Bismaleimide and preparation method thereof and method for preparing aviation heat-resistant mold plate

Through bismaleimide and its preparation method, the problem of poor dimensional stability of aviation temperature-resistant mold plates under high temperature conditions has been solved, dimensional stability and ease of operation under 200°C have been achieved, and the high temperature requirements in the aviation field have been met. application requirements.

CN117567346BActive Publication Date: 2024-10-29CHONGQING ANSHENG XINDA AVIATION TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311392825.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-25
Publication Date
2024-10-29
Estimated Expiration
2043-10-25

AI Technical Summary

Technical Problem

Existing aviation temperature-resistant mold plates have poor dimensional stability after repeated temperature resistance under high temperature conditions of 200°C. The main reason is that the performance of the main resin decreases in high and low temperature cycle environments, resulting in unstable thermal expansion coefficients, making it difficult to meet high temperature applications in the aviation field. Require.

Method used

Using bismaleimide and its preparation method, a dinitro compound is generated by reacting an alicyclic diol with a nitro acid compound, and then reacted with hydrazine hydrate and maleic anhydride, and finally dehydrated to obtain bismaleimide. imide acid, and obtain bismaleimide through dehydration reaction, which is used to prepare high-temperature-resistant composite sheets for aviation to ensure excellent dimensional stability at 200°C.

Benefits of technology

Bismaleimide can maintain excellent dimensional stability under high temperature conditions of 200°C, which significantly reduces application risks in the aviation field. It can remain in a liquid state for at least one day after heating, reducing the difficulty of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117567346B_ABST
    Figure CN117567346B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of high temperature resistant materials for aviation, and specifically relates to bismaleimide and a preparation method thereof and a method for preparing aviation heat resistant mold plate. The structural formula of the bismaleimide is: #imgabs0# wherein A is a single bond or is ‑C(O)NH(CH2)2C(O)‑, and Ra is selected from H or a carboxyl group. The bismaleimide of the present invention can be used to prepare high temperature resistant composite plates for aviation. Specifically, the high temperature resistant composite plates for aviation prepared using the bismaleimide of the present invention can still maintain excellent dimensional stability after repeated high temperature resistance for 200 times, which greatly reduces the risk of application in the aviation field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high temperature resistant materials for aviation, and in particular relates to bismaleimide and a preparation method thereof, and a method for preparing a heat resistant aviation mold plate. Background Art

[0002] In recent years, more and more composite sheets are used to replace metals in the aviation manufacturing field due to their low density, high strength, easy repair and shaping, and excellent processing performance. This reduces the potential application risk of stress concentration caused by scratches on metal parts. In the aviation field, any small flaw may cause the tragedy of aircraft destruction and death, so the dimensional stability of the material becomes particularly important, especially the stability at high temperatures.

[0003] However, the existing aviation heat-resistant mold plates will have CTE (coefficient of thermal expansion) instability after repeated heat resistance at 200°C. The main reason is that the performance of the main resin deteriorates in the repeated high and low temperature cycle environment, resulting in CTE changes. Ordinary epoxy resins and high-temperature resistant epoxy resins have poor dimensional stability under repeated high temperature conditions and are difficult to meet the requirements. Summary of the invention

[0004] The purpose of the present invention is to provide bismaleimide to solve the problem of poor repeated high temperature resistance dimensional stability of existing aviation heat-resistant mold plates.

[0005] The second object of the present invention is to provide a method for preparing bismaleimide to solve the problem of poor repeated high temperature dimensional stability of existing aviation heat-resistant mold plates.

[0006] The third object of the present invention is to provide a method for preparing an aviation heat-resistant mold plate material, so as to solve the problem of poor repeated high temperature resistance dimensional stability of existing aviation heat-resistant mold plates.

