A silicon-carbon negative electrode material for reducing interface side reactions and a preparation method thereof

By using porous carbon in the negative electrode material of lithium-ion battery to fill amorphous silicon and form an Al2O3 layer, and then coat the carbon layer, the problem of interface side reaction of silicon-carbon composite materials during circulation is solved, and the stability and conductivity of the material are improved , reduces production costs.

CN117542980BActive Publication Date: 2024-11-01XUANCHENG SILIKO NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311632343.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-01
Publication Date
2024-11-01
Estimated Expiration
2043-12-01

AI Technical Summary

Technical Problem

In the negative electrode materials of existing lithium-ion batteries, silicon-carbon composite materials are prone to interfacial side reactions during long-term circulation, resulting in reduced material performance and increased polarization, and the presence of SiO2 layer will reduce the first effect of the material.

Method used

Porous carbon is used to fill nano-level amorphous silicon through the vapor-phase silicon deposition process, and form an Al2O3 layer on the periphery of the porous carbon by aluminum thermal reduction reaction, and then coat the carbon layer on the Al2O3 layer to form a silicon-carbon negative electrode material that reduces interface side reactions. .

Benefits of technology

Effectively inhibit the expansion of silicon during lithium embedding and peeling of carbon layer, improve conductivity and material circulation stability, reduce production costs, and facilitate industrialization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117542980B_ABST
    Figure CN117542980B_ABST
Patent Text Reader

Abstract

The invention relates to the field of preparation of negative electrode materials for lithium ion batteries, and specifically to a silicon-carbon negative electrode material capable of reducing interface side reactions and a preparation method thereof; the silicon-carbon negative electrode material capable of reducing interface side reactions comprises: porous carbon, wherein the interior of the porous carbon is filled with nanometer-level amorphous silicon through a vapor phase silicon deposition process; an Al2O3 layer is formed on the periphery of the porous carbon through an aluminothermic reduction reaction; and a carbon coating layer is coated on the periphery of the Al2O3 layer; the silicon-carbon negative electrode material capable of reducing interface side reactions uses an oxidizing gas to oxidize the surface silicon of the silicon-carbon composite negative electrode material, and simultaneously reacts the surface SiO2 layer to generate an Al2O3 layer and amorphous Si according to an aluminothermic reduction reaction, and the formed Al2O3 layer plays a catalytic role in the vapor phase carbon deposition process, thereby increasing the sp2 hybridization ratio and improving the electrical conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of negative electrode materials for lithium ion batteries, and in particular to a silicon-carbon negative electrode material capable of reducing interface side reactions and a preparation method thereof. Background Art

[0002] At present, the negative electrode materials of commercial lithium-ion batteries are mainly graphite, including natural graphite and artificial graphite. However, with the rapid development of the new energy vehicle industry and the energy storage industry, consumers have put forward higher and higher requirements for the energy density of power batteries, which requires negative electrode materials with higher capacity.

[0003] Silicon has a capacity of 3580 mAh / g at room temperature. However, silicon has a large volume effect during lithium insertion and extraction and is difficult to form a stable SEI film. Silicon also produces more side reactions with the electrolyte. These factors limit the commercial application of silicon negative electrodes.

[0004] At present, a porous carbon siliconization process is provided in the patent application document with the patent application publication number CN108475779A, but it only coats a layer of carbon on the surface of the silicon-carbon composite particles. Since the carbon layer is relatively thin, it is easy to break in long-term cycles, resulting in the exposure of silicon, and the occurrence of interface side reactions cannot be prevented; and in the process of carbon coating, since silicon is in an amorphous state, it is easy to react with the carbon source to form by-products such as SiC, thereby reducing the first effect of the material and increasing polarization;

[0005] At the same time, the paper "Stable cycling of double-walled sillion nanotube batteryanodes through solid-electrolyte" mentioned that the SiO2 layer can promote the inward expansion of silicon, thereby forming a stable SEI film; the paper "Silicon carbide-free graphene growth on silicon for lithium-ion battery with high volumetric energy density" also mentioned that the SiO2 layer can promote the inward expansion of silicon, thereby forming a stable SEI film; and the presence of the SiO2 layer can inhibit the formation of SiC during the carbon deposition process. However, due to the presence of the SiO2 layer, the initial effect of the silicon-carbon composite negative electrode material will be reduced to a certain extent;

