Lithium supplement and preparation method thereof, positive electrode material and lithium ion battery
By using a combination of lithium-rich particles and heteroatom-doped carbon quantum dots supporting single-atom catalysts in the lithium replenishing agent, the problems of poor catalyst dispersion and high decomposition potential in the existing technology are solved, and the high capacity and high decomposition potential of lithium-ion batteries are achieved. Long cycle performance.
Patent Information
- Application Number
- CN202311689996.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-08
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-12-08
AI Technical Summary
The decomposition potential of existing lithium replenishing agents is high, and the catalyst is difficult to disperse well in the cathode material, resulting in low catalytic efficiency and inability to effectively reduce the decomposition potential, which limits the energy density and cycle stability of lithium-ion batteries.
A combination of lithium-rich particles and heteroatom-doped carbon quantum dots loaded with single-atom catalysts is used to form an efficient lithium replenishing agent through ball milling and sintering processes. The single-atom catalyst is dispersed on the carbon quantum dots to form π-π stacking, which improves the catalyst and The contact area of lithium-rich particles reduces the decomposition potential.
It significantly reduces the decomposition potential of the lithium supplement agent, improves the first irreversible capacity compensation capability of the lithium-ion battery, improves the energy density and cycle stability of the battery, and enables the lithium-ion battery to have high capacity and long cycle characteristics.
Smart Images

Figure CN117525635B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium supplement and a preparation method thereof, a positive electrode material and a lithium ion battery. Background Art
[0002] During the first charging process of a lithium-ion battery, a large amount of solid electrolyte interface film will be produced on the surface of the negative electrode of the battery, which consumes the limited lithium ions and electrolyte in the battery, causing irreversible capacity loss, reducing the energy density of the lithium-ion secondary battery, and limiting the application of lithium-ion batteries. In the prior art, by adding a positive electrode lithium supplement to the positive electrode material, the first irreversible capacity loss of the lithium battery can be effectively compensated. However, the decomposition potential of common lithium supplements is relatively high, and it is necessary to charge to a higher voltage during the first cycle of charging to exert its lithium supplement capacity. In order to reduce the decomposition voltage of the lithium supplement, the use of a catalyst is a more effective means. However, the introduction of the catalyst in the existing lithium supplement adopts a direct mixing technical means, which makes it difficult to achieve a good dispersion of the catalyst in the lithium supplement. There is a problem that the catalyst has a low catalytic efficiency and accounts for too much, and the decomposition potential of the lithium supplement cannot be effectively reduced. Therefore, it is necessary to improve the catalytic efficiency of the catalyst in the lithium supplement, enhance the lithium supplement efficiency, and thus improve the energy density and cycle stability of the battery. Summary of the invention
[0003] Based on this, the embodiment of the present invention provides a lithium supplement agent and a preparation method, a positive electrode material and a lithium ion battery. The catalyst introduced in the lithium supplement agent has good contact with the lithium-rich particles, high catalytic efficiency, can effectively reduce the decomposition potential of the lithium supplement agent, has a good lithium supplement effect, and is applied to lithium ion batteries. It can efficiently compensate for the first irreversible capacity loss of the lithium battery, so that the lithium ion battery has the characteristics of high capacity and long cycle, and improves the overall electrochemical performance of the battery.
[0004] In a first aspect, an embodiment of the present invention provides a lithium supplement, comprising lithium-rich particles and heteroatom-doped carbon quantum dots loaded with a single-atom catalyst and loaded on the lithium-rich particles.
[0005] In an embodiment of the present invention, the mass ratio of the lithium-rich particles to the single-atom catalyst is 100:(0.2-1); the mass ratio of the lithium-rich particles in the lithium supplement is 86%-95%.
[0006] In an embodiment of the present invention, the lithium-rich particles include secondary particles, and the secondary particles include an inner core agglomerated by multiple primary particles; wherein the heteroatom-doped carbon quantum dots loaded with single-atom catalysts are located in the grain boundaries between the primary particles and / or on the surface of the secondary particles.
[0007] In an embodiment of the present invention, π-π stacking is formed between the lithium-rich particles and the heteroatom-doped carbon quantum dots loaded with single-atom catalysts.
[0008] In an embodiment of the present invention, the particle size D50 of the inner core is 5 μm-50 μm.
[0009] In an embodiment of the present invention, the secondary particles further include a coating layer located on the surface of the inner core, and the material of the coating layer includes heteroatom-doped carbon quantum dots and / or carbon-based materials loaded with single-atom catalysts.
[0010] In an embodiment of the present invention, the lithium-rich particles include one or more of a ternary lithium-supplementing material, a binary lithium-supplementing material and an organic lithium-supplementing material.
[0011] In an embodiment of the present invention, the organic lithium supplement material includes one or more of Li2DHBN, Li2C2O4, Li2C4O4 and Li2C6O6.
[0012] In an embodiment of the present invention, the single atom catalyst includes one or more of a nickel atom, a cobalt atom and a zinc atom; and / or the heteroatom includes one or more of N, S, P and B.