[0007] To achieve the above object, the technical solution of the present invention is:

[0008] Bismaleimide, the structural formula of the bismaleimide is: Wherein, A is a single bond or -C(O)NH(CH2)2C(O)-, and Ra is selected from H or carboxyl. The bismaleimide of the present invention can be used to prepare a high temperature resistant composite sheet for aviation. Specifically, the high temperature resistant composite sheet for aviation obtained by using the bismaleimide of the present invention can still maintain excellent dimensional stability after repeated high temperature resistance for 200 times, which greatly reduces the risk of application in the aviation field.

[0009] Moreover, the existing bismaleimide is basically solid, and after being heated and melted into a liquid, it quickly turns back to a solid once the temperature drops to room temperature, which makes it difficult to use. The bismaleimide of the present invention can remain in a liquid state for at least one day after being heated and melted, which has sufficient operation time and reduces the difficulty of use.

[0010] According to an embodiment of the present invention, the structural formula of the bismaleimide is selected from any one of the following structural formulas:

[0011]

[0012] The present invention also provides a method for preparing the bismaleimide described above, which comprises: mixing an alicyclic diol with a nitro acid compound, reacting to obtain a dinitro compound, wherein the nitro acid compound contains a nitro group, and further contains a carboxyl group or fluorine, and the alicyclic diol comprises tricyclododecanedimethanol; mixing the dinitro compound with hydrazine hydrate, performing a reduction reaction, and obtaining a diamino compound; mixing the diamino compound with maleic anhydride, performing a reaction, and obtaining bismaleimide acid; mixing the bismaleimide acid with a dehydrating agent, performing a dehydration reaction, and obtaining bismaleimide. Therefore, the bismaleimide prepared by the method of the present invention can be used to synthesize a high-performance bismaleimide polymer, which has excellent dimensional stability under high temperature conditions of 200°C; the bismaleimide prepared by the method of the present invention can be used to prepare high-temperature resistant composite panels for aviation. Specifically, the base fabric is treated with the bismaleimide prepared by the method of the present invention, and the obtained composite panel can still maintain excellent dimensional stability after repeated high temperature resistance for 200 times, which greatly reduces the risk of application in the aviation field.

[0013] According to an embodiment of the present invention, the alicyclic diol includes tricyclododecanedimethanol (TCD). The structural formula of tricyclododecanedimethanol (TCD) is:

[0014] The nitroacid compound includes at least one of p-nitrobenzoyl-β-alanine, 2-nitrobenzoic acid, 3-nitrobenzoic acid, 4-nitrobenzoic acid, 2-nitroterephthalic acid, 2-fluoro-5-nitrobenzoic acid, 3-fluoro-2-nitrobenzoic acid, 4-fluoro-2-nitrobenzoic acid, and 2-nitro-4-benzyloxy-5-methoxybenzoic acid.

[0015] The molar ratio of the alicyclic diol to the nitro acid compound is greater than 0.5 and less than or equal to 0.6, for example, 0.55. This is conducive to obtaining the dinitro compound efficiently.

[0016] The reaction of the alicyclic diol and the nitro acid compound is carried out under the protection of an inert gas, wherein the inert gas includes nitrogen.

[0017] The temperature for the reaction of the alicyclic diol and the nitro acid compound is 70-90° C., such as 70° C., 80° C., or 90° C. This is conducive to obtaining the dinitro compound efficiently.

[0018] The reaction time of the alicyclic diol and the nitro acid compound is 8 to 12 hours, for example, 8 hours, 9 hours, 10 hours, 11 hours, and 12 hours.

[0019] According to an embodiment of the present invention, a solvent is further added during the reaction of the alicyclic diol and the nitro acid compound, and the solvent may be dimethyl sulfoxide (DMSO) or thionyl chloride. For example, when the nitro acid compound contains fluorine, the solvent may be dimethyl sulfoxide.

[0020] According to an embodiment of the present invention, a catalyst is further added to the reaction of the alicyclic diol and the nitro acid compound, and the catalyst is concentrated sulfuric acid, thereby facilitating the generation of the dinitro compound.

[0021] According to an embodiment of the present invention, after the reaction of the alicyclic diol and the nitro acid compound is completed, the method further comprises the step of precipitating the product with an aqueous NaCl solution, followed by recrystallization.