[0006] In view of the problems in the above-mentioned background technology, the present invention aims to provide a silicon-carbon negative electrode material and a preparation method thereof that can reduce interface side reactions. Summary of the invention

[0007] The object of the present invention is to provide a silicon-carbon negative electrode material with reduced interface side reactions and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] A silicon-carbon negative electrode material for reducing interface side reactions, the silicon-carbon negative electrode material for reducing interface side reactions comprising:

[0010] Porous carbon 3, porous carbon 3 is a spherical porous carbon with Dv50=3-10um, and the pore volume of porous carbon 3 is required to be 0.7-1.1cm 3 / g, the pore size requirement is that the pores with diameter less than 2nm account for more than 70%, and the surface area requirement is 1500~2000m 2 / g; the interior of the porous carbon 3 is filled with nano-scale amorphous silicon 4 through a vapor phase silicon deposition process; an Al2O3 layer 2 is formed on the periphery of the porous carbon 3 through an aluminothermic reduction reaction; and the periphery of the Al2O3 layer 2 is coated with a carbon coating layer 1.

[0011] The method for preparing the silicon-carbon negative electrode material for reducing interface side reactions comprises the following steps:

[0012] S1 Porous carbon vapor deposition silicon: Select porous carbon 3 that meets the raw material requirements and fill amorphous silicon 4 in the pores of the porous carbon 3 through the vapor deposition silicon process to form a silicon-carbon negative electrode material; the vapor deposition silicon process is to fill the nano-silicon formed by cracking monosilane into the pores of the porous carbon 3;

[0013] S2 Surface oxidation of silicon-carbon composite negative electrode material: Surface oxidation of the silicon-carbon negative electrode material formed in step S1;

[0014] S3 aluminothermic reduction to form an Al2O3 layer: the silicon-carbon negative electrode material whose surface is oxidized in step S2 is subjected to an aluminothermic reduction reaction using aluminum powder to form an Al2O3 layer 2 on the outside of the porous carbon 3;

[0015] S4 performs carbon coating: introducing organic gas to perform carbon coating on the outside of the Al2O3 layer 2 to form a carbon coating layer 1.

[0016] As a further solution of the present invention: S1 porous carbon vapor phase silicon deposition specific implementation method is:

[0017] Spherical porous carbon with Dv50=3~10um is selected and placed in a rotary kiln. The inside of the rotary kiln is evacuated with nitrogen for 2 hours (the purpose is to completely empty the oxygen-containing gas in the rotary kiln); then the rotary kiln is heated to 400~600℃ at 10℃ / min; at this time, SiH4 gas is introduced for 6 hours to perform vapor phase silicon deposition process on the porous carbon 3, and amorphous silicon 4 is filled in the pores inside the porous carbon 3 to form a silicon-carbon negative electrode material.

[0018] As a further solution of the present invention: The specific implementation method of surface oxidation of S2 silicon-carbon composite negative electrode material is as follows:

[0019] One or more oxidizing gases such as water vapor, ethanol vapor, N-methylpyrrolidone vapor, CO2, NO2, and air are introduced into the rotary kiln for 1 hour to oxidize the surface of the formed silicon-carbon negative electrode material, and then the introduction of the oxidizing gas into the rotary kiln is stopped and the silicon-carbon negative electrode material is allowed to cool naturally before being discharged from the rotary kiln; at the same time, it is required that after the silicon-carbon negative electrode material is introduced with the oxidizing gas, the overall oxygen content of the silicon-carbon negative electrode material is between 2 and 4wt%.

[0020] As a further solution of the present invention: S3 aluminothermic reduction to form Al2O3 layer. The specific implementation method is as follows:

[0021] The surface oxidized silicon-carbon negative electrode material obtained in step S2 is mixed with aluminum powder with a particle size of less than 200 mesh in a mixer at high speed for 2 hours; then the silicon-carbon negative electrode material mixed with aluminum powder is placed in a rotary furnace, the rotary furnace is evacuated with nitrogen for 2 hours, the temperature is increased to 300-800°C at 5°C / min, and the temperature is kept for 5-40 hours for aluminum thermal reduction reaction; at the same time, the ratio of aluminum powder to the silicon-carbon composite negative electrode material is between 1 and 5wt%.

