weld or the entire furnace shell, completely isolating the passage of corrosive media. 4) Clean the weld slag and grind the weld. After welding, the surface oil and slag are treated, and the weld seam is cleaned with a hand-held angle grinder. The rust, dead skin, corrosion and loose material on the steel plate surface at both ends of the weld are cleaned and polished with a hand-held steel wool ball. 5) Cover or weld the weld seam. After applying acid-resistant high-temperature paint to the cleaned weld seam in step 4), cover and inlay or weld the weld seam with a stainless steel plate several times wider than the weld seam (or use a special medium to bond the stainless steel plate to the furnace shell); at the same time, double-wheel rolling is used to make the welded or bonded stainless steel with a special high-temperature medium tightly bonded to the furnace shell to achieve a completely sealed and gapless joint. 6) Acid-resistant treatment After uniform stress relief treatment of the furnace shell welds and inlaid stainless steel plates, the inlaid or welded (or covered with special media) stainless steel plates and edges are coated with a 10cm high-temperature resistant acid-resistant coating for acid prevention. 7) Sealing treatment The upper part of the anti-corrosion treatment zone is connected and welded to the anchor structure at both ends by bridging, so that the subsequent acid-resistant spray coating can firmly adhere to the furnace shell, while also protecting the tightness of the weld and the inlaid stainless steel. 8) Spray coating protection treatment The entire furnace interior is then coated with a 10cm layer of acid-resistant paint for protection.

[0022] This invention addresses the cracking of the furnace shell caused by the combined effects of large amounts of nitrogen oxides and other corrosive media generated during the high blast temperatures required in the combustion and blasting periods of hot blast stoves, as well as the penetrating corrosion caused by the combination of water and other corrosive media during these periods. Drawing on the successful experience of using composite plates made of stainless steel and steel plates, combined with the corrosion resistance of stainless steel, this invention effectively isolates the corrosive media inside the furnace. Furthermore, it employs a method of covering and encasing the weld seams with anti-corrosion materials. These materials include stainless steel, ceramic materials, and acid-resistant paints. Under the influence of special media, they cover the weld seams and heat-affected zones, or completely cover them, to thoroughly isolate the corrosive media from the furnace shell or its weld seams, thus completely preventing stress corrosion cracking of the furnace shell.

[0023] Corrosion-resistant steel plates, foils, or stainless steel plates and foils are used. The thickness of the steel foil or plates is 0.1mm or more, and the width is sufficient to cover the weld seam of the furnace shell. The weld seam is covered by adhesive bonding, inlaying, or welding. This method separates the anti-corrosion material from nitrogen oxides and other corrosive media from the furnace shell weld seam, preventing the corrosive media from directly contacting and penetrating the weld seam, thus preventing corrosion and ensuring that the furnace shell will not crack and will have a stable and long service life. This method is simple and easy to implement, with a simple construction process and extremely low cost. It only requires simple welding coverage when welding the steel plates.

[0024] This invention is applicable to furnace shells made of all steel plate materials. Based on the existing furnace shell material, the high-temperature zone of the furnace shell base material is first coated with acid-resistant, high-temperature paint for rust and corrosion prevention. Then, a 0.01-3mm stainless steel plate is added on top (or a layer of ceramic glaze is sprayed on, and simultaneously fired using an 800-1000℃ high-temperature spray gun to create a ceramic inner liner, completely isolating corrosive media). This is done through inlaying, welding, or special media bonding. After completion, an acid-resistant and high-temperature resistant special protective coating is added to the outside. This coating seals the gaps in the 0.01-3mm stainless steel (usually 316L) isolation layer. Then, a 5-10cm layer of acid-resistant coating is sprayed on the outside to cover and wrap the furnace, ensuring the stainless steel layer is tightly sealed between the sprayed coating and the furnace shell, and is tightly bonded to the furnace shell. Another simple and easy method is to... After welding the furnace shell base material, the weld seams and heat-affected areas are coated with acid-resistant high-temperature paint for rust and corrosion prevention. Then, a 0.01-3mm thick stainless steel plate, wider than the weld seam and covering the heat-affected area, is applied over the weld seams and heat-affected areas (or a layer of ceramic glaze is sprayed, and simultaneously fired at 800-1000℃ using a high-temperature spray gun to create a ceramic inner liner, completely isolating the corrosive medium from passing through). This is done by inlaying, welding, or bonding with a special medium. After completion, an acid-resistant and high-temperature resistant special protective coating is added to the outside. This isolation layer material is applied to all weld seams and heat-affected areas to seal the gaps in the 0.01-3mm stainless steel isolation layer. Then, a 5-10cm layer of acid-resistant paint is sprayed over the entire interior of the furnace shell to cover and wrap it, ensuring that the stainless steel layer is tightly sealed between the sprayed coating and the furnace shell, and that the stainless steel strips pressing the seams are tightly bonded to the furnace shell weld seams and heat-affected areas.

