A two-component polyurethane glass adhesive, its preparation method and application

By using a specific formulation of two-component polyurethane glass adhesive, the problems of slow curing speed and complicated pretreatment of single-component polyurethane adhesives are solved, achieving rapid curing and high-strength glass bonding, and simplifying the process.

CN117535027BActive Publication Date: 2026-11-10HANGZHOU ZHIJIANG SILICONE CHEM +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311565666.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-22
Publication Date
2026-11-10
Estimated Expiration
2043-11-22

AI Technical Summary

Technical Problem

Existing single-component polyurethane adhesives have a slow curing speed, which cannot meet the needs of rapid assembly. Furthermore, increasing the curing speed using traditional methods can affect the final strength. In addition, the glass bonding process requires pretreatment, which leads to complex procedures and increased costs.

Method used

The two-component polyurethane glass adhesive consists of a polyether polyol, a small molecule diol, an amino curing agent, an adhesion promoter A, and a filler A, and a polyisocyanate, a polyurethane prepolymer, a plasticizer, an adhesion promoter B, and a filler B. By using a specific ratio and adding adhesion promoters A and B, it achieves rapid curing and good adhesion to glass without the need for a primer.

Benefits of technology

It achieves rapid curing, resulting in high shear strength, tensile strength, and elongation at break, while eliminating the need for primer treatment, thus improving adhesion and simplifying the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_8
    Figure SMS_8
Patent Text Reader

Abstract

This invention provides a two-component polyurethane glass adhesive, its preparation method, and its application. The two-component polyurethane glass adhesive includes component A and component B. Component A includes polyether polyol, small molecule diol, amino curing agent, adhesion promoter A, and filler A. Component B includes polyisocyanate, polyurethane prepolymer, plasticizer, adhesion promoter B, and filler B. By using the above-mentioned specific combination of components A and B, especially by adding adhesion promoter A and adhesion promoter B to components A and B respectively, the resulting two-component polyurethane glass adhesive has a fast curing speed and good adhesion to painted panels and glass without the need for a primer. At the same time, the cured glass adhesive also has excellent mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of glass adhesive technology, specifically relating to a two-component polyurethane glass adhesive, its preparation method, and its application. Background Technology

[0002] Currently, polyurethane (PU) is one of the world's six major synthetic materials, possessing both adhesive and sealing functions. Polyurethane sealants, silicone sealants, and polysulfide sealants constitute the three major types of high-end sealants. Among them, polyurethane sealants generally contain strongly polar groups, which can form a strong and tough elastic adhesive layer after curing. Polyurethane molecules can be divided into three components: polyether segments, isocyanate segments, and low molecular weight segments as chain extenders. Therefore, polyurethane molecules are regarded as block copolymers of flexible and rigid segments. Its structural characteristics enable polyurethane sealants to have good adhesion to a variety of materials. At the same time, polyurethane sealants also have excellent wear resistance, low-temperature flexibility, high mechanical strength, good adhesion, and good elasticity, and therefore have been widely used in all aspects of life.

[0003] With the rapid development of the passenger car, bus, and rail transit markets, these industries are using single-component polyurethane windshield adhesives and sealants. However, as customers demand faster assembly speeds, the requirements for the strength formation rate of glass adhesives are becoming increasingly stringent. For example, OEMs typically conduct road tests and rain tests 3-4 hours after glass installation. Traditional single-component moisture-curing polyurethane adhesives have a very slow curing speed, generally requiring 7 days to reach a shear strength of 1.5 MPa. Therefore, road tests and rain tests can cause glass displacement and leakage. As a result, traditional single-component polyurethane adhesives can no longer meet the requirements. Although the curing speed of single-component polyurethane adhesives can be increased by compounding catalysts and increasing their content, this method has limited effectiveness and cannot solve the problem. Furthermore, the excessively fast curing speed can cause carbon dioxide generated by the adhesive layer to be difficult to release, ultimately leading to defects in the adhesive layer and affecting the final cured strength.