[0022] As a further solution of the present invention: S4 performs carbon coating. The specific implementation method is: one or more organic gases such as methane, acetylene, ethylene, propylene, benzene, toluene, cyclopentane, etc. are introduced into a rotary kiln to carbon-coat the outer side of the Al2O3 layer 2 formed in step S3 for 6 hours to form a carbon coating layer 1, and then naturally cool it to take out the processed silicon-carbon negative electrode material with reduced interface side reactions.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The silicon-carbon negative electrode material for reducing interface side reactions has the following advantages:

[0025] 1. Oxidizing gas is used to oxidize the surface silicon of the silicon-carbon composite negative electrode material, and at the same time, the surface SiO2 layer is reacted to generate Al2O3 layer and amorphous Si according to the aluminum thermal reduction reaction; the formed Al2O3 layer has the following functions: 1. It can inhibit the expansion of silicon during the lithium insertion process; 2. It can prevent the side reaction of silicon and electrolyte after the carbon layer is peeled off during the cycle; 3. It plays a catalytic role in the process of gas phase carbon deposition, increases the sp2 hybridization ratio, and improves the conductivity; 4. Due to the interaction between oxygen and organic gas free radicals, the utilization rate of carbon source can be improved;

[0026] 2. The method for preparing the silicon-carbon negative electrode material for reducing interface side reactions has a simple process route, is easy to control, has low production cost, and is easy to scale up for industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention.

[0028] Figure 1 Schematic diagram of the structure of a silicon-carbon negative electrode material for reducing interface side reactions according to an embodiment of the present invention.

[0029] In the figure: 1-carbon coating layer, 2-Al2O3 layer, 3-porous carbon, 4-amorphous silicon. DETAILED DESCRIPTION

[0030] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0031] Example 1

[0032] See also Figure 1 , a silicon-carbon negative electrode material for reducing interface side reactions provided in an embodiment of the present invention, the silicon-carbon negative electrode material for reducing interface side reactions comprises:

[0033] Porous carbon 3, porous carbon 3 is a spherical porous carbon with Dv50=3-10um, and the pore volume of porous carbon 3 is required to be 0.7-1.1cm 3 / g, the pore size requirement is that the pores with diameter less than 2nm account for more than 70%, and the surface area requirement is 1500~2000m 2 / g; the interior of the porous carbon 3 is filled with nano-scale amorphous silicon 4 by a vapor phase silicon deposition process; an Al2O3 layer 2 is formed on the periphery of the porous carbon 3 by an aluminothermic reduction reaction; and a carbon coating layer 1 is coated on the periphery of the Al2O3 layer 2;

[0034] The method for preparing the silicon-carbon negative electrode material for reducing interface side reactions comprises the following steps:

[0035] S1 Porous carbon vapor deposition silicon: Select porous carbon 3 that meets the raw material requirements and fill amorphous silicon 4 in the pores of the porous carbon 3 through the vapor deposition silicon process to form a silicon-carbon negative electrode material; the vapor deposition silicon process is to fill the nano-silicon formed by cracking monosilane into the pores of the porous carbon 3;

[0036] S2 Surface oxidation of silicon-carbon composite negative electrode material: Surface oxidation of the silicon-carbon negative electrode material formed in step S1;

[0037] S3 aluminothermic reduction to form an Al2O3 layer: the silicon-carbon negative electrode material whose surface is oxidized in step S2 is subjected to an aluminothermic reduction reaction using aluminum powder to form an Al2O3 layer 2 on the outside of the porous carbon 3;

[0038] S4 performs carbon coating: introducing organic gas to perform carbon coating on the outer side of the Al2O3 layer 2 to form a carbon coating layer 1;

[0039] The specific implementation method of S1 porous carbon vapor deposition silicon is as follows:

[0040] Select Dv50 = 4um and pore volume of 0.9cm 3 / g, the pore size of pores <2nm accounts for 75%, compared with 1700m 2 The spherical porous carbon is placed in a rotary kiln, and the inside of the rotary kiln is evacuated with nitrogen for 2 hours (the purpose is to completely exhaust the oxygen-containing gas in the rotary kiln), and the nitrogen flow rate is 5L / min; then the rotary kiln is heated to 600°C at a rate of 10°C / min; at this time, SiH4 gas is introduced for 6 hours to perform a vapor phase silicon deposition process on the porous carbon 3 to fill the pores inside the porous carbon 3 with amorphous silicon 4 to form a silicon-carbon negative electrode material;

