A sodium ion battery formation method, sodium ion battery and battery module

By forming a dense SEI film in a sodium ion battery at low temperature, and then dissolving the inorganic sodium salt through multiple charge and discharge at high temperature to form a loose SEI film, the problem of easy damage to the SEI film at high temperature is solved and sodium ions are improved Cycling stability and high temperature performance of the battery.

CN117559017BActive Publication Date: 2024-11-29JIANGSU ZOOLNASM ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311630409.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-30
Publication Date
2024-11-29
Estimated Expiration
2043-11-30

AI Technical Summary

Technical Problem

During the charging process of sodium ion batteries, the solid electrolyte interface mask (SEI) is easily damaged at high temperatures, resulting in poor battery circulation stability.

Method used

A dense first layer of SEI film is formed at a low temperature, and then the inorganic sodium salt is dissolved by multiple charge and discharge at a high temperature to form a loose second layer of SEI film to achieve a saturation state and improve the stability of the SEI film.

Benefits of technology

By forming a SEI film structure with dense inner layer and uniform outer layer, the cycle stability and high-temperature cycling performance of sodium ion batteries are significantly improved, the SEI film is damaged, and the capacity retention rate and volume change rate of the battery are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117559017B_ABST
    Figure CN117559017B_ABST
Patent Text Reader

Abstract

The present application discloses a sodium ion battery formation method, a sodium ion battery and a battery module, which relate to the field of battery preparation technology, and can improve the stability of the SEI film, thereby improving the cycle performance of the sodium ion battery. The specific scheme includes: charging the prepared sodium ion battery at a first rate to the first capacity of the sodium ion battery at a preset pressure and a first temperature to obtain a first sodium ion battery with a first layer of SEI film, and the first temperature is ‑25°C to ‑15°C; performing multiple charge and discharge treatments on the first sodium ion battery at a preset pressure and a second temperature to make the SEI film components dissolved in the electrolyte of the sodium ion battery reach a saturated state, and obtaining a target sodium ion battery with a target SEI film, and the second temperature is 40°C to 60°C, and the target SEI film includes a first layer of SEI film and a second SEI film formed on the first layer of SEI film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of battery preparation, and in particular to a formation method of a sodium ion battery, a sodium ion battery and a battery module. Background Art

[0002] As a new type of secondary battery, sodium-ion batteries have good application prospects in electric vehicles, power station energy storage and other fields. The state of the surface film of the negative electrode of sodium-ion batteries directly affects the battery's initial efficiency, cycle stability, etc., so the formation process is a crucial part of the battery manufacturing process.

[0003] At present, in the formation process of sodium ion batteries, at a certain charging potential, the sodium ions at the electrode / electrolyte interface react irreversibly with the solvent molecules in the electrolyte to form a passivation layer covering the surface of the carbon electrode, which is called the solid electrolyte interface (SEI). Since the main components of the SEI film include organic sodium salts and inorganic sodium salts, and the inorganic sodium salts have a higher solubility in the electrolyte, the damage of the SEI film will be more obvious at high temperatures. Therefore, how to improve the stability of the SEI film has become an urgent problem to be solved. Summary of the invention

[0004] The present application provides a sodium ion battery formation method, a sodium ion battery and a battery module, which can improve the stability of the SEI film.

[0005] In order to achieve the above objectives, this application adopts the following technical solutions:

[0006] In a first aspect of an embodiment of the present application, a formation method for a sodium ion battery is provided, the method comprising:

[0007] Under a preset pressure and a first temperature, charging the prepared sodium ion battery at a first rate to a first capacity of the sodium ion battery to obtain a first sodium ion battery having a first SEI film, wherein the first temperature is -25°C to -15°C;

[0008] At a preset pressure and a second temperature, the first sodium ion battery is subjected to multiple charge and discharge treatments to make the SEI membrane components dissolved in the electrolyte of the sodium ion battery reach a saturated state, thereby obtaining a target sodium ion battery having a target SEI membrane. The second temperature is 40° C. to 60° C., and the target SEI membrane includes a first SEI membrane and a second SEI membrane formed on the first SEI membrane.

[0009] In one embodiment, the charge and discharge process includes:

[0010] The first sodium ion battery is charged at a second rate to a second capacity of the sodium ion battery, and after standing for a preset time, is discharged at the second rate to a third capacity of the sodium ion battery.