[0013] In the lithium supplement agent provided by the embodiment of the present invention, the single-atom catalyst is loaded on the heteroatom-doped carbon quantum dots, and can be dispersed on the surface of the lithium-rich particles with the help of the effective diffusivity of the heteroatom-doped carbon quantum dots. In particular, it can be combined between the interfaces of the lithium-rich particles in the process of agglomeration to form secondary particles. The contact area with the lithium-rich particles is large, the catalytic efficiency is high, the decomposition potential of the lithium supplement agent can be effectively reduced, and the lithium supplement effect is good. When applied to lithium-ion batteries, it can efficiently compensate for the first irreversible capacity loss of the lithium battery, so that the lithium-ion battery has the characteristics of high capacity and long cycle, and the overall electrochemical performance of the battery is improved.
[0014] In a second aspect, an embodiment of the present invention provides a method for preparing a lithium supplement, comprising:
[0015] placing the carbon quantum dots in an atmosphere of an inert gas and a heteroatom source gas for heat treatment to obtain heteroatom-doped carbon quantum dots;
[0016] Dispersing the heteroatom-doped carbon quantum dots in a single-atom catalyst salt solution containing an alkali to carry out a complex reaction, thereby obtaining heteroatom-doped carbon quantum dots loaded with single-atom catalyst ions;
[0017] Placing the heteroatom-doped carbon quantum dots loaded with single-atom catalyst ions in a reducing gas atmosphere for reduction reaction to obtain heteroatom-doped carbon quantum dots loaded with single-atom catalysts;
[0018] The lithium-rich particles and the heteroatom-doped carbon quantum dots loaded with single-atom catalysts are ball-milled and sintered to obtain a lithium supplement agent, which includes lithium-rich particles and heteroatom-doped carbon quantum dots loaded with single-atom catalysts loaded on the lithium-rich particles.
[0019] The preparation method of the lithium supplement provided by the embodiment of the present invention has simple process, convenient operation, and is conducive to the use of the lithium supplement.
[0020] In a third aspect, an embodiment of the present invention provides a positive electrode material, including a positive electrode active material and a lithium supplement material, wherein the lithium supplement material includes the lithium supplement agent described in the first aspect or the lithium supplement agent prepared by the preparation method described in the second aspect.
[0021] The positive electrode material provided by the embodiment of the present invention contains the lithium supplement agent in any of the above embodiments. The lithium supplement agent has high lithium supplement efficiency and can effectively alleviate the capacity decay, so that the obtained positive electrode material has good cycle stability, further improving the performance of the lithium ion battery.
[0022] In a fourth aspect, an embodiment of the present invention provides a lithium-ion battery, comprising a positive electrode, a negative electrode, and a separator and an electrolyte located between the positive electrode and the negative electrode, wherein the positive electrode comprises the positive electrode material described in the third aspect.
[0023] The lithium ion battery provided by the embodiment of the present invention contains the lithium supplement agent in any of the above-mentioned embodiments, which can effectively compensate for the first irreversible capacity loss of the lithium battery, so that the obtained lithium ion battery has the characteristics of high capacity and long cycle, improves the overall electrochemical performance of the battery, and is conducive to wide use. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings required to be used in the embodiment of the present invention will be described below.
[0025] Figure 1 is a schematic diagram of the distribution of heteroatom-doped carbon quantum dots loaded with single-atom catalysts on secondary particles in one embodiment of the present invention;
[0026] Figure 2 is a schematic cross-sectional view of heteroatom-doped carbon quantum dots loaded with single-atom catalysts in one embodiment of the present invention;
[0027] Figure 3 is a schematic cross-sectional view of a secondary particle in one embodiment of the present invention. DETAILED DESCRIPTION
[0028] The embodiments of the present invention are described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0029] In recent years, the rapid development of portable electronic products, new energy vehicles, smart grids, distributed energy storage, and the Internet of Things has continuously put forward higher requirements for the performance of lithium-ion batteries, among which the improvement of battery energy density is the most urgent. Lithium-ion battery lithium supplementation technology is an important means to improve battery energy density. During the formation process of lithium-ion batteries, SEI growth on the negative electrode surface will consume active lithium, resulting in battery energy loss. The lithium supplementation technology can compensate for active lithium and achieve the effect of improving the energy density of lithium-ion batteries. At present, the decomposition potential of common lithium supplements is relatively high, and it is necessary to charge to a higher voltage during the first cycle of charging to exert its lithium supplement capacity, which seriously limits the application of lithium supplements. In order to reduce the high decomposition voltage of lithium supplements, the use of catalysts is a more effective means. However, the existing technical means have the problem that the catalyst catalytic efficiency is low and the decomposition potential of the lithium supplement cannot be effectively reduced. Therefore, it is necessary to improve the catalytic efficiency of the catalyst in the lithium supplement and enhance the lithium supplement efficiency, thereby improving the energy density and cycle stability of the battery.
[0030] Based on this, an embodiment of the present invention provides a lithium supplement, including lithium-rich particles and heteroatom-doped carbon quantum dots loaded with a single-atom catalyst and loaded on the lithium-rich particles.