[0041] The specific implementation method of surface oxidation of S2 silicon-carbon composite negative electrode material is as follows:

[0042] Air is introduced into the rotary kiln at a flow rate of 1 L / min for 1 hour to oxidize the surface of the formed silicon-carbon negative electrode material, and then the introduction of oxidizing gas into the rotary kiln is stopped and the silicon-carbon negative electrode material is allowed to cool naturally before being discharged from the rotary kiln; at the same time, it is required that after the silicon-carbon negative electrode material is introduced into the oxidizing gas, the overall oxygen content of the silicon-carbon negative electrode material is between 2 and 4 wt%;

[0043] The specific implementation method of S3 aluminothermic reduction to form Al2O3 layer is as follows:

[0044] The surface-oxidized silicon-carbon negative electrode material obtained in step S2 is mixed with aluminum powder with a particle size of less than 200 meshes in a mixer at high speed for 2 hours; then the silicon-carbon negative electrode material mixed with aluminum powder is placed in a rotary kiln, and the rotary kiln is evacuated with nitrogen for 2 hours, the nitrogen flow rate is 5L / min, the temperature is increased to 750°C at 5°C / min, and the temperature is kept for 15 hours for aluminothermic reduction reaction; at the same time, the ratio of aluminum powder to the silicon-carbon composite negative electrode material is 2wt%;

[0045] The specific implementation method of carbon coating in S4 is as follows:

[0046] Into the rotary kiln, acetylene organic gas is introduced to carbon-coat the outer side of the Al2O3 layer 2 formed in step S3 for 6 hours to form a carbon coating layer 1, and then naturally cooled, the flow rate of acetylene is 1L / min, and the processed silicon-carbon negative electrode material with reduced interface side reactions is taken out;

[0047] Example 2

[0048] See also Figure 1 , a silicon-carbon negative electrode material for reducing interface side reactions provided in an embodiment of the present invention, the silicon-carbon negative electrode material for reducing interface side reactions comprises:

[0049] Porous carbon 3, porous carbon 3 is a spherical porous carbon with Dv50=3-10um, and the pore volume of porous carbon 3 is required to be 0.7-1.1cm 3 / g, the pore size requirement is that the pores with diameter less than 2nm account for more than 70%, and the surface area requirement is 1500~2000m 2 / g; the interior of the porous carbon 3 is filled with nano-scale amorphous silicon 4 by a vapor phase silicon deposition process; an Al2O3 layer 2 is formed on the periphery of the porous carbon 3 by an aluminothermic reduction reaction; and a carbon coating layer 1 is coated on the periphery of the Al2O3 layer 2;

[0050] The method for preparing the silicon-carbon negative electrode material for reducing interface side reactions comprises the following steps:

[0051] S1 Porous carbon vapor deposition silicon: Select porous carbon 3 that meets the raw material requirements and fill amorphous silicon 4 in the pores of the porous carbon 3 through the vapor deposition silicon process to form a silicon-carbon negative electrode material; the vapor deposition silicon process is to fill the nano-silicon formed by cracking monosilane into the pores of the porous carbon 3;

[0052] S2 Surface oxidation of silicon-carbon composite negative electrode material: Surface oxidation of the silicon-carbon negative electrode material formed in step S1;

[0053] S3 aluminothermic reduction to form an Al2O3 layer: the silicon-carbon negative electrode material whose surface is oxidized in step S2 is subjected to an aluminothermic reduction reaction using aluminum powder to form an Al2O3 layer 2 on the outside of the porous carbon 3;

[0054] S4 performs carbon coating: introducing organic gas to perform carbon coating on the outer side of the Al2O3 layer 2 to form a carbon coating layer 1;

[0055] The specific implementation method of S1 porous carbon vapor deposition silicon is as follows:

[0056] Select Dv50 = 4um and pore volume of 0.9cm 3 / g, the pore size of pores <2nm accounts for 75%, compared with 1700m 2 The spherical porous carbon is placed in a rotary kiln, and the inside of the rotary kiln is evacuated with nitrogen for 2 hours (the purpose is to completely exhaust the oxygen-containing gas in the rotary kiln), and the nitrogen flow rate is 5L / min; then the rotary kiln is heated to 600°C at a rate of 10°C / min; at this time, SiH4 gas is introduced for 6 hours to perform a vapor phase silicon deposition process on the porous carbon 3 to fill the pores inside the porous carbon 3 with amorphous silicon 4 to form a silicon-carbon negative electrode material;