[0011] In one embodiment, the first capacity is 15% to 20%, the second capacity is 30% to 50%, and the third capacity is 5% to 10%;

[0012] The first magnification is 0.01-0.05C, and the second magnification is 0.05-0.1C.

[0013] In one embodiment, after obtaining the formed sodium ion battery, the method further comprises:

[0014] The formed sodium ion battery is subjected to a second sealing and degassing treatment to obtain a formed target sodium ion battery.

[0015] In one embodiment, the preset pressure is 200-400 KPa, and the number of charge and discharge treatments is 2-6 times.

[0016] In one embodiment, the preset time is 0.5 to 5 hours.

[0017] In one embodiment, the electrolyte in the sodium ion battery includes: a non-aqueous organic solvent, a sodium salt, and an additive;

[0018] Non-aqueous organic solvents include cyclic carbonate compounds and chain carbonate compounds;

[0019] The additive includes a first additive, and the first additive includes sodium fluoride, sodium carbonate and sodium oxide.

[0020] In one embodiment, the additive further includes a second additive including vinylene carbonate, fluoroethylene carbonate, vinyl sulfate, and 1,3-propylene sultone.

[0021] In a second aspect of an embodiment of the present application, a sodium ion battery is provided. The sodium ion battery is prepared by the sodium ion battery formation method of the first aspect of the embodiment of the present application.

[0022] According to a third aspect of the embodiments of the present application, a battery module is provided. The battery module includes the sodium ion battery provided in the second aspect of the embodiments of the present application.

[0023] The beneficial effects brought by the technical solution provided by the embodiment of the present application include at least:

[0024] The sodium ion battery formation method provided in the embodiment of the present application is to charge the prepared sodium ion battery in a low temperature environment of -25°C to -15°C to form a first SEI film, and the SEI formed at low temperature is a dense and structurally stable SEI film, and then continue to charge in a high temperature environment of 40°C to 60°C, at which time a second SEI film is formed on the surface of the first SEI film, wherein the second SEI film is a loose SEI film, and the loose SEI film will be partially dissolved in the subsequent multiple charge and discharge processes in a high temperature environment, and due to the negative electrode of the sodium ion battery The inorganic sodium salt in the SEI film component has a high solubility in the electrolyte. Through multiple charge and discharge treatments in a high temperature environment of 40°C to 60°C, the second SEI film is formed and dissolved multiple times, and finally the solubility of the inorganic sodium salt in the electrolyte of the sodium ion battery reaches a saturated state. This can avoid the problem of SEI film damage caused by the electrolyte dissolving the SEI film again, and finally form a SEI film structure with a dense inner layer and a uniform and loose outer layer on the negative electrode surface of the sodium ion battery, thereby improving the stability of the SEI film of the sodium ion battery, and further improving the cycle stability of the sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a test result diagram of the normal temperature cycle capacity retention rate of the sodium ion battery in the embodiment of the present application;

[0026] Figure 2 This is a test result diagram of the volume change rate of the sodium ion battery cell in the embodiment of the present application;

[0027] Figure 3 This is a test result diagram of the high temperature storage capacity retention rate of the sodium ion battery in the embodiment of the present application;

[0028] Figure 4 This is a test result diagram of the high temperature storage capacity recovery rate of the sodium ion battery in the embodiment of the present application. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0030] For the following defined terms, these definitions shall apply unless a different definition is given in the claims or elsewhere in this specification. All numerical values, whether or not explicitly indicated, are defined herein as modified by the term "about". The term "about" generally refers to a numerical range that a person of ordinary skill in the art considers to be equivalent to the stated values ​​to produce substantially the same properties, functions, results, etc. A numerical range indicated by a lower value and a higher value is defined to include all numerical values ​​included in the numerical range and all subranges included in the numerical range.

[0031] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions.

[0032] The following describes a sodium ion battery formation method provided in an embodiment of the present application, the method comprising:

[0033] Under a preset pressure and a first temperature, charging the prepared sodium ion battery at a first rate to a first capacity of the sodium ion battery to obtain a first sodium ion battery having a first SEI film, wherein the first temperature is -25°C to -15°C;

[0034] At a preset pressure and a second temperature, the first sodium ion battery is subjected to multiple charge and discharge treatments to make the SEI membrane components dissolved in the electrolyte of the sodium ion battery reach a saturated state, thereby obtaining a target sodium ion battery having a target SEI membrane. The second temperature is 40° C. to 60° C., and the target SEI membrane includes a first SEI membrane and a second SEI membrane formed on the first SEI membrane.