[0022] According to an embodiment of the present invention, the molar ratio of the dinitro compound to the hydrazine hydrate is 1:(2.5-3), such as 1:2.5, 1:2.6, 1:2.7, 1:2.8, 1:2.9, 1:3. This is conducive to the complete reduction of the dinitro compound to generate the diamino compound.

[0023] The reduction reaction is further performed by adding an alcohol solvent, wherein the alcohol solvent includes but is not limited to anhydrous ethanol, and the reduction reaction is performed under reflux conditions.

[0024] According to an embodiment of the present invention, a palladium-carbon (Pd / C) catalyst is further added to the reduction reaction, thereby facilitating the generation of the diamino compound.

[0025] According to an embodiment of the present invention, the preparation of the diamino compound includes: mixing a dinitro compound with a palladium carbon catalyst and anhydrous ethanol, heating to reflux, slowly adding hydrazine hydrate to the reaction system through a dropping funnel, and after the addition is completed, refluxing for 12 hours to obtain the diamino compound.

[0026] According to an embodiment of the present invention, the molar ratio of the diamino compound to the maleic anhydride is 1:(2-2.5), such as 1:2, 1:2.1, 1:2.2, 1:2.3, 1:2.4, 1:2.5. This is conducive to the complete reaction of all diamino compounds to generate bismaleimide acid.

[0027] The reaction of the diamino compound and maleic anhydride is carried out under the protection of an inert gas, wherein the inert gas includes any one of nitrogen and argon.

[0028] The reaction temperature of the diamino compound and maleic anhydride is 20-30° C., for example, 20° C., 25° C., 30° C. Under this condition, bismaleimide acid can be efficiently generated.

[0029] The reaction time of the diamino compound and maleic anhydride is 2 to 4 hours, such as 2 hours, 3 hours, or 4 hours. Under such conditions, the diamino compound and maleic anhydride are conducive to complete reaction to generate bismaleimide acid.

[0030] According to an embodiment of the present invention, a solvent is further added during the reaction of the diamino compound and maleic anhydride, and the solvent includes at least one of dimethylformamide, dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone.

[0031] According to an embodiment of the present invention, the dehydrating agent comprises acetic anhydride.

[0032] A catalyst is also added to the dehydration reaction, and the catalyst includes at least one of magnesium acetate, sodium acetate, nickel acetate, cobalt acetate, magnesium chloride, cobalt chloride, magnesium sulfate, and cobalt sulfate.

[0033] The dehydration reaction is carried out under the protection of an inert gas, wherein the inert gas includes any one of nitrogen and argon.

[0034] The temperature of the dehydration reaction is 60-80° C., for example, 60° C., 70° C., 80° C. Under this condition, it is favorable for the bismaleimide acid to react with the dehydrating agent to obtain bismaleimide.

[0035] The dehydration reaction time is 2 to 4 hours, for example, 2 hours, 3 hours, or 4 hours. Under such conditions, the bismaleimide acid and the dehydrating agent react completely to obtain bismaleimide.

[0036] The bismaleimide prepared by the present invention can be used to prepare high temperature resistant products. For example, the bismaleimide prepared by the present invention can be used to prepare glass fiber or carbon fiber type high temperature resistant molding molds, or the bismaleimide prepared by the present invention can be used to prepare high temperature resistant tooling fixtures.

[0037] The present invention also provides a method for preparing an aviation heat-resistant mold plate material, the method comprising: providing a modified solution containing bismaleimide and a curing agent, the bismaleimide being the bismaleimide described above or being prepared using the method for preparing bismaleimide described above; the modified solution undergoes a polymerization reaction to obtain an aviation heat-resistant mold plate material; or the modified solution is used to treat a base fabric, so that the modified solution soaks the base fabric, heats it, and undergoes a polymerization reaction to obtain an aviation heat-resistant mold plate material. The aviation heat-resistant mold plate material prepared by the method has excellent dimensional stability, and under high temperature conditions of 200°C, it can maintain performance without degradation after repeated heat resistance (more than 200 times). At the same time, the method also has the advantage of fast processing rate, which can improve production efficiency.