[0004] Furthermore, in the current manufacturing and repair of automobiles, trucks, trains, or ships, glass bonding typically requires pretreatment of the substrate with cleaning agents or primers to ensure bonding safety. However, pretreatment implies additional time-consuming steps, incurring expenses and increasing the complexity and error rate of the bonding process. To reduce costs and improve process safety, there is a strong desire for a polyurethane glass adhesive that can reliably and as quickly as possible form good adhesion, even without pretreatment of the substrate with cleaning agents or primers.

[0005] CN104497956A discloses a fast-curing two-component polyurethane elastic adhesive and its preparation method. The adhesive is composed of a polyurethane adhesive (component A) and a curing accelerator (component B) mixed in a certain proportion. Component A comprises: 20-60 wt.% of a polyurethane prepolymer containing at least one isocyanate end group; 10-40 wt.% of a plasticizer; 0.1-3 wt.% of a dehydrating agent; 10-40 wt.% of a reinforcing filler; 0.1-1 wt.% of a silane coupling agent; and 1-6 wt.% of a solvent. Component B comprises: 20-50 wt.% of a plasticizer; and 30 wt.% of a filler. ~60wt.%; polyether polyol 0~10wt.%; water 2~20wt.%; catalyst 0.2~7wt.%; the mixing volume ratio of component A and component B is 100:1~100:25; the polyurethane elastomer adhesive provided by this invention has excellent storage stability, can cure quickly, has high initial strength, and a relatively long working time after mixing, ensuring sufficient time to complete the bonding of the adhesive to the two bonding substrates during construction, ensuring effective adhesion. However, it requires a cleaning agent and a primer to promote adhesion, making the operation very cumbersome.

[0006] CN101379106A discloses a two-component polyurethane composition with high early strength, consisting of a first component A and a second component B. The first component is also cured independently by reacting with moisture in the air, and the second component contains water and acid. However, the two-component polyurethane composition provided by this invention has a short working time and releases volatile and strongly odorous decomposition products, especially aldehydes or ketones, with an unpleasant smell during actual use.

[0007] Therefore, in order to address the above-mentioned technical problems, there is an urgent need to develop a two-component polyurethane glass adhesive with high strength that can be applied without a primer. Summary of the Invention

[0008] To address the shortcomings of existing technologies, the present invention aims to provide a two-component polyurethane glass adhesive, its preparation method, and its application. The two-component polyurethane glass adhesive exhibits good adhesion to painted panels and glass without the need for a primer, and can cure rapidly to achieve a certain strength. Furthermore, the cured glass adhesive possesses high shear strength, tensile strength, and elongation at break.

[0009] To achieve this objective, the present invention adopts the following technical solution:

[0010] In a first aspect, the present invention provides a two-component polyurethane glass sealant, the two-component polyurethane glass sealant comprising component A and component B;

[0011] Component A includes polyether polyol, small molecule diol, amino curing agent, adhesion promoter A and filler A;

[0012] Component B includes polyisocyanate, polyurethane prepolymer, plasticizer, adhesion promoter B, and filler B.

[0013] The two-component polyurethane glass adhesive provided by this invention comprises component A and component B. Component A includes polyether polyol, small molecule diol, amino curing agent, adhesion promoter A, and filler A. Component B includes polyisocyanate, polyurethane prepolymer, plasticizer, adhesion promoter B, and filler B. By using the above-mentioned specific combination of components A and B, especially by adding adhesion promoter A and adhesion promoter B to components A and B respectively, the resulting two-component polyurethane glass adhesive has a fast curing speed and good adhesion to glass without the need for a primer. At the same time, the cured film also has excellent mechanical properties, such as high tensile strength, shear strength, and elongation at break.

[0014] Preferably, component A comprises the following components in parts by weight:

[0015]

[0016]

[0017] As a preferred embodiment of the present invention, further limiting the proportions of each raw material in component A within a specific range helps to further improve the bonding and mechanical properties of the two-component polyurethane glass adhesive; wherein, the polyether polyol can be 37 parts by weight, 39 parts by weight, 41 parts by weight, 43 parts by weight, 45 parts by weight, 47 parts by weight, or 49 parts by weight, etc.; the small molecule diol can be 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, or 4.5 parts by weight, etc.; the amino curing... The agent can be 0.7 parts by weight, 0.9 parts by weight, 1.1 parts by weight, 1.3 parts by weight, 1.5 parts by weight, 1.7 parts by weight, or 1.9 parts by weight, etc.; the adhesive accelerator A can be 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5 parts by weight, or 5.5 parts by weight, etc.; the filler A can be 37 parts by weight, 39 parts by weight, 41 parts by weight, 43 parts by weight, 45 parts by weight, 47 parts by weight, 49 parts by weight, 51 parts by weight, or 53 parts by weight, etc.