[0057] The specific implementation method of surface oxidation of S2 silicon-carbon composite negative electrode material is as follows:

[0058] NO2 is introduced into the rotary kiln at a flow rate of 1 L / min for 1 hour to oxidize the surface of the formed silicon-carbon negative electrode material, and then the introduction of oxidizing gas into the rotary kiln is stopped and the silicon-carbon negative electrode material is allowed to cool naturally before being discharged from the rotary kiln; at the same time, it is required that after the silicon-carbon negative electrode material is introduced into the oxidizing gas, the overall oxygen content of the silicon-carbon negative electrode material is between 2 and 4 wt%;

[0059] The specific implementation method of S3 aluminothermic reduction to form Al2O3 layer is as follows:

[0060] The surface-oxidized silicon-carbon negative electrode material obtained in step S2 is mixed with aluminum powder with a particle size of less than 200 meshes in a mixer at high speed for 2 hours; then the silicon-carbon negative electrode material mixed with aluminum powder is placed in a rotary kiln, and the rotary kiln is evacuated with nitrogen for 2 hours, the nitrogen flow rate is 5L / min, the temperature is increased to 750°C at 5°C / min, and the temperature is kept for 15 hours for aluminothermic reduction reaction; at the same time, the ratio of aluminum powder to the silicon-carbon composite negative electrode material is 3.6wt%;

[0061] The specific implementation method of carbon coating in S4 is as follows:

[0062] Into the rotary kiln, propylene organic gas is introduced to carbon-coat the outer side of the Al2O3 layer 2 formed in step S3 for 6 hours to form a carbon coating layer 1, and then naturally cooled, the flow rate of propylene is 1L / min, and the processed silicon-carbon negative electrode material with reduced interface side reactions is taken out;

[0063] Example 3

[0064] See also Figure 1 , a silicon-carbon negative electrode material for reducing interface side reactions provided in an embodiment of the present invention, the silicon-carbon negative electrode material for reducing interface side reactions comprises:

[0065] Porous carbon 3, porous carbon 3 is a spherical porous carbon with Dv50=3-10um, and the pore volume of porous carbon 3 is required to be 0.7-1.1cm 3 / g, the pore size requirement is that the pores with diameter less than 2nm account for more than 70%, and the surface area requirement is 1500~2000m 2 / g; the interior of the porous carbon 3 is filled with nano-scale amorphous silicon 4 by a vapor phase silicon deposition process; an Al2O3 layer 2 is formed on the periphery of the porous carbon 3 by an aluminothermic reduction reaction; and a carbon coating layer 1 is coated on the periphery of the Al2O3 layer 2;

[0066] The method for preparing the silicon-carbon negative electrode material for reducing interface side reactions comprises the following steps:

[0067] S1 Porous carbon vapor deposition silicon: Select porous carbon 3 that meets the raw material requirements and fill amorphous silicon 4 in the pores of the porous carbon 3 through the vapor deposition silicon process to form a silicon-carbon negative electrode material; the vapor deposition silicon process is to fill the nano-silicon formed by cracking monosilane into the pores of the porous carbon 3;

[0068] S2 Surface oxidation of silicon-carbon composite negative electrode material: Surface oxidation of the silicon-carbon negative electrode material formed in step S1;

[0069] S3 aluminothermic reduction to form an Al2O3 layer: the silicon-carbon negative electrode material whose surface is oxidized in step S2 is subjected to an aluminothermic reduction reaction using aluminum powder to form an Al2O3 layer 2 on the outside of the porous carbon 3;

[0070] S4 performs carbon coating: introducing organic gas to perform carbon coating on the outer side of the Al2O3 layer 2 to form a carbon coating layer 1;

[0071] The specific implementation method of S1 porous carbon vapor deposition silicon is as follows:

[0072] Select Dv50 = 4um and pore volume of 0.9cm 3 / g, the pore size of pores <2nm accounts for 75%, compared with 1700m 2 The spherical porous carbon is placed in a rotary kiln, and the inside of the rotary kiln is evacuated with nitrogen for 2 hours (the purpose is to completely exhaust the oxygen-containing gas in the rotary kiln), and the nitrogen flow rate is 5L / min; then the rotary kiln is heated to 600°C at a rate of 10°C / min; at this time, SiH4 gas is introduced for 6 hours to perform a vapor phase silicon deposition process on the porous carbon 3 to fill the pores inside the porous carbon 3 with amorphous silicon 4 to form a silicon-carbon negative electrode material;