[0031] Carbon Quantum Dots (CQDs) are a type of zero-dimensional carbon nanomaterials, consisting of ultrafine, dispersed, quasi-spherical carbon nanoparticles with a size less than 10nm. In the lithium supplement provided by the embodiment of the present invention, the single-atom catalyst is loaded on the heteroatom-doped carbon quantum dots, which can be dispersed on the surface of lithium-rich particles with the help of the effective diffusivity of the carbon quantum dots, and can be combined between the interfaces of lithium-rich primary particles in the process of agglomeration of lithium-rich primary particles to form secondary particles. The contact area with the lithium-rich particles is large, the catalytic efficiency is high, and the decomposition potential of the lithium supplement can be effectively reduced, so as to promote the decomposition of the lithium supplement to release more active lithium, and better compensate for the irreversible active lithium loss of the battery. At the same time, the lithium supplement agent has a stable structure and good cycle performance. Specifically, the single-atom catalyst is combined with multiple doped heteroatoms in the heteroatom-doped carbon quantum dots, and the structure is stable. At the same time, the heteroatom-doped carbon quantum dots loaded with single-atom catalysts can be complexed with lithium-rich particles through π-π action, so that the heteroatom-doped carbon quantum dots loaded with single-atom catalysts and the lithium-rich particles have a strong binding effect, which is not easy to fall off during use, which is conducive to the lithium supplement agent in the process of composite positive electrode material homogenization. It can maintain close contact with the catalyst, and then catalyze the lithium supplement agent with high decomposition voltage, reducing its decomposition voltage. Furthermore, the heteroatom-doped carbon quantum dots have good electrical conductivity, which is conducive to accelerating the electron mobility rate and the migration rate of lithium ions in the lithium supplement agent, thereby improving the lithium supplement efficiency of the lithium supplement agent. The lithium supplement agent provided in the embodiment of the present invention has good lithium supplement efficiency, and is applied to lithium ion batteries, which can efficiently compensate for the first irreversible capacity loss of lithium batteries, so that lithium ion batteries have the characteristics of high capacity and long cycle, and improve the overall electrochemical performance of the battery.
[0032] In an embodiment of the present invention, the mass ratio of lithium-rich particles and single-atom catalysts can be 100:(0.2-1). The catalyst in the lithium supplement provided by the embodiment of the present invention has good catalytic efficiency. The decomposition voltage of the lithium supplement can be reduced by using a small amount of catalyst. The mass ratio of lithium-rich particles and single-atom catalysts is set to 100:(0.2-1), which can effectively reduce the decomposition voltage of the lithium supplement and avoid the problem of reduced lithium supplement capacity due to excessive proportion of catalyst. In some embodiments, the mass ratio of lithium-rich particles and single-atom catalysts can be 100:0.2, 100:0.3, 100:0.4, 100:0.5, 100:0.6, 100:0.7, 100:0.8, 100:0.9 or 100:1.
[0033] In an embodiment of the present invention, the mass proportion of lithium-rich particles in the lithium supplement agent can be 86%-95%. The mass proportion of lithium-rich particles in the lithium supplement agent is relatively high, and the lithium supplement agent has a high lithium supplement capacity, which can release more active lithium ions to compensate for the irreversible capacity loss of the battery. In some embodiments, the mass proportion of lithium-rich particles in the lithium supplement agent can be 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94% or 95%.
[0034] In an embodiment of the present invention, the lithium-rich particles include secondary particles, and the secondary particles include a core agglomerated by a plurality of primary particles; wherein the heteroatom-doped carbon quantum dots loaded with a single-atom catalyst are located in the grain boundaries between the primary particles and / or on the surface of the secondary particles, and a π-π stacking is formed between the lithium-rich particles and the heteroatom-doped carbon quantum dots loaded with a single-atom catalyst. The term "grain boundary" as used herein refers to the interface between two adjacent primary particles, and here, the interface between the primary particles exists in the secondary particles; "primary particles" refer to particles agglomerated to form secondary particles, and the primary particles may have any suitable shape, including rod-like or rectangular shapes; "secondary particles" refer to particles that include agglomerates of a plurality of primary particles and do not include other non-lithium-rich particles, and the secondary particles may have a spherical shape.
[0035] In a specific embodiment, Figure 1 As shown, the lithium supplement includes secondary particles 110 and heteroatom-doped carbon quantum dots 10 loaded with single-atom catalysts, wherein the secondary particles 110 are cores 111 formed by agglomeration of multiple primary particles 100, and the heteroatom-doped carbon quantum dots 10 loaded with single-atom catalysts are located in the grain boundaries between the primary particles 100 and on the surface of the secondary particles 110, and the multiple primary particles 100 may have the same particle size or different particle sizes. In some embodiments, as Figure 2 As shown, the heteroatom-doped carbon quantum dots 10 loaded with single-atom catalysts are composed of heteroatom-doped carbon quantum dots 12 and single-atom catalysts 11 loaded on the surface of the heteroatom-doped carbon quantum dots 12. The heteroatom-doped carbon quantum dots 10 loaded with single-atom catalysts are small in size (<10 nm), and can not only be dispersed on the surface of the secondary particles 110, but also enter the grain boundaries between the primary particles 100. The contact area between the heteroatom-doped carbon quantum dots 10 loaded with single-atom catalysts and the secondary particles 110 is large, which is beneficial to improving the catalytic efficiency of the single-atom catalyst.