[0018] Preferably, the number average molecular weight of the polyether polyol is 2000 to 7000, such as 3000, 4000, 5000 or 6000.

[0019] Preferably, the functionality of the polyether polyol is 2 to 3.

[0020] Preferably, the polyether polyol includes polyethylene oxide polyol and / or polypropylene oxide polyol.

[0021] Preferably, the polyether polyol can be specifically selected from... C2020 C2030 F3135 F3128 Any one or a combination of at least two of the following: F3156, DL2000, 330N, or C3050.

[0022] Preferably, the small molecule diol includes any one or a combination of at least two of ethylene glycol, butanediol, propylene glycol, glycerol, dipropylene glycol, 1,4-butanediol, 1,6-hexanediol, or 2-ethyl-1,3-hexanediol.

[0023] Preferably, the amino curing agent includes polyetheramine, specifically selected from any one or a combination of at least two of T403, T5000, D230, D400, ED600, ED900 or ED200.

[0024] Preferably, the content of adhesive accelerator A in component A is 1 to 3 parts by weight.

[0025] Preferably, the adhesion promoter A is obtained by reacting aminophenylsilane and a silane modifier.

[0026] Preferably, the molar ratio of the aminophenylsilane to the silane modifier is 1:(0.9-1.1), for example, 1:0.92, 1:0.94, 1:0.96, 1:0.98, 1:1, 1:1.02, 1:1.04, 1:1.06 or 1:1.08, etc.

[0027] Preferably, the aminophenyl silane includes any one or a combination of at least two of N-phenyl-γ-aminopropyltrimethoxysilane, N-phenyl-γ-aminopropyltriethoxysilane, N-phenylaminomethyltrimethoxysilane, N-phenylaminomethyltriethoxysilane, or γ-aminopropyltriethoxysilane.

[0028] Preferably, the silane modifier comprises any one or a combination of at least two of o-tolyl glycidyl ether, p-tolyl glycidyl ether, phenyl glycidyl ether, triphenylmethyl-(S)-glycidyl ether and resorcinol diglycidyl ether or γ-glycidyl etheroxypropyltrimethoxysilane.

[0029] Preferably, the filler A includes any one or a combination of at least two of the following: kaolin, clay, nano-calcium carbonate, light calcium carbonate, or talc.

[0030] Preferably, component A further includes a catalyst and / or fumed silica.

[0031] Preferably, the catalyst content in component A is 0.1 to 0.5 parts by weight, for example, 0.15 parts by weight, 0.2 parts by weight, 0.25 parts by weight, 0.3 parts by weight, 0.35 parts by weight, 0.4 parts by weight, or 0.45 parts by weight.

[0032] Preferably, the catalyst comprises any one or a combination of at least two of the following: dibutyltin dichloride, dibutyltin dilaurate, stannous octoate, dibutyltin diacetate, N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl)aldehyde, N-ethylmorpholine, N-methylmorpholine, or N,N'-diethylpiperazine.

[0033] Preferably, the content of fumed silica in component A is 1 to 5 parts by weight, such as 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight or 4.5 parts by weight.

[0034] Preferably, the fumed silica is a hydrophobic fumed silica, for example, the silica can be any one or a combination of at least two of Wacker H18, Wacker H20, Evonik R974, Evonik R202 or Cabot TS720.