[0073] The specific implementation method of surface oxidation of S2 silicon-carbon composite negative electrode material is as follows:

[0074] Water vapor is introduced into the rotary kiln at a flow rate of 1 L / min for 1 hour to oxidize the surface of the formed silicon-carbon negative electrode material, and then the introduction of oxidizing gas into the rotary kiln is stopped and the silicon-carbon negative electrode material is allowed to cool naturally before being discharged from the rotary kiln; at the same time, it is required that after the silicon-carbon negative electrode material is introduced into the oxidizing gas, the overall oxygen content of the silicon-carbon negative electrode material is between 2 and 4 wt%;

[0075] The specific implementation method of S3 aluminothermic reduction to form Al2O3 layer is as follows:

[0076] The surface-oxidized silicon-carbon negative electrode material obtained in step S2 is mixed with aluminum powder with a particle size of less than 200 meshes in a mixer at high speed for 2 hours; then the silicon-carbon negative electrode material mixed with aluminum powder is placed in a rotary kiln, and the rotary kiln is evacuated with nitrogen for 2 hours, the nitrogen flow rate is 5L / min, the temperature is increased to 750°C at 5°C / min, and the temperature is kept for 15 hours for aluminothermic reduction reaction; at the same time, the ratio of aluminum powder to the silicon-carbon composite negative electrode material is 4.4wt%;

[0077] The specific implementation method of carbon coating in S4 is as follows:

[0078] Into the rotary kiln, introduce methane organic gas to carbon-coat the outer side of the Al2O3 layer 2 formed in step S3 for 6 hours to form a carbon coating layer 1, and then cool naturally, the flow rate of methane is 1L / min, and the processed silicon-carbon negative electrode material with reduced interface side reactions is taken out;

[0079] Example 4

[0080] See also Figure 1 , a silicon-carbon negative electrode material for reducing interface side reactions provided in an embodiment of the present invention, the silicon-carbon negative electrode material for reducing interface side reactions comprises:

[0081] Porous carbon 3, porous carbon 3 is a spherical porous carbon with Dv50=3-10um, and the pore volume of porous carbon 3 is required to be 0.7-1.1cm 3 / g, the pore size requirement is that the pores with diameter less than 2nm account for more than 70%, and the surface area requirement is 1500~2000m 2 / g; the interior of the porous carbon 3 is filled with nano-scale amorphous silicon 4 by a vapor phase silicon deposition process; an Al2O3 layer 2 is formed on the periphery of the porous carbon 3 by an aluminothermic reduction reaction; and a carbon coating layer 1 is coated on the periphery of the Al2O3 layer 2;

[0082] The method for preparing the silicon-carbon negative electrode material for reducing interface side reactions comprises the following steps:

[0083] S1 Porous carbon vapor deposition silicon: Select porous carbon 3 that meets the raw material requirements and fill amorphous silicon 4 in the pores of the porous carbon 3 through the vapor deposition silicon process to form a silicon-carbon negative electrode material; the vapor deposition silicon process is to fill the nano-silicon formed by cracking monosilane into the pores of the porous carbon 3;

[0084] S2 Surface oxidation of silicon-carbon composite negative electrode material: Surface oxidation of the silicon-carbon negative electrode material formed in step S1;

[0085] S3 aluminothermic reduction to form an Al2O3 layer: the silicon-carbon negative electrode material whose surface is oxidized in step S2 is subjected to an aluminothermic reduction reaction using aluminum powder to form an Al2O3 layer 2 on the outside of the porous carbon 3;

[0086] S4 performs carbon coating: introducing organic gas to perform carbon coating on the outer side of the Al2O3 layer 2 to form a carbon coating layer 1;

[0087] The specific implementation method of S1 porous carbon vapor deposition silicon is as follows:

[0088] Select Dv50 = 4um and pore volume of 0.9cm 3 / g, the pore size of pores <2nm accounts for 75%, compared with 1700m2 The spherical porous carbon is placed in a rotary kiln, and the inside of the rotary kiln is evacuated with nitrogen for 2 hours (the purpose is to completely exhaust the oxygen-containing gas in the rotary kiln), and the nitrogen flow rate is 5L / min; then the rotary kiln is heated to 600°C at a rate of 10°C / min; at this time, SiH4 gas is introduced for 6 hours to perform a vapor phase silicon deposition process on the porous carbon 3 to fill the pores inside the porous carbon 3 with amorphous silicon 4 to form a silicon-carbon negative electrode material;

[0089] The specific implementation method of surface oxidation of S2 silicon-carbon composite negative electrode material is as follows:

[0090] CO2 is introduced into the rotary kiln at a flow rate of 1 L / min for 1 hour to oxidize the surface of the formed silicon-carbon negative electrode material, and then the introduction of oxidizing gas into the rotary kiln is stopped and the silicon-carbon negative electrode material is allowed to cool naturally before being discharged from the rotary kiln; at the same time, it is required that after the silicon-carbon negative electrode material is introduced into the oxidizing gas, the overall oxygen content of the silicon-carbon negative electrode material is between 2 and 4 wt%;

[0091] The specific implementation method of S3 aluminothermic reduction to form Al2O3 layer is as follows:

[0092] The surface-oxidized silicon-carbon negative electrode material obtained in step S2 is mixed with aluminum powder with a particle size of less than 200 meshes in a mixer at high speed for 2 hours; then the silicon-carbon negative electrode material mixed with aluminum powder is placed in a rotary kiln, and the rotary kiln is evacuated with nitrogen for 2 hours, the nitrogen flow rate is 5L / min, the temperature is increased to 750°C at 5°C / min, and the temperature is kept for 15 hours for aluminothermic reduction reaction; at the same time, the ratio of aluminum powder to the silicon-carbon composite negative electrode material is 3.6wt%;

[0093] The specific implementation method of carbon coating in S4 is as follows:

[0094] Into the rotary kiln, introduce methane organic gas to carbon-coat the outer side of the Al2O3 layer 2 formed in step S3 for 6 hours to form a carbon coating layer 1, and then cool naturally, the flow rate of methane is 1L / min, and the processed silicon-carbon negative electrode material with reduced interface side reactions is taken out;

[0095] Comparative Example:

[0096] Step S1: Dv50 = 4um, pore volume 0.9cm 3 / g, the pore size is less than 2nm, accounting for 75%, compared with 1700m 2 The spherical porous carbon is placed in a rotary kiln;

[0097] Step S2: The rotary kiln is emptied with a nitrogen flow rate of 5 L / min for 2 h; the rotary kiln is heated to 600° C. at 10° C. / min, SiH4 gas is introduced for 6 h, and SiH4 is turned off;

[0098] Step S3: acetylene was introduced into the rotary kiln at a flow rate of 1 L / min for carbon coating for 6 h;

[0099] By implementing four different embodiments and comparing them with the comparative examples, the physical and chemical parameters and electrical performance parameters obtained are shown in Table 1:

[0100] Table 1:

[0101]

[0102] From Table 1 we can draw the following conclusions:

[0103] 1. As the proportion of aluminum increases, the proportion of oxygen captured by the aluminothermic reduction reaction increases, which in turn improves the initial effect of the silicon-carbon composite material;

[0104] 2. With the increase of aluminum ratio, the proportion of oxygen captured by aluminothermic reduction reaction increases, and the proportion of Al2O3 increases, which increases the proportion of sp2 hybridized carbon formed in the process of catalytic cracking of organic carbon source, thereby improving the powder conductivity;

[0105] 3. As the proportion of aluminum increases, the proportion of oxygen captured by the aluminothermic reduction reaction increases, the proportion of Al2O3 increases, and the thickness of the Al2O3 layer increases, resulting in a decrease in the expansion performance of the silicon-carbon composite negative electrode material and a decrease in the proportion of the side reaction between exposed silicon and the electrolyte, thereby increasing the cycle stability;