[0035] The first temperature may be, but not limited to, -25°C to -15°C, and the second temperature may be, but not limited to, 40°C to 60°C.

[0036] The upper limit of the first temperature may be -15°C, -14°C, -13°C, -12°C and -11°C, and the lower limit of the first temperature may be -25°C, -24°C, -23°C, -22°C and -21°C. The upper limit of the second temperature may be 60°C, 58°C, 56°C, 54°C, 52°C, and the lower limit of the second temperature may be 40°C, 42°C, 46°C, 48°C, 50°C.

[0037] It should be noted that the process of generating the SEI film can be: under the charging potential, the sodium ions at the electrode / electrolyte interface react with the solvent molecules in the electrolyte to generate the SEI film covering the surface of the carbon electrode. The process of dissolving the SEI film can be: since the main components of the SEI film include organic sodium salts and inorganic sodium salts, and the inorganic sodium salts have a high solubility in the electrolyte, part of the SEI film will dissolve in the electrolyte during the static process or discharge process of the sodium ion battery.

[0038] The present invention forms a first SEI film by charging the prepared sodium ion battery in a low temperature environment of -25°C to -15°C. The SEI formed at low temperature is a dense and structurally stable SEI film. Then, the battery is charged in a high temperature environment of 40°C to 60°C. At this time, a second SEI film is formed on the surface of the first SEI film. The second SEI film is a loose SEI film. The loose SEI film will be partially dissolved in the subsequent multiple charge and discharge processes in a high temperature environment. In addition, since there is no SEI film component in the negative electrode of the sodium ion battery, the SEI film of the negative electrode of the sodium ion battery is not charged. Organic sodium salts have high solubility in electrolytes. Through multiple charge and discharge treatments in a high-temperature environment of 40°C to 60°C, the second SEI film is formed and dissolved multiple times, and finally the solubility of inorganic sodium salts in the electrolyte of the sodium ion battery reaches a saturated state. This can avoid the problem of SEI film damage caused by the electrolyte dissolving the SEI film again, and finally form a SEI film structure with a dense inner layer and a uniform and loose outer layer on the negative electrode surface of the sodium ion battery, thereby improving the stability of the SEI film of the sodium ion battery, and further improving the cycle stability of the sodium ion battery.

[0039] Optionally, the charge and discharge process includes: charging the first sodium ion battery at a second rate to a second capacity of the sodium ion battery, and discharging the first sodium ion battery at the second rate to a third capacity of the sodium ion battery after standing for a preset time.

[0040] The first capacity includes but is not limited to 15% to 20%, the second capacity includes but is not limited to 30% to 50%, and the third capacity includes but is not limited to 5% to 10%; the first rate includes but is not limited to 0.01 to 0.05C, and the second rate includes but is not limited to 0.05 to 0.1C. The uniformity of SEI film formation can be improved by charging and discharging at a small rate of 0.05 to 0.1C.

[0041] Specifically, the above process can be: charging the first sodium ion battery at a rate of 0.05-0.1C to 30%-50% of the sodium ion battery capacity, and after standing for a preset time, discharging at a rate of 0.05-0.1C to 5%-10% of the sodium ion battery capacity.

[0042] In addition, during the charging process, the SEI film is formed when the sodium ions are charged to 30% to 50% of the battery capacity. Therefore, after charging to 30% to 50% of the battery capacity, the battery can be discharged without fully charging, which can improve the formation efficiency.

[0043] Optionally, after obtaining the formed sodium ion battery, the method further comprises: performing a second sealing and degassing treatment on the formed sodium ion battery to obtain a formed target sodium ion battery.

[0044] Since multiple charge and discharge cycles will produce more gas in sodium-ion batteries, the cycle performance of sodium-ion batteries can be further improved through secondary degassing treatment.

[0045] Optionally, the preset pressure can be 200-400Kpa. It can be understood that since the prepared sodium ion battery is a soft pack battery, the preset pressure of 200-400Kpa prevents the battery from breaking and prevents the generation of gas in the sodium ion battery, thereby affecting the cycle performance of the sodium ion battery. The upper limit of the pressure can be but not limited to 400Kpa, 390Kpa, 380Kpa, 370Kpa, etc., and the lower limit of the pressure can be but not limited to 200Kpa, 210Kpa, 220Kpa, 230Kpa, etc.