[0035] Preferably, component B comprises the following components in parts by weight:

[0036]

[0037] As a preferred embodiment of the present invention, the B component is formulated with the aforementioned specific amounts of raw materials, which can further improve the bonding performance and mechanical properties of the two-component polyurethane glass adhesive. Specifically, the polyisocyanate can be 7 parts by weight, 9 parts by weight, 11 parts by weight, 13 parts by weight, 15 parts by weight, 17 parts by weight, or 19 parts by weight, etc.; the polyisocyanate polymer can be 42 parts by weight, 44 parts by weight, 46 parts by weight, 48 parts by weight, 50 parts by weight, 52 parts by weight, 54 parts by weight, 56 parts by weight, 58 parts by weight, 60 parts by weight, 62 parts by weight, or 64 parts by weight, etc.; the plasticizer can be 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, or 14 parts by weight, etc.; the adhesion promoter B can be 2 parts by weight, 3 parts by weight, 4 parts by weight, or 5 parts by weight, etc.; and the filler B can be 11 parts by weight, 13 parts by weight, 15 parts by weight, 17 parts by weight, or 19 parts by weight, etc.

[0038] Preferably, the polyisocyanate can be any one or a combination of at least two of Yantai Wanhua MDI100L, MDI-50, modified MDI8219, PM200, Suprasec 3051 or Suprasec2647.

[0039] Preferably, the isocyanate group content in the polyurethane prepolymer is 2-6% by mass, such as 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or 5.5%.

[0040] Preferably, the raw materials for preparing the polyurethane prepolymer include diisocyanate and hydroxyl compounds.

[0041] Preferably, the hydroxyl compound includes polyether polyols and / or hydroxyl-terminated polybutadiene.

[0042] Preferably, the polyurethane prepolymer is obtained by reacting diisocyanate and hydroxyl compound.

[0043] Preferably, the plasticizer comprises any one or a combination of at least two of the following: di-n-octyl phthalate, diethyl phthalate dipropylene glycol dibenzoate, alkyl sulfonate, diisononyl phthalate, or ethyl 2-isobutoxybenzoate.

[0044] Preferably, the content of adhesion promoter B in component B is 1 to 6 parts by weight.

[0045] Preferably, the adhesion promoter B is obtained by reacting an isocyanate-based compound with a secondary aminosilane.

[0046] Preferably, the isocyanate-based compound includes any one or a combination of at least two of toluene diisocyanate, diphenylmethane diisocyanate, polymeric diphenylmethane diisocyanate, isoflurone diisocyanate, toluene diisocyanate trimer, isoflurone diisocyanate trimer, or hexamethylene diisocyanate trimer; for example, Dongxu HDX-100, HDX-50EA, Wanhua Chemical HB3175, and Takenate D-268T can be selected. Any one or at least two of N3300, N100, N75, N3200, N3400 or N3600.

[0047] Preferably, the secondary aminosilane comprises any one or a combination of at least two of bis-(γ-trimethoxysilylpropyl)amine, N-phenyl-γ-aminopropyltrimethoxysilane, N-n-butyl-aminopropyl-trimethoxysilane, N-phenyl-γ-aminopropyltriethoxysilane, N-butyl-γ-aminopropyltriethoxysilane, N-ethyl-3-aminopropyltrimethoxysilane, and N-ethyl-3-aminopropyltriethoxysilane.

[0048] Preferably, the filler B comprises any one or a combination of at least two of the following: special carbon black, kaolin, nano-calcium carbonate, light calcium carbonate, or talc.

[0049] Preferably, component B further includes a dehydrating agent;

[0050] Preferably, the content of the dehydrating agent in component B is not higher than 3 parts by weight, such as 2.8 parts by weight, 2.6 parts by weight, 2.4 parts by weight, 2.2 parts by weight, or 2 parts by weight.

[0051] In a second aspect, the present invention provides a method for preparing a two-component polyurethane glass adhesive as described in the first aspect, characterized in that the preparation method comprises:

[0052] The polyether polyol, small molecule diol, amino curing agent, adhesion promoter A, filler A, optional catalyst and optional fumed silica are mixed to obtain component A;

[0053] The polyisocyanate, polyurethane prepolymer, plasticizer, adhesion promoter B, filler B, and optionally dehydrating agent are mixed to obtain component B.

[0054] Thirdly, the present invention provides a method for using the two-component polyurethane glass adhesive as described in the first aspect, characterized in that the method includes: mixing component A and component B, applying the mixture to the surface of the glass to be bonded, and curing it to complete the use of the two-component polyurethane glass adhesive.

[0055] Preferably, the curing temperature is room temperature.

[0056] Fourthly, the present invention provides an application of the two-component polyurethane glass adhesive as described in the first aspect in windshield bonding.