[0038] According to an embodiment of the present invention, after providing bismaleimide, the method further comprises heating bismaleimide, melting bismaleimide from solid to liquid, and then cooling. Specifically, the heating temperature can be 140 ℃ -150 ℃, and the insulation time can be 4h, and when all bismaleimides are melted from solid to liquid, cool to room temperature. After the bismaleimide of the present invention is melted into liquid, it will remain in liquid state for a period of time (about 1 day), and then slowly turn back to solid, and use it when the bismaleimide is in liquid state.

[0039] According to an embodiment of the present invention, the mass ratio of the bismaleimide to the curing agent is 100:(20-35), for example, 100:20, 100:25, 100:30, 100:35.

[0040] The curing agent includes at least one of triphenylphosphine (TPP), 2,4,6-tris(dimethylaminomethyl)phenol (DMP-30), benzyldimethylamine (BDMA), o-hydroxybenzyldimethylamine (DMP-10), 4,4'-dimethylaminodiphenylmethane (TMD), tri-(2-ethylacetic acid) salt of 2,4,6-tris(dimethylaminomethyl)phenol, trioleate of 2,4,6-tris(dimethylaminomethyl)phenol, 2-methylimidazole, 2-methyl-4-ethylimidazole, dibenzoyl peroxide (BPO), tert-butyl perbenzoate (BPB), azobisisobutyronitrile (AIBN), and azobisisoheptylonitrile (ABVN). Different curing agents vary greatly in curing efficiency and curing temperature. In order to maximize the curing efficiency and reduce the curing temperature, technicians can select different curing agents and compound them in a certain ratio.

[0041] According to an embodiment of the present invention, the modified solution further includes a filler, a filler modifier and a diluent.

[0042] The mass ratio of the bismaleimide to the filler, the filler modifier, and the diluent is 100:(18-22):(0.4-1):(2-5), for example, 100:18:0.4:2, 100:20:0.5:2.5, and 100:22:1:5. Thus, the different components with specific contents cooperate with each other and support each other, so that the aviation heat-resistant mold plate has excellent dimensional stability after repeated heat resistance.

[0043] According to an embodiment of the present invention, the filler includes at least one of molten silicon micropowder, soft composite silicon micropowder, rounded crystalline silicon micropowder, and hollow glass microspheres.

[0044] The D50 of the filler is 20 μm-30 μm, and the D90 of the filler is 30 μm-40 μm.

[0045] The filler modifier is a silane coupling agent, which includes at least one of γ-(2,3-epoxypropoxy)propyltrimethoxysilane (Z-6040), 3-aminopropyltriethoxysilane (KH-550), γ-glycidyloxypropyltrimethoxysilane (KH-560), γ-methacryloxypropyltrimethoxysilane (KH-570), and N-phenyl-aminopropyltrimethoxysilane. The present invention uses a silane coupling agent as a filler modifier, and the silane coupling agent has two groups of different properties, one end of which is a vinyl, epoxy, amino, methacrylate, or sulfate group. etc. can react with the functional group of bismaleimide, thereby realizing the connection between the filler modifier and the organic polymer base material; the alkoxy group (such as methoxy group and ethoxy group) after hydrolysis at the other end can react with the Si-OH group on the surface of the silicon filler, and after four processes of hydrolysis, condensation, hydrogen bond formation and covalent bond formation, a strong Si-O-Si covalent bond is formed between the filler modifier and the silicon filler, which becomes the link between the resin or organic polymer base material and the silicon filler, improves the bonding force between the resin and the plate or filler, and then can improve the strength and other properties of the hard composite material reinforced with glass fiber or carbon fiber.