[0046] The number of charge and discharge treatments is 2 to 6 times. The preset time can be 0.5 to 5 hours, that is, the above charge and discharge process is repeated 2 to 6 times. And it is still after each charge or discharge to avoid polarization problems during the charge and discharge process. The upper limit of the preset time can be but not limited to 5.0h, 4.8h, 4.6h, 4.4h, 4.2h, and the lower limit of the preset time can be but not limited to 0.5h, 0.7h, 0.9h, 1.1h, 1.3h.

[0047] Furthermore, the positive electrode material of the sodium-ion battery is easy to absorb water. Through multiple charge and discharge treatment methods, it can be ensured that the water in the positive electrode material is completely decomposed in the formation stage, ensuring that hydrogen is no longer generated due to the presence of water during subsequent cycles, and preventing water from reacting with sodium hexafluorophosphate in the electrolyte to generate hydrofluoric acid and corrode the electrode.

[0048] Optionally, the electrolyte used in the sodium ion battery includes: a non-aqueous organic solvent, a sodium salt and an additive; the non-aqueous organic solvent includes a cyclic carbonate compound and a chain carbonate compound; the additive includes a first additive, and the first additive includes sodium fluoride, sodium carbonate and sodium oxide.

[0049] By adding sodium fluoride, sodium carbonate and sodium oxide to the electrolyte at the same time, the density and uniformity of the SEI film can be increased and the dissolution degree of the SEI film can be reduced, thereby reducing the consumption of electrolyte and sodium ions, improving the cycle performance of sodium ion batteries, especially the cycle performance at high temperatures, and reducing the gas production of sodium ion batteries.

[0050] In addition, the additive further includes a second additive, and the second additive includes one or more of vinylene carbonate, fluoroethylene carbonate, vinyl sulfate, and 1,3-propene sultone.

[0051] By using the first additive and the second additive in combination, the density and uniformity of the SEI film can be further increased, and the dissolution degree of the SEI film can be reduced, thereby further reducing the consumption of electrolyte and sodium ions, thereby further improving the cycle performance of the sodium ion battery, especially the cycle performance at high temperature, and further reducing the gas production of the sodium ion battery.

[0052] Based on the formation method of the sodium ion battery provided in the above embodiment, the embodiment of the present application also provides a method for preparing a sodium ion battery, which specifically includes:

[0053] Will Na 1.2 Fe(SO4) 1.6 / CNT-5%, Super-p and polyvinylidene fluoride were dispersed in N-methylpyrrolidone at a mass ratio of 92:2:6 and mixed evenly to obtain a slurry. The slurry was coated on both surfaces of the carbon-coated aluminum foil, dried at 120°C under vacuum for 12 hours, and rolled to a compacted density of 2.0 g / cm 3 Finally, the positive electrode sheet is die-cut into a square positive electrode sheet with a width of 220 mm and a length of 138 m. The thickness of the carbon layer on the surface of the carbon-coated aluminum foil is 1 μm. In addition, the positive electrode material of the sodium ion battery can also be one or more of transition metal layered oxides, polyanion compounds, and Prussian blue analogs. These materials can be used alone or in combination of two or more.

[0054] Hard carbon, Super-p, styrene-butadiene rubber and carboxymethyl cellulose were dispersed in deionized water at a mass ratio of 95:1.5:2:1.5 and mixed to obtain a slurry. The slurry was coated on both surfaces of the aluminum foil, dried at 120°C under vacuum for 12 hours, and then rolled to a compacted density of 1.0 g / cm 3, and then weld the pole ears to obtain the negative electrode sheet. The negative electrode sheet is die-cut into a square negative electrode sheet with a width of 223 mm and a length of 140 m. The material, composition and manufacturing method of the negative electrode sheet may include any technology known in the prior art. The negative electrode sheet may include a negative electrode current collector and a negative electrode active material layer arranged on at least one surface of the negative electrode current collector. The material of the negative electrode current collector may be aluminum foil. The negative electrode active material layer includes a negative electrode active material. The negative electrode active material may include hard carbon. The negative electrode active material layer may include a negative electrode conductive agent. The negative electrode conductive agent may include, but is not limited to, one or more of conductive carbon black, carbon nanotubes, acetylene black and graphene. In addition, the negative electrode active material layer may include a negative electrode binder. The negative electrode binder may include, but is not limited to, one or more of styrene-butadiene rubber and carboxymethyl cellulose.