[0036] In an embodiment of the present invention, the particle size D50 of the core 111 may be 5 μm-50 μm, which not only ensures the dispersion of the single-atom catalyst on the surface of the secondary particles and the grain boundary between the primary particles, but also facilitates processing. In some embodiments, the particle size D50 of the core 111 may be 5 μm, 8 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm or 50 μm.
[0037] In an embodiment of the present invention, the secondary particles further include a coating layer located on the surface of the inner core. The coating layer can improve the stability of the lithium supplement, increase the diffusion rate of lithium ions, and protect lithium ions from oxidation reactions, thereby improving battery performance and life.
[0038] In a specific embodiment, Figure 3 As shown, the secondary particle 110 includes a core 111 and a coating layer 112 disposed on the core.
[0039] In an embodiment of the present invention, the material of the coating layer may include heteroatom-doped carbon quantum dots loaded with single-atom catalysts, which can not only increase the contact area between the single-atom catalysts and the lithium-rich particles and improve the catalytic efficiency of the single-atom catalysts, but also improve the structural stability of the lithium supplement and extend the service life of the lithium supplement.
[0040] In an embodiment of the present invention, the material of the coating layer may include a carbon-based material, which has high conductivity and chemical stability, can improve the conductivity and ion diffusion rate of the lithium supplement particles, promote the migration of lithium ions in the electrode material, and thus improve the charge and discharge performance and power density of the battery. In some embodiments, the carbon-based material may be graphene, carbon nanotubes, carbon fibers, amorphous carbon, carbon black, or mesoporous carbon.
[0041] The coating layer can be one material including heteroatom-doped carbon quantum dots loaded with single-atom catalysts and carbon-based materials, or it can be multiple materials. The multiple materials can form a mixed material layer or a stacked multilayer structure.
[0042] In the embodiments of the present invention, the lithium-rich particles can be one or more of ternary lithium supplement materials, binary lithium supplement materials, and organic lithium supplement materials. Among them, the ternary lithium supplement material is a material mainly composed of a compound containing three elements and lithium element, and other trace elements can be doped. For example, it can be a material mainly composed of a lithium salt of a transition metal oxide, or a material such as lithium nickel cobalt manganate (NCM) that contains three main elements in addition to the lithium element. When no other trace elements are doped, "ternary" refers to three elements: lithium, transition metal, and oxygen. When other trace elements are doped, "ternary" can be a combination of more than three elements in addition to the lithium element; similarly, the binary lithium supplement material is a material mainly composed of a compound containing two elements and lithium element, and other trace elements can be doped. When other trace elements are doped, "binary" can be a combination of more than two elements in addition to the lithium element. For another example, the chemical formula of the ternary lithium supplement material can be Li x A y O z , where A is one or more elements among Fe, Ni, Mn, Cu, Zn, Co, Cr, Zr, Sb, Ti, V, Mo, and Sn, 2≤x≤8, 0<y, 0<z<7. The chemical formula of the binary lithium supplement material can be Li w B, where B includes at least one element among C, N, O, P, S, F, B, and Se, 0<w≤5. If a catalyst is needed to reduce the decomposition voltage in these lithium supplement materials, this method can be used; the organic lithium supplement material can include one or more of Li2DHBN, Li2C2O4, Li2C4O4, and Li2C6O6. The lithium supplement specific capacity of the lithium-rich particles provided by the embodiments of the present invention is high and the stability is good. In some embodiments, the lithium-rich particles can be Li6CoO4, Li5FeO4, LiCoO2, LiMn2O4, LiNi 0.5 Mn 1.5 O4, Li2NiO2, Li2O, Li2O2, LiF, Li2S, Li3N, Li3B, Li3P, or Li2Se particles. Especially for lithium supplement agents with high decomposition voltages, such as Li2C2O4 and Li2O, etc., they have high specific capacities per gram, but the decomposition voltages are relatively high. Therefore, using the catalyst in this solution can effectively improve the catalytic efficiency and reduce the decomposition voltage.
[0043] In the embodiments of the present invention, the single-atom catalyst can be one or more of nickel atoms, cobalt atoms, and zinc atoms. The single-atom catalyst provided by the embodiments of the present invention can effectively reduce the decomposition potential of the lithium supplement agent, accelerate the release of active lithium from the lithium supplement agent, and efficiently make up for the irreversible lithium loss in the battery.
[0044] In the embodiment of the present invention, the heteroatom includes one or more of N, S, P and B. Introducing the above heteroatoms into the lattice of carbon quantum dots can not only enhance the binding force between the single-atom catalyst and the carbon quantum dots, improve the structural stability of the lithium supplement agent, but also increase the conductivity and electron transfer rate of the carbon quantum dots, thereby improving the lithium supplement efficiency of the lithium supplement agent.