[0046] The diluent includes at least one of butyl glycidyl ether, 1,4-butanediol diglycidyl ether, ethylene glycol diglycidyl ether, phenyl glycidyl ether, benzyl glycidyl ether, o-cresyl glycidyl ether, and neopentyl glycol diglycidyl ether; thus, the diluent can not only effectively reduce the viscosity of the system, increase fluidity, and facilitate construction over a larger area, but also can effectively cross-link with the curing agent to form a spatial network structure, and has a certain promoting effect on the performance of the cured product.

[0047] According to an embodiment of the present invention, treating the base fabric with the modified solution includes: pouring the modified solution onto the base fabric, so that the modified solution soaks the base fabric. Subsequently, the reaction system is evacuated, and the reaction system is kept vacuum after the evacuation is completed. Subsequently, the reaction system is heated, and a polymerization reaction is carried out to obtain an aviation heat-resistant mold plate. Thus, by evacuating and maintaining the vacuum, a dense and bubble-free effect can be achieved. Further, the evacuation of the reaction system needs to be carried out slowly. When the vacuum degree of the reaction system reaches a certain degree (for example, when it reaches -0.065Mpa), the evacuation rate should be reduced (for example, more than 90% of the valves are closed), and the evacuation is continued slowly. For example, the vacuum degree of the reaction system can be evacuated to -0.01Mpa in 25 to 35 minutes, and then the vacuum is maintained for 2 to 4 hours. If the speed of evacuating the reaction system is too fast, the liquid is easily sucked out, and there is a problem of overflowing glue. Further, after the vacuum is maintained, the method also includes: observing whether bubbles are generated on the surface of the base fabric, and if bubbles are generated, it is necessary to continue evacuating.

[0048] According to an embodiment of the present invention, the temperature of the polymerization reaction is 150-200°C. Thus, bismaleimide can be polymerized to generate an aviation heat-resistant mold plate with high dimensional stability after repeated heat resistance. Specifically, the temperature of the reaction system can be gradually increased to 150°C and kept for 2-3 hours, then increased to 200°C, kept for 2-3 hours, and finally gradually cooled to room temperature to obtain an aviation heat-resistant mold plate.

[0049] According to an embodiment of the present invention, the base fabric includes at least one of carbon fiber non-woven fabric and glass fiber non-woven fabric.

[0050] According to an embodiment of the present invention, the weight ratio of the base fabric to the modified solution is (0.5-2):1, for example, 0.5:1, 1:1, 1.5:1, 2:1. DETAILED DESCRIPTION

[0051] The existing aviation heat-resistant mold sheet has the problem of poor dimensional stability in repeated high temperature resistance. In order to improve this technical problem, the present invention provides bismaleimide and its preparation method and a method for preparing aviation heat-resistant mold sheet. The structural formula of the bismaleimide is: Wherein, A is a single bond or -C(O)NH(CH2)2C(O)-, and Ra is selected from H or a carboxyl group. The bismaleimide of the present invention can be used to prepare a high temperature resistant composite sheet for aviation. Specifically, the high temperature resistant composite sheet for aviation obtained by using the bismaleimide of the present invention can still maintain excellent dimensional stability after repeated high temperature resistance for 200 times, which greatly reduces the risk of application in the aviation field.

[0052] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments.

[0053] The tricyclododecanedimethanol (TCD) used in the following examples is a commercially available product with CAS number: 26896-48-0.

[0054] Example 1

[0055] This embodiment provides bismaleimide and a method for preparing bismaleimide.

[0056] The method for preparing bismaleimide comprises the following steps:

[0057] Synthesis of dinitro compounds: Use 55 mol of alicyclic diol (tricyclododecanedimethanol (TCD)) and 100 mol of nitro acid compound (p-nitrobenzoyl-β-alanine) in dimethyl sulfoxide, stir and heat in a water bath at 70°C, and introduce nitrogen for protection. React for 10 hours, cool to room temperature, and then use NaCl (1 g of NaCl to 20 ml of water) aqueous solution to precipitate the product, and then use excess ethylene glycol methyl ether for recrystallization to obtain the dinitro compound with a yield of more than 80%.