[0025] After these measures are implemented, an additional layer of thermal insulation and heat-resistant coating is added to the outside of the sprayed layer to cool and protect the covered areas of the paint and acid-resistant paint. This protective layer is typically 5-20mm thick and serves to protect the acid-resistant layer and absorb the expansion and contraction of the refractory lining. The first layer of fiber cotton is covered by 114mm thick ordinary lightweight bricks for thermal and acid-resistant protection. The second layer is 230mm thick high-grade lightweight bricks for thermal and acid-resistant protection. Finally, in the high-temperature zone of the hot blast stove, a 230-450mm thick layer of high-temperature resistant and acid-resistant silica bricks is constructed to isolate the combustion space and the entire acid-resistant protective layer. At this point, the entire furnace shell's anti-corrosion and high-temperature resistant structure is complete. With these measures, the hot blast stove shell can... To ensure a service life of over 30 years, the method is simple, novel, and unique, with an extremely short manufacturing and processing period. It completely solves the problems of furnace shell cracking and stress corrosion cracking, prevents furnace shell deformation and damage, and can adapt to high-pressure blast temperature conditions. It increases the overall service life of the furnace shell by 3-10 times, while saving investment. It is only equivalent to 10% of the investment, construction period, and total process quality of measures taken for 4800 and 5500 m³ blast furnaces. Its service life is over 30 years without cracking or any obstacles. It can improve blast temperature, increase production capacity, and save more than 100 million yuan in economic losses for extra-large blast furnaces every year. It is an innovation in the method of preventing intergranular stress corrosion and stress corrosion cracking of hot blast stove furnace shells, with good economic and social benefits.

[0026] It should be noted that the above are merely preferred embodiments of the present invention and are not intended to limit the present invention in any way. Any modifications or alterations made by those skilled in the art without departing from the scope of the present invention to create equivalent embodiments based on the disclosed technical content shall fall within the protection scope of the present invention.