[0106] In the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A silicon-carbon negative electrode material for reducing interface side reactions, comprising: The porous carbon (3) is a spherical porous carbon with a Dv50 of 3 to 10 μm, and the pore volume of the porous carbon (3) is required to be 0.7 to 1.1 cm 3 / g, the pore size requirement is less than 2nm and the proportion of pores is more than 70%, and the specific surface area is required to be between 1500 and 2000m 2 / g; it is characterized by: The interior of the porous carbon (3) is filled with nano-scale amorphous silicon (4) through a vapor deposition silicon process. The vapor deposition silicon process is to fill nano-silicon formed by cracking monosilane into the pores of the porous carbon (3); an Al2O3 layer (2) is formed on the periphery of the porous carbon (3) through an aluminothermic reduction reaction. The aluminothermic reduction reaction is to perform an aluminothermic reduction reaction using aluminum powder after surface oxidation of the silicon-carbon negative electrode material formed by the vapor deposition silicon process; and a carbon coating layer (1) is coated on the periphery of the Al2O3 layer (2).

2. A method for preparing a silicon-carbon negative electrode material for reducing interface side reactions as claimed in claim 1, characterized in that The following steps are involved: S1 Porous carbon vapor deposition silicon: Select porous carbon (3) that meets the raw material requirements and fill amorphous silicon (4) in the pores of the porous carbon (3) through a vapor deposition silicon process to form a silicon-carbon negative electrode material; S2 Surface oxidation of silicon-carbon composite negative electrode material: Surface oxidation of the silicon-carbon negative electrode material formed in step S1; S3 aluminothermic reduction to form an Al2O3 layer: the silicon-carbon negative electrode material whose surface is oxidized in step S2 is subjected to an aluminothermic reduction reaction using aluminum powder to form an Al2O3 layer (2) on the outside of the porous carbon (3); S4 performs carbon coating: introducing organic gas to perform carbon coating on the outside of the Al2O3 layer (2) to form a carbon coating layer (1).

3. The method for preparing a silicon-carbon negative electrode material for reducing interface side reactions according to claim 2, characterized in that: The specific implementation method of S1 porous carbon vapor deposition silicon is as follows: Spherical porous carbon with Dv50=3-10um is placed in a rotary kiln, and the interior of the rotary kiln is evacuated with nitrogen for 2 hours; the rotary kiln is then heated to 400-600°C at a rate of 10°C / min; SiH4 gas is introduced for 6 hours to perform a vapor phase silicon deposition process on the porous carbon (3), filling the pores inside the porous carbon (3) with amorphous silicon (4) to form a silicon-carbon negative electrode material.

4. The method for preparing a silicon-carbon negative electrode material for reducing interface side reactions according to claim 2, characterized in that: The specific implementation method of surface oxidation of S2 silicon-carbon composite negative electrode material is as follows: One or more oxidizing gases such as water vapor, ethanol vapor, N-methylpyrrolidone vapor, CO2, NO2, and air are introduced into the rotary kiln for 1 hour to oxidize the surface of the formed silicon-carbon negative electrode material, and then the introduction of the oxidizing gas into the rotary kiln is stopped and the silicon-carbon negative electrode material is allowed to cool naturally before being discharged from the rotary kiln; at the same time, it is required that after the silicon-carbon negative electrode material is introduced with the oxidizing gas, the overall oxygen content of the silicon-carbon negative electrode material is between 2 and 4wt%.

5. The method for preparing a silicon-carbon negative electrode material for reducing interface side reactions according to claim 2, characterized in that: The specific implementation method of S3 aluminothermic reduction to form Al2O3 layer is as follows: The surface oxidized silicon-carbon negative electrode material obtained in step S2 is mixed with aluminum powder with a particle size of less than 200 mesh in a mixer at high speed for 2 hours; then the silicon-carbon negative electrode material mixed with aluminum powder is placed in a rotary furnace, the rotary furnace is evacuated with nitrogen for 2 hours, the temperature is increased to 300-800°C at 5°C / min, and the temperature is kept for 5-40 hours for aluminum thermal reduction reaction; at the same time, the ratio of aluminum powder to the silicon-carbon composite negative electrode material is between 1 and 5wt%.

6. The method for preparing a silicon-carbon negative electrode material for reducing interface side reactions according to claim 2, characterized in that: The specific implementation method of carbon coating in S4 is: one or more organic gases such as methane, acetylene, ethylene, propylene, benzene, toluene, cyclopentane, etc. are introduced into a rotary kiln to carbon coat the outer side of the Al2O3 layer (2) formed in step S3 for 6 hours to form a carbon coating layer (1), and then naturally cool it to take out the processed silicon-carbon negative electrode material with reduced interface side reactions.