[0058] Synthesis of diamino compounds: Add 40 mol of a dinitro compound and a palladium-carbon catalyst, heat anhydrous ethanol to reflux, and then slowly add 85% hydrazine hydrate through a constant pressure dropping funnel. The molar ratio of the dinitro compound to the hydrazine hydrate is 1:2.8. The addition is completed within 2 hours, and then reflux for 12 hours. The diamino compound is precipitated by standing, and the yield is greater than 90%.

[0059] Synthesis of bismaleimide acid: firstly add dimethylformamide as a solvent, then add 60 mol of maleic anhydride and 180 mol of ethyl acetate into a reaction kettle, stir until the solution turns into a transparent liquid, then add 30 mol of a diamino compound and introduce nitrogen protection, the solution turns yellow, reacts at 25°C for 2h, then filters, and heats and dries the filtered product to obtain bismaleimide acid, which is cooled to room temperature in a vacuum environment for standby use, with a yield greater than 90%.

[0060] Dehydration of bismaleimide acid: Add the obtained bismaleimide acid into a reaction kettle, then add magnesium acetate and acetic anhydride, introduce nitrogen protection, react at 70°C for 2h, filter, and recrystallize with acetic anhydride to obtain bismaleimide monomer 1, with a yield of more than 80%.

[0061] The structural formula of bismaleimide monomer 1 is shown below:

[0062]

[0063] In some embodiments of the present invention, in the step of synthesizing the dinitro compound, p-nitrobenzoyl-β-alanine can be replaced by any one of 2-nitrobenzoic acid, 3-nitrobenzoic acid, 4-nitrobenzoic acid, 2-nitroterephthalic acid, and 2-nitro-4-benzyloxy-5-methoxybenzoic acid in an equimolar amount.

[0064] Example 2

[0065] This embodiment provides bismaleimide and a method for preparing bismaleimide.

[0066] The method for preparing bismaleimide comprises the following steps:

[0067] Synthesis of dinitro compounds: Use 55 mol of alicyclic diol (tricyclododecanedimethanol (TCD)) and 100 mol of nitro acid compound (p-nitrobenzoyl-β-alanine) in the presence of thionyl chloride and concentrated sulfuric acid, stir and heat in a water bath at 70°C, and introduce nitrogen for protection. React for 10 hours, cool to room temperature, and then use NaCl (1 g of NaCl to 20 ml of water) aqueous solution to precipitate the product, and then use excess ethylene glycol methyl ether for recrystallization to obtain the dinitro compound with a yield greater than 80%.

[0068] Synthesis of diamino compounds: Add 40 mol of a dinitro compound and a palladium-carbon catalyst, heat anhydrous ethanol to reflux, and then slowly add 85% hydrazine hydrate through a constant pressure dropping funnel. The molar ratio of the dinitro compound to the hydrazine hydrate is 1:2.8. The addition is completed in about 2 hours, and then reflux for 12 hours. The diamino compound is precipitated by standing, and the yield is greater than 90%.

[0069] Synthesis of bismaleimide acid: firstly add dimethylformamide as a solvent, then add 60 mol of maleic anhydride and 180 mol of ethyl acetate into a reaction kettle, stir until the solution turns into a transparent liquid, then add 30 mol of a diamino compound and introduce nitrogen protection, the solution turns yellow, reacts at 25°C for 2h, then filters, and heats and dries the filtered product to obtain bismaleimide acid, which is cooled to room temperature in a vacuum environment for standby use, with a yield greater than 90%.

[0070] Dehydration of bismaleimide acid: Add the obtained bismaleimide acid into a reaction kettle, then add magnesium acetate and acetic anhydride, introduce nitrogen protection, react at 70°C for 2h, filter, and recrystallize with acetic anhydride to obtain bismaleimide monomer II, with a yield of more than 80%.