[0055] To prepare a sodium ion battery, the positive electrode sheet, the separator, and the negative electrode sheet are stacked in the order of positive electrode sheet, separator, and negative electrode sheet, and after being wound and fixed, they are placed in a semi-sealed aluminum-plastic film, and then after top sealing and side sealing, they are transferred to 85°C and dried under vacuum conditions for 48 hours, and then the electrolyte is injected and the sodium ion battery is obtained after vacuum packaging.

[0056] In one embodiment, the positive electrode surface density of the sodium ion battery is 17.55 mg / cm 2 , negative electrode surface density 6mg / cm 2 The number of stacking layers is 36 positive and 37 negative, and a prepared sodium ion battery is obtained, wherein the design capacity of the sodium ion battery is 22Ah.

[0057] The following is a specific embodiment of the present application for a prepared sodium ion battery, combined with the formation method of a sodium ion battery provided in the embodiment of the present application. The following examples describe the technical solution of the present application in more detail, and these examples are only used for illustrative purposes, because it is obvious to those skilled in the art to make various modifications and changes within the scope of the disclosure of the present application. The reagents used in the examples can be obtained by commercial purchase or synthesized according to conventional methods, and can be used directly without further treatment, and the instruments and devices used in the examples can be commercially available.

[0058] Example 1: For the prepared sodium ion battery, under the condition of 300KPa and -20°C, the sodium ion battery is charged to 20% of the capacity of the sodium ion battery at a rate of 0.01C; the temperature is adjusted to 45°C and left to stand for 2h; under the condition of 45°C, the sodium ion battery is charged to 40% of the capacity of the sodium ion battery at a rate of 0.05C, and left to stand for 3h, and then discharged to 10% of the battery capacity at a rate of 0.1C and left to stand for 3h. Repeat the above charging and discharging process 3 times to obtain a sodium ion battery that has been formed.

[0059] Example 2: For the prepared sodium ion battery, under the condition of 300KPa and -20°C, the sodium ion battery is charged to 20% of the capacity of the sodium ion battery at a rate of 0.01C; the temperature is adjusted to 45°C and left to stand for 2h; under the condition of 55°C, the sodium ion battery is charged to 40% of the capacity of the sodium ion battery at a rate of 0.05C and left to stand for 3h, and then discharged to 10% of the battery capacity at a rate of 0.1C and left to stand for 3h. Repeat the above charging and discharging process 3 times to obtain a sodium ion battery that has been formed.

[0060] Example 3, for the prepared sodium ion battery, under the condition of 300KPa pressure and -20°C temperature, the sodium ion battery is charged to 20% of the sodium ion battery capacity at a rate of 0.01C; the temperature is adjusted to 45°C and left to stand for 2h; under the condition of 55°C temperature, the sodium ion battery is charged to 40% of the sodium ion battery capacity at a rate of 0.1C, and left to stand for 3h, and then discharged to 10% of the battery capacity at a rate of 0.1C, and left to stand for 3h. Repeat the above charging and discharging process 3 times to obtain a sodium ion battery that has been formed.

[0061] Example 4: For the prepared sodium ion battery, the sodium ion battery is charged to 20% of the capacity of the sodium ion battery at a rate of 0.01C under a pressure of 300KPa and a temperature of -20°C; the temperature is adjusted to 45°C and left to stand for 2h; at a temperature of 55°C, the sodium ion battery is charged to 40% of the capacity of the sodium ion battery at a rate of 0.05C, and left to stand for 3h, and then discharged to 10% of the battery capacity at a rate of 0.1C and left to stand for 3h. Repeat the above charging and discharging process 6 times to obtain a sodium ion battery that has been formed.

[0062] In comparative example 1, the prepared sodium ion battery was charged to 40% of its capacity at a rate of 0.05C under a pressure of 300 KPa and a temperature of 25°C to obtain a formed sodium ion battery.

[0063] Comparative Example 2: For the prepared sodium ion battery, the sodium ion battery was charged to 20% of the capacity of the sodium ion battery at a rate of 0.01C under a pressure of 300KPa and a temperature of -20°C; the temperature was adjusted to 45°C and allowed to stand for 2h; at a temperature of 25°C, the sodium ion battery was charged to 40% of the capacity of the sodium ion battery at a rate of 0.05, and allowed to stand for 2h, and then discharged to 10% of the battery capacity and allowed to stand for 3h. The above charging and discharging process was repeated 3 times to obtain a sodium ion battery that had been formed.