[0045] The present invention also provides a method for preparing the lithium supplement agent of any of the above embodiments, comprising:
[0046] S1, placing the carbon quantum dots in an atmosphere of inert gas and heteroatom source gas for heat treatment to obtain heteroatom-doped carbon quantum dots;
[0047] S2, dispersing the heteroatom-doped carbon quantum dots in a single-atom catalyst salt solution containing an alkali to carry out a complex reaction, thereby obtaining heteroatom-doped carbon quantum dots loaded with single-atom catalyst ions;
[0048] S3, placing the heteroatom-doped carbon quantum dots loaded with single-atom catalyst ions in a reducing gas atmosphere for reduction reaction to obtain heteroatom-doped carbon quantum dots loaded with single-atom catalysts;
[0049] S4. Ball-milling and sintering the lithium-rich particles and the heteroatom-doped carbon quantum dots loaded with single-atom catalysts to obtain a lithium supplement, which includes lithium-rich particles and heteroatom-doped carbon quantum dots loaded with single-atom catalysts loaded on the lithium-rich particles.
[0050] The preparation method provided by the embodiment of the present invention has simple process, convenient operation and is conducive to the use of lithium supplement.
[0051] In an embodiment of the present invention, in step S1, the temperature of the heat treatment may be 400°C-700°C, and the time may be 2h-6h, which is beneficial to heteroatom doping and avoids the formation of by-products. In some embodiments, the temperature of the heat treatment may be 400°C, 450°C, 500°C, 550°C, 600°C, 650°C or 700°C, and the time of the heat treatment may be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h.
[0052] In an embodiment of the present invention, the single-atom catalyst salt solution may be NiSO4, CoSO4, ZnSO4, NiCl2, CoSO4, ZnSO4, Ni(NO3)2, Co(NO3)2 or Zn(NO3)2, and the raw materials are cheap and readily available, which is conducive to reducing the preparation cost. In some embodiments, the concentration of the single-atom catalyst salt solution may be 0.1mol / L-1mol / L, which is conducive to the rapid progress of the complex reaction and avoids the waste of raw materials. In some embodiments, the concentration of the single-atom catalyst salt solution may be 0.1mol / L, 0.2mol / L, 0.3mol / L, 0.4mol / L, 0.5mol / L, 0.6mol / L, 0.7mol / L, 0.8mol / L, 0.9mol / L or 1mol / L.
[0053] In the embodiment of the present invention, the base can be sodium hydroxide or potassium hydroxide. The base provides hydroxide ions to neutralize the positive charge of the ions, thereby making it easier to combine with the ligand, which is conducive to the rapid progress of the complexation reaction.
[0054] In an embodiment of the present invention, the reducing gas may be H2, CO or CH4, the temperature of the reduction reaction may be 300°C-700°C, and the time of the reduction reaction may be 2h-6h, which is conducive to the rapid progress of the reduction reaction and avoids the occurrence of side reactions. In some embodiments, the temperature of the reduction reaction may be 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C or 700°C, and the time of the reduction reaction may be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h.
[0055] In an embodiment of the present invention, in step S4, the feed mass ratio of lithium-rich particles and heteroatom-doped carbon quantum dots loaded with single-atom catalysts can be 100:(5-16), which is conducive to the full mixing of lithium-rich particles and heteroatom-doped carbon quantum dots loaded with single-atom catalysts, and does not cause waste of raw materials. In some embodiments, the feed mass ratio of lithium-rich particles and heteroatom-doped carbon quantum dots loaded with single-atom catalysts can be 100:5, 100:6, 100:7, 100:8, 100:9, 100:10.5, 100:12, 100:13, 100:14, 100:15 or 100:16.
[0056] In the embodiment of the present invention, in step S4, the ball-to-material ratio is (7-10):1, and the ball-to-material ratio refers to the ratio of the mass of the grinding body (steel balls, steel rods, gravel, etc.) in the ball mill to the mass of the material to be ground. Setting the ball-to-material ratio to (7-10):1 is conducive to the full refinement and mixing of lithium-rich particles and heteroatom-doped carbon quantum dots loaded with single-atom catalysts without causing energy loss. In some embodiments, the ball-to-material ratio can be 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1 or 10:1.
[0057] In an embodiment of the present invention, in step S4, the ball milling rate may be 150 rpm-300 rpm, which is conducive to sufficient mixing of the lithium-rich particles and the heteroatom-doped carbon quantum dots loaded with the single-atom catalyst. In some embodiments, the ball milling rate may be 150 rpm, 180 rpm, 200 rpm, 250 rpm, 280 rpm or 300 rpm.
[0058] In an embodiment of the present invention, in step S4, the sintering temperature may be 250°C-550°C, and the sintering time may be 2h-6h, which can improve the strength of the obtained lithium supplement. In some embodiments, the sintering temperature may be 250°C, 300°C, 350°C, 400°C, 450°C, 500°C or 550°C, and the sintering time may be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h.
[0059] The embodiment of the present invention further provides a positive electrode material, including a positive electrode active material and a lithium supplement material, wherein the lithium supplement material includes the lithium supplement agent in any of the above embodiments or the lithium supplement agent prepared by the preparation method in any of the above embodiments.