[0057] Compared with the prior art, the present invention has the following beneficial effects:

[0058] The two-component polyurethane glass adhesive provided by this invention includes component A and component B. Component A includes polyether polyol, small molecule diol, amino curing agent, adhesion promoter A, and filler A. Component B includes polyisocyanate, polyurethane prepolymer, plasticizer, adhesion promoter B, and filler B. By using the above-mentioned specific combination of components A and B, especially by adding adhesion promoter A and adhesion promoter B to components A and B respectively, the resulting two-component polyurethane glass adhesive has a fast curing speed and can have good adhesion to glass without the need for a primer. At the same time, the coating film formed after curing also has excellent mechanical properties. Detailed Implementation

[0059] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0060] The following is some information about the raw materials involved in the specific embodiments of the present invention:

[0061] Component A:

[0062] (1) γ-aminopropyltriethoxysilane: Jingzhou Jianghan Fine Chemical Co., Ltd.

[0063] (2) γ-glycidyl etheroxypropyltrimethoxysilane: Jingzhou Jianghan Fine Chemical Co., Ltd.

[0064] (3) Polyether polyols: Yantai Wanhua Chemical Group, F3128;

[0065] (4) 1,4-Butanediol (BDO): Sinopharm Group;

[0066] (5) 2-Ethyl-1,3-hexanediol (EHD): Jiangsu Runfeng Synthetic Technology Co., Ltd.;

[0067] (6) Amino curing agent: Wuhan Huaxiang Kejie Biotechnology Co., Ltd., ED600;

[0068] (7) Clay: Shanxi Jinyu Kelin Technology Co., Ltd., B-95;

[0069] (8) Catalysts: Evonik, Polycat SA20;

[0070] (9) Fumed silica: Wacker Chemie (China) Co., Ltd., H18.

[0071] Component B:

[0072] (1) Polyisocyanates: Yantai Wanhua Chemical Group, PM-200;

[0073] (2) HDI trimer: N3600;

[0074] (3) Polymeric diphenylmethane diisocyanate: Huntsman, Suprasec'2647;

[0075] (4) Secondary aminosilanes: Evonik, N-n-butyl-aminopropyl-trimethoxysilane (1189);

[0076] (5) Plasticizers: Lanxess Chemicals (China) Co., Ltd., MESAMOLL;

[0077] (6) Carbon black: Cabot, M-580.

[0078] Preparation Example 1

[0079] An adhesion promoter A is prepared by means of: adding 884g of γ-aminopropyltriethoxysilane to a three-necked flask, stirring under vacuum, heating to 55°C, removing the vacuum with nitrogen, then slowly adding 944g of γ-glycidoxypropyltrimethoxysilane to the three-necked flask, reacting at 55°C under vacuum and stirring for 4 hours, and then cooling and discharging to obtain the adhesion promoter A.

[0080] Preparation Example 2

[0081] A polyurethane prepolymer, wherein the mass percentage of isocyanate groups is 4.31%, is prepared by means of: adding 787g of hydroxyl-terminated polybutadiene (polyvestHT) to a 1L three-necked flask, heating to 60℃, adding 213g of MDI-100, and reacting at 80℃ for 5h to obtain the polyurethane prepolymer.

[0082] Preparation Example 3

[0083] An adhesion promoter B is prepared by means of: adding 300g of HDI trimer and 200g of polymerized diphenylmethane diisocyanate into a 1L three-necked flask, heating to 50°C, mixing under vacuum for 1h, then slowly adding 500g of secondary aminosilane, controlling the temperature at 50°C, and stirring under vacuum for 2.5h to obtain an isocyanate-terminated silane polymer with an NCO group content of 4.1%, which is adhesion promoter B.

[0084] Examples 1-8

[0085] A two-component polyurethane glass sealant includes component A and component B. The specific compositions of components A and B are shown in Table 1. In Table 1, the amount of each component is in "parts by weight".