[0064] Comparative Example 3: For the prepared sodium ion battery, the sodium ion battery was charged to 40% of the sodium ion battery capacity at a rate of 0.05C under a pressure of 300 KPa and a temperature of 45°C, and then discharged to 10% of the battery capacity after standing for 2 hours, and then stood for 3 hours. The above charging and discharging process was repeated 3 times to obtain a sodium ion battery that was formed.

[0065] Table 1 shows the cycle performance data of the sodium ion battery prepared by the sodium ion battery formation method provided in the above embodiments and comparative examples. According to the data comparison of the embodiments and comparative examples in Table 1, the cycle performance of the sodium ion battery prepared by the sodium ion battery formation method provided by the present application is significantly improved, whether it is the capacity retention rate, capacity cycle rate, volume change rate and capacity recovery rate of the sodium ion battery.

[0066] Table 1 Capacity retention rate of sodium ion batteries

[0067]

[0068] Further, the sodium ion batteries formed in Example 1 and Comparative Example 1 were tested for capacity retention at room temperature, and the specific test methods were as follows:

[0069] At 25°C, charge at 0.2C constant current to 4.5V, discharge at 0.2C constant current to 2V, test the discharge capacity of the sodium ion battery and record it as C0; repeat the cycle charge and discharge under the same conditions, measure the discharge capacity of the battery after the 500th cycle and record it as C1. The capacity retention rate of the sodium ion battery after 500 cycles at 25°C = C1 / C0×100%. Figure 1 The figure shows the test results of the normal temperature cycle capacity retention rate of the sodium ion battery after the formation of Example 1 and the sodium ion battery after the formation of Comparative Example 1. Figure 1 It can be seen that the room temperature cycle capacity retention rate of the sodium ion battery in Example 1 is significantly better than that in Comparative Example 1. Therefore, it can be explained that the formation method of the sodium ion battery provided in the embodiment of the present application can improve the room temperature cycle capacity retention rate of the sodium ion battery.

[0070] Further, the sodium ion batteries formed in Example 1 and Comparative Example 1 were tested for capacity retention at room temperature, and the specific test methods were as follows:

[0071] Under the condition of 55°C, the sodium ion battery is charged at a constant current of 0.2C to a voltage of 4.5V, and discharged at a constant current of 0.2C to a voltage of 2V, and the discharge capacity of the sodium ion battery is tested and recorded as C0; the cyclic charge and discharge is repeated under the same conditions as above, and the discharge capacity of the battery after the 300th cycle is measured and recorded as C1. The capacity retention rate of the sodium ion battery after 300 cycles at 55°C = C1 / C0×100%. The specific test results are shown in Table 1. It can be seen from Table 1 that the high-temperature cycle capacity retention rate of the sodium ion batteries of Example 1, Example 2, Example 3 and Example 4 is significantly better than the high-temperature cycle capacity retention rate of the sodium ion batteries of Comparative Example 1, Comparative Example 2 and Comparative Example 3. Therefore, it can be explained that the formation method of the sodium ion battery provided in the embodiment of the present application can improve the high-temperature cycle capacity retention rate of the sodium ion battery.

[0072] The volume change test was performed on the sodium ion batteries after the formation of Example 1, Example 2, Example 3, Example 4, Comparative Example 1, Comparative Example 2 and Comparative Example 3, respectively. The specific test method is as follows:

[0073] At 25°C, take a large enough container and fill it with a certain amount of water. Place the container with water on an electronic balance, fix the sodium-ion battery, and slowly immerse the battery in water, making sure that the battery does not come into contact with the container. At this time, the reading on the balance will change compared to before the battery entered the container. According to Archimedes' principle, the value of the change in the balance reading is the volume of the battery, recorded as V1. After cycling this battery cell for a certain number of times, repeat the above steps for testing, and record the volume as V2. The volume change rate (volume expansion rate) is (V2-V1) / V1. The test results are as follows: Figure 2 As shown, from Figure 2 It can be seen that the volume change rates of Example 1, Example 2, Example 3 and Example 4 are significantly smaller than the volume change rates of Comparative Example 1, Comparative Example 2 and Comparative Example 3. Therefore, it can be shown that the formation method of the sodium ion battery provided in the embodiment of the present application can significantly reduce the volume change rate of the sodium ion battery.