[0060] In an embodiment of the present invention, the positive electrode material may include components such as a positive electrode active material, a lithium supplement, a conductive agent, and a binder. The present invention does not specifically limit these materials, and suitable materials can be selected according to actual application requirements. The positive electrode active material may be a phosphate positive electrode active material and a ternary positive electrode active material. In some embodiments, it includes one or more of lithium cobaltate, lithium manganate, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, fluorolithium vanadium phosphate, lithium titanate, lithium nickel cobalt manganate, and lithium nickel cobalt aluminum. The conductive agent includes one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, and carbon nanotubes. The type of binder may include one or more of polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan, and chitosan derivatives.
[0061] The positive electrode material provided by the embodiment of the present invention contains the above-mentioned lithium supplement agent, which can effectively alleviate the attenuation of capacity, so that the obtained positive electrode material has good cycle stability, and further improves the performance of the lithium ion battery.
[0062] An embodiment of the present invention further provides a lithium-ion battery, comprising a positive electrode, a negative electrode, and a separator and an electrolyte located between the positive electrode and the negative electrode, wherein the positive electrode comprises the positive electrode material in any of the above embodiments.
[0063] The lithium ion battery provided by the embodiment of the present invention contains the above-mentioned lithium supplement agent, which can effectively compensate for the first irreversible capacity loss of the lithium battery, so that the obtained lithium ion battery has the characteristics of high capacity and long cycle, improves the overall electrochemical performance of the battery, and is conducive to wide use.
[0064] The technical solution of the present application is further illustrated below through specific embodiments and comparative examples.
[0065] Example 1
[0066] 10g of carbon quantum dots were annealed at 500℃ for 2h in NH3 / Ar atmosphere for nitrogen doping; the obtained nitrogen-doped carbon quantum dots were then dispersed in 1mol / L Ni2SO4 solution, and then sodium hydroxide solution was added to make Ni + The obtained product was complexed with nitrogen-doped carbon quantum dots and precipitated; after the precipitate was dried, it was reduced at 600°C in a H2 atmosphere for 4 hours to obtain nitrogen-doped carbon quantum dots loaded with nickel atom catalyst; finally, the nitrogen-doped carbon quantum dots loaded with nickel atom catalyst were ball-milled with 100g of lithium oxalate (Li2C2O4) particles to obtain lithium oxalate (Li2C2O4) primary particles, and sintered at 500°C for 4 hours to agglomerate the lithium oxalate (Li2C2O4) primary particles to form secondary particles. During the agglomeration process, the nitrogen-doped carbon quantum dots loaded with nickel atom catalyst were combined with the grain boundaries between the lithium oxalate (Li2C2O4) primary particles and the surfaces of the secondary particles to finally obtain a lithium supplement having a particle size D50 of 20μm. The mass ratio of lithium oxalate (Li2C2O4) particles, nitrogen-doped carbon quantum dots and nickel atom catalyst in the lithium supplement was 100:10:0.5.
[0067] Example 2
[0068] The difference from Example 1 is that the mass ratio of lithium oxalate (Li2C2O4) particles, nitrogen-doped carbon quantum dots and nickel atom catalyst in the lithium supplement is 100:15:1.
[0069] Example 3
[0070] The difference from Example 1 is that the mass ratio of lithium oxalate (Li2C2O4) particles, nitrogen-doped carbon quantum dots and nickel atom catalyst in the lithium supplement is 100:5:0.2.
[0071] Example 4
[0072] 10g of carbon quantum dots were annealed at 500℃ for 2h in NH3 / Ar atmosphere for nitrogen doping; the obtained nitrogen-doped carbon quantum dots were then dispersed in 1mol / L Ni2SO4 solution, and then sodium hydroxide solution was added to make Ni + The nitrogen-doped carbon quantum dots were complexed and precipitated; the precipitate was dried and reduced at 600℃ in H2 atmosphere for 4h to obtain the nitrogen-doped carbon quantum dots loaded with nickel atom catalyst; the nitrogen-doped carbon quantum dots loaded with nickel atom catalyst were ball-milled with 100g of lithium oxalate (Li2C2O4) particles to obtain lithium oxalate (Li2C2O4) primary particles, and sintered at 500℃ for 4h to agglomerate the lithium oxalate (Li2C2O4) primary particles to form secondary particles. During the agglomeration process, the nitrogen-doped carbon quantum dots loaded with nickel atom catalyst were combined with the grain boundaries between the lithium oxalate (Li2C2O4) primary particles and the surface of the secondary particles. The particle size D50 of the secondary particles was 25μm, and the mass ratio of lithium oxalate (Li2C2O4) particles, nitrogen-doped carbon quantum dots and nickel atom catalyst in the secondary particles was 100:10:0.5. Finally, the obtained secondary particles were mixed with 20g of glucose and carbonized at 800℃ for 4h to obtain carbon-coated lithium supplement.