[0086] Table 1

[0087]

[0088] The preparation methods of the two-component polyurethane glass sealant provided in Examples 1-8 include the preparation of component A and component B;

[0089] The preparation method of component A includes: adding polyether polyol, small molecule diol and amino curing agent into a 5L planetary mixer, stirring at medium speed under vacuum for 10 minutes, adding filler and fumed silica, heating to 110℃, stirring and dehydrating under vacuum for 2.5 hours, and then cooling to room temperature; then adding adhesion promoter A and catalyst, stirring evenly under vacuum for 1 hour, dispensing the adhesive into a glue tube, and sealing and storing it.

[0090] The preparation method of component B includes: adding polyisocyanate, polyurethane prepolymer and plasticizer into a 5L planetary mixer, stirring at medium speed under vacuum for 30 minutes, adding filler, stirring under vacuum for 1 hour, controlling the temperature to be less than 80℃, then adding adhesion promoter B, stirring under vacuum for 45 minutes, dispensing the adhesive into a tube, and sealing and storing it.

[0091] Comparative Examples 1-5

[0092] A two-component polyurethane glass sealant includes component A and component B. The specific compositions of components A and B are shown in Table 2. In Table 2, the amount of each component is in "parts by weight".

[0093] Table 2

[0094]

[0095] The preparation methods of the two-component polyurethane glass adhesives provided in Comparative Examples 1 to 5 are the same as those in Example 1.

[0096] Performance testing:

[0097] (1) Shear strength at different curing times: Component A and component B of the two-component polyurethane glass adhesive were mixed at a mass ratio of 1:0.8, coated on a 2mm thick painted board, and then another painted board was attached. The mixture was cured at a temperature of 23±2℃ and a relative humidity of 50%. The initial shear strength at different curing times was tested. The width of the shear sample was 10mm and the thickness of the adhesive layer was 4.0±0.2mm. The shear strength was tested according to the test method provided in GB / T 7124-2008.

[0098] The two-component polyurethane glass adhesives provided in Examples 1-8 and Comparative Examples 1-5 were tested according to the above test methods. The test results are shown in Table 3.

[0099] Table 3

[0100]

[0101] According to the data in Table 3:

[0102] The two-component polyurethane glass adhesive provided by this invention has a high curing speed, with a shear strength of up to 4.95 MPa after 4 hours of curing, while the two-component polyurethane glass adhesive without the addition of adhesion promoter A and / or adhesion promoter B has a shear strength of up to 2.41 MPa after 4 hours of curing.

[0103] (2) Shear strength: The A and B components of the two-component polyurethane glass adhesive were mixed at a mass ratio of 1:0.8 and coated on a 2mm thick painted board. Then another painted board was attached and cured for 168h at a temperature of 23±2℃ and a relative humidity of 50%. The width of the shear sample was 10mm and the thickness of the adhesive layer was 4.0±0.2mm. The test was then conducted according to the test method provided in GB / T7124-2008, and the test speed was 20±2mm / min.

[0104] (3) Tensile strength and elongation at break: The A and B components of the two-component polyurethane glass sealant were mixed at a mass ratio of 1:0.8 and placed under standard test conditions for 168 hours. The dumbbell-shaped specimens were used and the test was conducted according to the test method provided in GB / T 528-2009. The test speed was 500±50mm / min.

[0105] (4) Interfacial adhesion: Component A and component B of the two-component polyurethane glass sealant were mixed at a mass ratio of 1:0.8; the substrate was a painted board or a glass board, the size of the painted board was 150×100×0.9mm, and the size of the glass board was 150×100×4mm; test steps: a) clean the glass board and painted board and let them air dry for 5 minutes; b) use a glue gun to apply the glass sealant to the sample in the shape of a ф10×150mm semi-circular strip; c) place the sample under standard conditions for 168 hours to allow it to fully cure; d) take out the sample and use pliers to clamp one end of the cured strip, pull the strip while cutting the strip horizontally with a blade, and observe the damage (CF is the damage of the colloid itself, cohesive damage).

[0106] The standard conditions are as follows: temperature: 23℃, relative humidity: 55%; aging conditions for heat resistance samples: temperature 90℃, 300h, and the samples are placed in a standard environment for 24h after being removed; aging conditions for damp heat resistance samples: temperature 70℃, relative humidity 95%, 300h, and the samples are placed in a standard environment for 24h after being removed; aging conditions for water resistance samples: constant temperature water bath at 40℃, 72h, and the samples are placed in a standard environment for 24h after being removed.