[0071] The structural formula of bismaleimide monomer II is as follows:

[0072]

[0073] In some embodiments of the present invention, in the step of synthesizing the dinitro compound, p-nitrobenzoyl-β-alanine can be replaced by any one of 2-nitrobenzoic acid, 3-nitrobenzoic acid, 4-nitrobenzoic acid, 2-nitroterephthalic acid, and 2-nitro-4-benzyloxy-5-methoxybenzoic acid in an equimolar amount.

[0074] Example 3

[0075] This embodiment provides bismaleimide and a method for preparing bismaleimide.

[0076] The method for preparing bismaleimide comprises the following steps:

[0077] Synthesis of dinitro compounds: Use 55 mol of alicyclic diol (tricyclododecanedimethanol (TCD)) and 100 mol of nitro acid compound (4-fluoro-2-nitrobenzoic acid) in dimethyl sulfoxide, stir and heat in a 70°C water bath, and introduce nitrogen for protection. React for 10 hours, cool to room temperature, and then use NaCl (1 g of NaCl to 20 ml of water) aqueous solution to precipitate the product, and then use excess ethylene glycol methyl ether for recrystallization to obtain the dinitro compound with a yield of more than 80%.

[0078] Synthesis of diamino compounds: Add 40 mol of a dinitro compound and a palladium-carbon catalyst, heat anhydrous ethanol to reflux, and then slowly add 85% hydrazine hydrate through a constant pressure dropping funnel. The molar ratio of the dinitro compound to the hydrazine hydrate is 1:2.8. The addition is completed in about 2 hours, and then reflux for 12 hours. The diamino compound is precipitated by standing, and the yield is greater than 90%.

[0079] Synthesis of bismaleimide acid: first add dimethylformamide as a solvent, then add 60 mol of maleic anhydride and 180 mol of ethyl acetate into the reactor, stir until the solution turns into a transparent liquid, then add 30 mol of a diamino compound and introduce nitrogen protection, the solution turns yellow, react at 25°C for 2h, then filter, and heat and dry the filtered product to obtain bismaleimide acid, cool to room temperature in a vacuum environment for use, and the yield is greater than 90%.

[0080] Dehydration of bismaleimide acid: Add the obtained bismaleimide acid into a reaction kettle, then add magnesium acetate and acetic anhydride, introduce nitrogen protection, react at 70°C for 2h, filter, and recrystallize with acetic anhydride to obtain bismaleimide monomer three, with a yield of more than 80%.

[0081] The bismaleimide monomers include compounds shown in the following formula:

[0082]

[0083] In some embodiments of the present invention, in the step of synthesizing the dinitro compound, 4-fluoro-2-nitrobenzoic acid can be replaced by any one of 2-fluoro-5-nitrobenzoic acid and 3-fluoro-2-nitrobenzoic acid in an equimolar amount.

[0084] The physical properties of the products prepared in Examples 1-3 are shown in Table 1 below.

[0085] Table 1 Physical properties of the products prepared in Examples 1-3

[0086]

[0087] Preparation Example 1: Preparation of bismaleimide polymer

[0088] The raw materials for preparing bismaleimide polymer are:

[0089] Bismaleimide monomer 1: 100g;

[0090] Diluent: butyl glycidyl ether 2.5g;

[0091] Curing agent: triphenylphosphine 5g, 2-methylimidazole 20g;

[0092] Filler: 20g fused silica powder;

[0093] Filler modifier: silane coupling agent, the silane coupling agent is 0.5g of 3-aminopropyltriethoxysilane (KH-550).

[0094] Bismaleimide polymer curing process:

[0095] 1) Take an appropriate amount of bismaleimide monomer and put it into a beaker, then put it into an oven, raise the temperature to 150°C, keep the temperature constant until the solid bismaleimide is completely melted into liquid (about 2h), then cool it down to room temperature for use;

[0096] 2) Weigh 100 g of liquefied bismaleimide monomer and 2.5 g of diluent; stir evenly under vacuum;

[0097] 3) Weigh 20g of molten silicon powder and 0.5g of 3-aminopropyltriethoxysilane (KH-550), and stir evenly under vacuum;

[0098] 4) Weigh 5 g of curing agent triphenylphosphine and 20 g of 2-methylimidazole, stir them evenly in vacuum to obtain a standby sample named BMIP1;

[0099] 5) Pour BMIP1 into an aluminum mold, put it into an oven, heat it to 150°C, keep it warm for 2 hours, then heat it to 200°C, keep it warm for 3 hours, and cool it naturally to obtain a bismaleimide polymer sample 1.