[0073] Example 5
[0074] The difference from Example 1 is that an equal amount of cobalt atom catalyst is used to replace the nickel atom catalyst in Example 1, and the mass ratio of lithium oxalate (Li2C2O4) particles, nitrogen-doped carbon quantum dots and cobalt atom catalyst in the prepared lithium supplement is 100:10:0.5.
[0075] Example 6
[0076] The difference from Example 1 is that the mass ratio of lithium oxalate (Li2C2O4) particles, carbon quantum dots and nickel atom catalyst is 100:1:0.1.
[0077] Comparative Example 1
[0078] The difference from Example 1 is that the lithium supplement contains only lithium oxalate (Li2C2O4) particles, and does not contain nitrogen-doped carbon quantum dots and nickel atom catalysts.
[0079] Comparative Example 2
[0080] The difference from Example 1 is that the mass ratio of lithium oxalate (Li2C2O4) particles and nitrogen-doped carbon quantum dots in the lithium supplement is 100:10, and no nickel atom catalyst is contained.
[0081] Comparative Example 3
[0082] The difference from Example 1 is that the nitrogen-doped carbon quantum dots loaded with nickel atom catalyst and lithium oxalate (Li2C2O4) particles are not mixed and ball-milled and sintered, but are directly physically mixed to obtain a lithium supplement. The mass ratio of lithium oxalate (Li2C2O4) particles, nitrogen-doped carbon quantum dots and nickel atom catalyst in the lithium supplement is 100:10:0.5.
[0083] The lithium supplements of Examples 1-6 and Comparative Examples 1-3 of the present invention were subjected to electrochemical performance tests:
[0084] The lithium supplement provided in the above examples 1-6 and the lithium supplement provided in the comparative examples 1-3 are respectively assembled into a positive electrode and a lithium ion battery according to the following method:
[0085] Positive electrode: The lithium supplement agent, polyvinylidene fluoride and special high conductive carbon black (SP-Li) were mixed with ball mill in a mass ratio of 80:8:12 to obtain a positive electrode slurry, and the positive electrode slurry was coated on the surface of aluminum foil, vacuum dried at 110°C overnight, and roller pressed to obtain a positive electrode sheet;
[0086] Negative electrode: Graphite, carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR) and conductive carbon black (SP) were mixed in a mass ratio of 95.8:1.2:2:1, and the mixture was ball-milled and stirred to obtain a negative electrode slurry. The negative electrode slurry was coated on the surface of copper foil, and vacuum dried at 110°C overnight to obtain a negative electrode sheet.
[0087] Electrolyte: Ethylene carbonate and ethyl methyl carbonate are mixed in a volume ratio of 3:7, and LiPF6 is added to form an electrolyte with a concentration of LiPF6 of 1 mol / L. In addition, some electrolyte additives are added, and the electrolyte can withstand a high voltage of 4.9V;
[0088] Diaphragm: Polypropylene microporous separator;
[0089] Lithium-ion battery assembly: Assemble button-type lithium-ion full batteries in an inert atmosphere glove box in the order of graphite negative electrode sheet - separator - electrolyte - positive electrode sheet.
[0090] Electrochemical performance test:
[0091] The electrochemical performance of each lithium ion battery assembled in the above lithium ion battery embodiment was tested as shown in Table 1, and the test conditions were as follows:
[0092] Constant current and constant voltage charging, the first cycle charging and discharging voltage is 2.0V-4.9V, the current is 0.1C, the cut-off current is 0.01C, and the charging cut-off voltage is 4.9V.
[0093] The test results of the lithium batteries of the above embodiments and comparative examples are shown in Table 1 below.
[0094] Table 1 Electrochemical performance test results
[0095] Serial number First charge specific capacity (mAh / g) <![CDATA[De-lithiation decomposition potential (V vs. Li + / Li)]]> Example 1 480 4.3 Example 2 421 4.1 Example 3 446 4.5 Example 4 437 4.3 Example 5 467 4.2 Example 6 413 4.7 Comparative Example 1 371 4.9 Comparative Example 2 380 4.9 Comparative Example 3 392 4.7
[0096] It can be seen from Table 1 that the first charge specific capacity of the batteries assembled with the lithium supplement provided by Examples 1-6 of the present invention is higher than the values in Comparative Examples 1-3, and the decomposition potential of lithium removal is lower than the values in Comparative Examples 1-2, indicating that the lithium supplement of the present invention has the characteristics of high lithium supplement specific capacity and low decomposition potential of lithium removal.
[0097] From Examples 1, 2, 3, and 6, it can be seen that the higher the mass proportion of the single-atom catalyst in the lithium supplement, the lower the lithium decomposition voltage of the lithium supplement, and the higher the lithium decomposition efficiency. When the mass ratio of the single-atom catalyst to the lithium-rich particles in the lithium supplement is (0.2-1):100, the lithium decomposition efficiency and the lithium supplement specific capacity can be better balanced. By comparing Example 1 with Example 4, it can be seen that Example 4 has the same lithium decomposition potential as Example 1, but the charge specific capacity of Example 4 is lower than that of Example 1. This is mainly because the presence of the coating layer of the lithium supplement of Example 4 reduces the mass proportion of the lithium-rich particles in the lithium supplement, so the charge specific capacity of Example 4 is lower than that of Example 1.