[0107] The two-component polyurethane glass adhesives provided in Examples 1-8 and Comparative Examples 1-5 were tested according to the above test methods. The test results are shown in Tables 4 and 5.

[0108] Table 4

[0109]

[0110]

[0111] Table 5

[0112]

[0113]

[0114] Based on the data in Tables 4 and 5, it can be seen that:

[0115] This invention combines specific components A and B, and adds adhesion promoter A and adhesion promoter B to components A and B respectively, so that the resulting two-component polyurethane glass adhesive can still achieve 100% cohesive failure at the interface under the condition of no primer coating, and has excellent adhesion to painted boards and glass boards.

[0116] Meanwhile, by adding adhesion promoter A and adhesion promoter B to components A and B respectively, the resulting two-component polyurethane glass adhesive also exhibits high shear strength, tensile strength, and elongation at break after curing.

[0117] The applicant declares that this invention illustrates a two-component polyurethane glass adhesive, its preparation method, and its application through the above embodiments. However, this invention is not limited to the above embodiments, meaning that this invention does not necessarily rely on the above embodiments for implementation. Those skilled in the art should understand that any improvements to this invention, equivalent substitutions of the raw materials in the product of this invention, additions of auxiliary components, and selection of specific methods, all fall within the protection and disclosure scope of this invention.

Claims

1. A two-component polyurethane glass sealant, characterized in that, The two-component polyurethane glass sealant includes component A and component B; Component A comprises the following components in parts by weight: 35-50 parts by weight of polyether polyol; 1-5 parts by weight of small molecule diols; Amino curing agent 0.5~2 parts by weight; Adhesion accelerator A1 ~ 6 parts by weight; Packing material A: 35~55 parts by weight; The adhesion promoter A is obtained by reacting aminosilane and silane modifier; The aminosilane includes any one or a combination of at least two of N-phenyl-γ-aminopropyltrimethoxysilane, N-phenyl-γ-aminopropyltriethoxysilane, N-phenylaminomethyltrimethoxysilane, N-phenylaminomethyltriethoxysilane or γ-aminopropyltriethoxysilane. The silane modifier includes any one or a combination of at least two of o-tolyl glycidyl ether, p-tolyl glycidyl ether, phenyl glycidyl ether, triphenylmethyl-(S)-glycidyl ether and resorcinol diglycidyl ether or γ-glycidyl etheroxypropyltrimethoxysilane. Component B comprises the following components in parts by weight: 5-20 parts by weight of polyisocyanate; 40-65 parts by weight of polyisocyanate polymer; Plasticizer 5-15 parts by weight; Adhesion accelerator B1, 6 parts by weight; Packing material B: 10-20 parts by weight; The raw materials for preparing the polyisocyanate polymer include diisocyanate and hydroxyl compounds; The adhesion promoter B is obtained by reacting an isocyanate-based compound with a secondary aminosilane; The isocyanate-based compound includes any one or a combination of at least two of toluene diisocyanate, diphenylmethane diisocyanate, polymeric diphenylmethane diisocyanate, isophorone diisocyanate, toluene diisocyanate trimer, isophorone diisocyanate trimer, or hexamethylene diisocyanate trimer. The secondary aminosilane includes any one or a combination of at least two of the following: bis-(γ-trimethoxysilylpropyl)amine, N-phenyl-γ-aminopropyltrimethoxysilane, N-n-butyl-aminopropyl-trimethoxysilane, N-phenyl-γ-aminopropyltriethoxysilane, N-butyl-γ-aminopropyltriethoxysilane, N-ethyl-3-aminopropyltrimethoxysilane, and N-ethyl-3-aminopropyltriethoxysilane.

2. The two-component polyurethane glass sealant according to claim 1, characterized in that, The number average molecular weight of the polyether polyol is 2000~7000.

3. The two-component polyurethane glass sealant according to claim 1, characterized in that, The functionality of the polyether polyol is 2 to 3.

4. The two-component polyurethane glass sealant according to claim 3, characterized in that, The polyether polyols include polyethylene oxide polyols and / or polypropylene oxide polyols.