Claims

1. A method of preventing intergranular stress corrosion and stress corrosion cracking of a hot blast stove shell, characterized in that Includes the following steps: 1) Selection of furnace shell material Select steel plates with good weldability, high flexibility, and resistance to cracking during processing as furnace shell plates; 2) Scientific calculations and pre-fabrication design of the furnace shell The compressive and load-bearing thickness of the furnace shell is determined by using the calculation formula in the national hot blast stove shell specification or by adopting a calculation formula based on the comprehensive scientific transformation of pressure, weld coefficient, corrosion coefficient, included angle coefficient, explosion load and load-bearing capacity, so as to adapt to high pressure and high blast temperature working conditions. 3) Rolling, installation, and welding of the furnace shell After calculating and determining according to step 2), roll and manufacture according to the design drawings, then install and weld. Heat treatment is performed before welding, and annealing treatment is performed after welding. Then, apply acid-resistant high-temperature paint to the furnace shell or the longitudinal and transverse welds of the furnace shell and the heat-affected zone in the high-temperature zone of the hot blast stove for rust and corrosion prevention. Then, add a 0.01-3mm stainless steel plate on top for inlay, welding or pasting. Then apply acid-resistant high-temperature paint again to seal the gaps of this 0.01-3mm stainless steel isolation layer to isolate the corrosive medium. Alternatively, apply corrosion-resistant and high-temperature resistant ceramic glaze to the furnace shell or the longitudinal and transverse welds of the furnace shell and the heat-affected zone in the high-temperature zone of the hot blast stove. While spraying, use an 800-1000℃ high-temperature spray gun to ceramicize and bake, so that the weld or the entire furnace shell forms a ceramic body structure or ceramic inner liner structure, completely isolating the passage of corrosive media. 4) Clean the weld slag and grind the weld. After welding, surface oil and welding slag are removed. A handheld angle grinder is used to clean the slag corrosion of the weld seam, and a handheld angle grinder with steel wool is used to clean and polish the rust, dead skin, corrosion and loose material on the surface of the steel plate at both ends of the weld seam. 5) Inlaying, welding, or pasting the weld seam. After the weld seam in step 4) is cleaned and treated with acid-resistant high-temperature paint, a stainless steel plate several times wider than the weld seam is used to cover and inlay the weld seam, or weld it, or a special medium is used to bond the stainless steel plate to the furnace shell; at the same time, the welded or bonded stainless steel is double-rolled to make it tightly bonded to the furnace shell to achieve a completely sealed and gapless joint. 6) Acid-resistant treatment After uniform stress relief treatment of the furnace shell welds and inlaid stainless steel plates, the inlaid, welded, or specially coated stainless steel plates and edges are sealed with a 10cm high-temperature resistant acid-resistant coating for acid protection. 7) Sealing treatment In step 6), the upper part of the acid-resistant treatment strip is connected and welded to the anchoring structure at both ends by bridging, so that the subsequent acid-resistant spray coating is firmly attached to the furnace shell, while also protecting the tightness of the covering weld and the inlaid stainless steel. 8) Spray coating protection treatment The entire furnace interior is then coated with a 5-10cm layer of acid-resistant paint for protection.

2. The method for preventing intergranular stress corrosion and stress corrosion cracking of hot blast stove shell according to claim 1, characterized in that, In step 8), the acid-resistant spray coating has a protective layer of 5-20cm.

3. The method for preventing intergranular stress corrosion and stress corrosion cracking of hot blast stove shell according to claim 2, characterized in that, The protective layer consists of absorbent, acid-resistant, and fire-resistant fiber cotton and various refractory bricks. A 65-230mm thick layer of fiber cotton is wrapped around the outside of the acid-resistant spray coating. Then, ordinary lightweight bricks with a density of 0.5-1.2 and a thickness of 114-230mm are laid sequentially for heat insulation, acid isolation, and thermal insulation; high-grade lightweight bricks with a density of 0.8-1.2 and a thickness of 114-230mm are laid for heat insulation, acid isolation, and thermal insulation; finally, a 300-450mm thick layer of high-temperature resistant and acid-resistant silica bricks is laid as an inner lining to comprehensively isolate the high-temperature combustion space from the entire acid-resistant protective layer.

4. The method for preventing intergranular stress corrosion and stress corrosion cracking of hot blast stove shell according to claim 1, characterized in that, The calculation formula, based on a comprehensive scientific analysis of pressure, weld coefficient, corrosion coefficient, included angle coefficient, explosion load, and load-bearing capacity, is as follows: For the straight section, S = PDi / (2*[σt]*Φ-P) + C Transition segment S = PDi / (2*[σt]*Φ-P)*1 / cosα+C Where Di is the inner diameter of the cylinder, in mm. [σ]t - Allowable stress of the container component material at the design temperature, MPa C - Wall thickness allowance, mm P - Design pressure (MPa) α - Half vertex angle ° Φ - Weld coefficient.

5. The method for preventing intergranular stress corrosion and stress corrosion cracking of hot blast stove shell according to claim 1, characterized in that, The special medium is a high-temperature, high-strength adhesive.

Citation Information

Patent Citations

  • Method for preventing intergranular stress corrosion of vault of hot blast heater

    CN101603108A

  • Acid-resisting coating composition for ironmaking blast-furnace hot blast stove and using method thereof