[0098] By comparing Example 1 and Comparative Example 3, it can be seen that although the compositions of the lithium supplements of Example 1 and Comparative Example 3 are the same, the charging specific capacity of Example 1 is higher than that of Comparative Example 3, and the delithiation potential is lower than that of Comparative Example 3. This is because the preparation methods of the lithium supplements of Example 1 and Comparative Example 3 are different. Compared with the lithium supplement prepared by mixing in Comparative Example 1, the heteroatom-doped carbon quantum dots supporting the single-atom catalyst in the lithium supplement prepared by ball milling and sintering in Example 1 are supported on lithium-rich particles. The contact area between the single-atom catalyst and the lithium-rich particles is larger, and the catalytic efficiency is better. Therefore, the lithium supplement of Example 1 has a lower delithiation potential and a higher charging specific capacity.
[0099] In addition, by comparing Example 1 with Comparative Examples 1 and 2, it can be seen that the heteroatom-doped carbon quantum dots have no catalytic effect on reducing the decomposition potential of the lithium supplement agent, indicating that the lithium supplement agent must contain a single atom catalyst to reduce the decomposition voltage; although the decomposition potential of Comparative Example 2 is consistent with that of Comparative Example 1, Comparative Example 2 has a higher charge specific capacity than Comparative Example 1, mainly because the high conductivity of the heteroatom-doped carbon quantum dots in Comparative Example 2 enhances the migration rate of lithium ions in the lithium supplement agent and improves the lithium supplement efficiency, thereby prompting lithium oxalate (Li2C2O4) to release more lithium ions.
[0100] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
Claims
1. A lithium supplement, characterized in that: The lithium supplement comprises lithium-rich particles and heteroatom-doped carbon quantum dots loaded with single-atom catalysts loaded on the lithium-rich particles; the lithium-rich particles comprise secondary particles, and the secondary particles comprise a core agglomerated by a plurality of primary particles; Wherein, the heteroatom-doped carbon quantum dots loaded with single-atom catalysts are located in the grain boundaries between the primary particles.
2. The lithium supplement according to claim 1, characterized in that The mass ratio of the lithium-rich particles to the single-atom catalyst is 100:(0.2-1); the mass ratio of the lithium-rich particles in the lithium supplement agent is 86%-95%.
3. The lithium supplement according to claim 1, characterized in that The heteroatom-doped carbon quantum dots loaded with single-atom catalysts are also located on the surface of the secondary particles.
4. The lithium supplement according to claim 1, characterized in that π-π stacking is formed between the lithium-rich particles and the heteroatom-doped carbon quantum dots loaded with single-atom catalysts.
5. The lithium supplement according to claim 1, characterized in that: The particle size D50 of the inner core is 5 μm-50 μm.
6. The lithium supplement according to claim 1, characterized in that: The secondary particles further include a coating layer located on the surface of the core, and the material of the coating layer includes heteroatom-doped carbon quantum dots and / or carbon-based materials loaded with single-atom catalysts.
7. The lithium supplement according to claim 1, characterized in that: The lithium-rich particles include one or more of a ternary lithium-supplementing material, a binary lithium-supplementing material and an organic lithium-supplementing material.
8. The lithium supplement according to claim 7, characterized in that: The organic lithium supplement material includes one or more of Li2DHBN, Li2C2O4, Li2C4O4 and Li2C6O6.
9. The lithium supplement according to claim 1, characterized in that: The single atom catalyst comprises one or more of a nickel atom, a cobalt atom and a zinc atom; and / or, The heteroatom includes one or more of N, S, P and B.
10. A method for preparing a lithium supplement according to any one of claims 1 to 9, characterized in that: include: placing the carbon quantum dots in an atmosphere of an inert gas and a heteroatom source gas for heat treatment to obtain heteroatom-doped carbon quantum dots; Dispersing the heteroatom-doped carbon quantum dots in a single-atom catalyst salt solution containing an alkali to carry out a complex reaction, thereby obtaining heteroatom-doped carbon quantum dots loaded with single-atom catalyst ions; Placing the heteroatom-doped carbon quantum dots loaded with single-atom catalyst ions in a reducing gas atmosphere for reduction reaction to obtain heteroatom-doped carbon quantum dots loaded with single-atom catalysts; The lithium-rich particles and the heteroatom-doped carbon quantum dots loaded with single-atom catalysts are ball-milled and sintered to obtain a lithium supplement agent, which includes lithium-rich particles and heteroatom-doped carbon quantum dots loaded with single-atom catalysts loaded on the lithium-rich particles.
11. A positive electrode material, characterized in that: The invention comprises a positive electrode active material and a lithium supplement material, wherein the lithium supplement material comprises the lithium supplement agent according to any one of claims 1 to 9 or the lithium supplement agent prepared by the preparation method according to claim 10.
12. A lithium ion battery, characterized in that: The invention comprises a positive electrode, a negative electrode, and a separator and an electrolyte located between the positive electrode and the negative electrode, wherein the positive electrode comprises the positive electrode material as claimed in claim 11.