[0074] The sodium ion batteries formed in Example 1, Example 2, Example 3, Example 4, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were tested for high temperature storage capacity retention rate and capacity recovery rate, respectively. The specific test methods are as follows:

[0075] At 25°C, the sodium ion battery is charged to a voltage of 4.5V at a constant current of 0.2C, and discharged to a voltage of 2V at a constant current of 0.2C, and the discharge capacity of the sodium ion battery is tested and recorded as C0; under the same conditions as above, the battery is charged to 4.5V, and the battery is placed in a 55°C incubator for 7 days. After being taken out, it is placed at 25°C for 6 hours, and then discharged to 2V at a constant current of 0.2C, and the discharge capacity of the sodium ion battery is tested and recorded as C1; the sodium ion battery is then charged to a voltage of 4.5V at a constant current of 0.2C, and discharged to a voltage of 2V at a constant current of 0.2C, and the discharge capacity of the sodium ion battery is tested and recorded as C2; then the capacity retention rate of 55°C full charge and 7 days is C1 / C0*100%; the capacity recovery rate of 55°C full charge and 7 days is C2 / C0*100%; wherein, the test results of the capacity retention rate are as follows Figure 3 As shown in Figure 2, the test results of capacity recovery rate are as follows: Figure 4 As shown. Figure 3 and Figure 4 It can be seen that the capacity retention rate and capacity recovery rate of Example 1, Example 2, Example 3 and Example 4 are significantly greater than the capacity retention rate and capacity recovery rate of high temperature storage of Comparative Example 1, Comparative Example 2 and Comparative Example 3. Therefore, it can be explained that the formation method of the sodium ion battery provided in the embodiments of the present application can significantly improve the capacity retention rate and capacity recovery rate of the sodium ion battery in high temperature storage.

[0076] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0077] The above embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.

Claims

1. A formation method for a sodium ion battery, It is characterized in that The method comprises: Under a preset pressure and a first temperature, charging the prepared sodium ion battery at a first rate to a first capacity of the sodium ion battery to obtain a first sodium ion battery having a first SEI film, wherein the first temperature is -25°C to -15°C, and the first rate is 0.01 to 0.05C; The first sodium ion battery is subjected to multiple charge and discharge treatments at the preset pressure and the second temperature so that the SEI membrane components dissolved in the electrolyte of the sodium ion battery reach a saturated state, thereby obtaining a target sodium ion battery having a target SEI membrane, wherein the second temperature is 40° C. to 60° C., and the target SEI membrane includes the first SEI membrane and a second SEI membrane formed on the first SEI membrane.

2. The method according to claim 1, It is characterized in that The charge and discharge process comprises: The first sodium ion battery is charged at a second rate to a second capacity of the sodium ion battery, and after standing for a preset time, is discharged at the second rate to a third capacity of the sodium ion battery.

3. The method according to claim 2, It is characterized in that The first capacity is 15% to 20%, the second capacity is 30% to 50%, and the third capacity is 5% to 10%; The second magnification is 0.05-0.1C.

4. The method according to any one of claims 1 to 3, It is characterized in that After obtaining the target sodium ion battery having the target SEI film, the method further comprises: The target sodium ion battery is subjected to a second sealing and degassing treatment to obtain a formed target sodium ion battery.

5. The method according to claim 1, It is characterized in that The preset pressure is 200-400 KPa, and the number of times of charge and discharge treatment is 2-6 times.

6. The method according to claim 2, It is characterized in that The preset time is 0.5 to 5 hours.

7. The method according to claim 1, It is characterized in that The electrolyte in the sodium ion battery comprises: a non-aqueous organic solvent, a sodium salt and an additive; The non-aqueous organic solvent includes cyclic carbonate compounds and chain carbonate compounds; The additives include a first additive including sodium fluoride, sodium carbonate, and sodium oxide.

8. The method according to claim 7, It is characterized in that The additive further includes a second additive including vinylene carbonate, fluoroethylene carbonate, vinyl sulfate, and 1,3-propylene sultone.

9. A sodium ion battery, It is characterized in that The sodium ion battery is prepared by the sodium ion battery formation method according to any one of claims 1 to 8.

10. A battery module, It is characterized in that The battery module includes the sodium ion battery according to claim 9.

Citation Information

Patent Citations

  • Formation method for sodium ion cell or battery

    CN108140880A

  • Sodium oxide composite sodium-supplementing positive electrode active material, positive electrode material, positive electrode, sodium-ion battery and sodium supplementing method for electric formation of sodium-ion battery

    CN111293289A