5. The two-component polyurethane glass sealant according to claim 1, characterized in that, The small molecule diols include any one or a combination of at least two of ethylene glycol, butanediol, propylene glycol, glycerol, dipropylene glycol, 1,4-butanediol, 1,6-hexanediol, or 2-ethyl-1,3-hexanediol.

6. The two-component polyurethane glass sealant according to claim 1, characterized in that, The amino curing agent includes polyetheramine.

7. The two-component polyurethane glass sealant according to claim 1, characterized in that, The content of adhesion promoter A in component A is 1 to 3 parts by weight.

8. The two-component polyurethane glass sealant according to claim 1, characterized in that, The molar ratio of the aminosilane to the silane modifier is 1:(0.9-1.1).

9. The two-component polyurethane glass sealant according to claim 1, characterized in that, The filler A includes any one or a combination of at least two of the following: kaolin, clay, nano-calcium carbonate, light calcium carbonate, or talc.

10. The two-component polyurethane glass sealant according to claim 1, characterized in that, Component A also includes a catalyst and / or fumed silica.

11. The two-component polyurethane glass sealant according to claim 10, characterized in that, The catalyst content in component A is 0.1 to 0.5 parts by weight.

12. The two-component polyurethane glass sealant according to claim 10, characterized in that, The catalyst comprises any one or a combination of at least two of the following: dibutyltin dichloride, dibutyltin dilaurate, stannous octoate, dibutyltin diacetate, N,N-dimethylcyclohexylamine, bis(2-dimethylaminoethyl)aldehyde, N-ethylmorpholine, N-methylmorpholine, or N,N'-diethylpiperazine.

13. The two-component polyurethane glass sealant according to claim 10, characterized in that, The content of fumed silica in component A is 1 to 5 parts by weight.

14. The two-component polyurethane glass sealant according to claim 10, characterized in that, The fumed silica is a hydrophobic fumed silica.

15. The two-component polyurethane glass sealant according to claim 1, characterized in that, The isocyanate group content in the polyisocyanate polymer is 2-6% by mass.

16. The two-component polyurethane glass sealant according to claim 1, characterized in that, The hydroxyl compounds include polyether polyols and / or hydroxyl-terminated polybutadiene.

17. The two-component polyurethane glass sealant according to claim 1, characterized in that, The plasticizer includes any one or a combination of at least two of the following: di-n-octyl phthalate, diethyl phthalate dipropylene glycol dibenzoate, alkyl sulfonate, diisononyl phthalate, or ethyl 2-isobutoxybenzoate.

18. The two-component polyurethane glass sealant according to claim 1, characterized in that, The filler B includes any one or a combination of at least two of the following: special carbon black, kaolin, nano calcium carbonate, light calcium carbonate, or talc.

19. The two-component polyurethane glass sealant according to claim 1, characterized in that, Component B also includes a dehydrating agent.

20. The two-component polyurethane glass sealant according to claim 19, characterized in that, The content of the dehydrating agent in component B is no more than 3 parts by weight.

21. A method for preparing a two-component polyurethane glass sealant as described in any one of claims 1 to 20, characterized in that, The preparation method includes: mixing polyether polyol, small molecule diol, amino curing agent, adhesion promoter A, filler A, optional catalyst and optional fumed silica to obtain component A; The polyisocyanate, polyurethane prepolymer, plasticizer, adhesion promoter B, filler B, and optionally dehydrating agent are mixed to obtain component B.

22. A method of using a two-component polyurethane glass sealant as described in any one of claims 1 to 20, characterized in that, The method of use includes: mixing component A and component B, applying the mixture to the glass surface to be bonded, and curing it to complete the use of the two-component polyurethane glass adhesive.

23. The method of use according to claim 22, characterized in that, The curing temperature is room temperature.

24. The application of a two-component polyurethane glass adhesive as described in any one of claims 1 to 20 in windshield bonding.

Citation Information

Patent Citations

  • Two-component polyurethane composition having high early strength

    CN101379106A

  • Rapidly-cured double-component polyurethane elastic adhesive and preparation method thereof

    CN104497956A

  • High-strength first-coat-free single-component polyurethane windshield glass glue and preparation method thereof

    CN108239516A

  • Two-component polyurethane adhesive

    CN110114380A

  • Bi-component polyurethane structural adhesive for bonding power batteries and preparation method thereof