[0100] The performance test results of bismaleimide polymer sample 1 are shown in Table 2 below.

[0101] Table 2 Performance test results of bismaleimide polymer sample 1

[0102] Inspection items unit Test value hardness D 85-87 Glass transition temperature (Tg) ℃ 300 Coefficient of thermal expansion CTE (10-50℃) <![CDATA[10 -6 K -1 ]]> 40 Coefficient of thermal expansion CTE (150-200℃) <![CDATA[10 -6 K -1 ]]> 55 Bending Strength MPa 220 Flexural modulus MPa 8000

[0103] Preparation Example 2: Preparation of bismaleimide polymer

[0104] The raw materials for preparing bismaleimide polymer are:

[0105] Bismaleimide monomer 2: 100 g;

[0106] Diluent: butyl glycidyl ether 2.5g;

[0107] Curing agent: triphenylphosphine 5g, 2-methylimidazole 20g;

[0108] Filler: 20g fused silica powder;

[0109] Filler modifier: silane coupling agent, the silane coupling agent is 0.5g of 3-aminopropyltriethoxysilane (KH-550).

[0110] Bismaleimide polymer curing process:

[0111] 1) Take an appropriate amount of bismaleimide monomer II and put it into a beaker, then put it into an oven, raise the temperature to 150°C, keep the temperature constant until the solid bismaleimide is completely melted into liquid (about 2h), then cool it down to room temperature for standby use;

[0112] 2) Weigh 100 g of liquefied bismaleimide monomer and 2.5 g of diluent; stir evenly under vacuum;

[0113] 3) Weigh 20g of molten silicon powder and 0.5g of 3-aminopropyltriethoxysilane (KH-550), and stir evenly under vacuum;

[0114] 4) Weigh 5 g of curing agent triphenylphosphine and 20 g of 2-methylimidazole, stir them evenly in vacuum to obtain a standby sample named BMIP2;

[0115] 5) Pour BMIP2 into an aluminum mold, put it into an oven, heat it to 150°C, keep it warm for 2 hours, then heat it to 200°C, keep it warm for 3 hours, and cool it naturally to obtain bismaleimide polymer sample 2;

[0116] The performance test results of bismaleimide polymer sample 2 are shown in Table 3 below.

[0117] Table 3 Performance test results of bismaleimide polymer sample 2

[0118] Inspection items unit Test value hardness D 85-87 Glass transition temperature (Tg) ℃ 320 Coefficient of thermal expansion CTE (10-50℃) <![CDATA[10 -6 K -1 ]]> 38 Coefficient of thermal expansion CTE (150-200℃) <![CDATA[10 -6 K -1 ]]> 53 Bending Strength MPa 230 Flexural modulus MPa 8500

[0119] Preparation Example 3: Preparation of bismaleimide polymer

[0120] The raw materials for preparing bismaleimide polymer are:

[0121] Bismaleimide monomer 3: 100g;

[0122] Diluent: butyl glycidyl ether 2.5g;

[0123] Curing agent: triphenylphosphine 5g, 2-methylimidazole 20g;

[0124] Filler: 20g fused silica powder;

[0125] Filler modifier: silane coupling agent, the silane coupling agent is 0.5g of 3-aminopropyltriethoxysilane (KH-550).

[0126] Bismaleimide polymer curing process:

[0127] 1) Take an appropriate amount of bismaleimide monomer 3 and put it into a beaker, then put it into an oven, raise the temperature to 150°C, keep the temperature constant until the solid bismaleimide is completely melted into liquid (about 2h), then cool it down to room temperature for use;

[0128] 2) Weigh 100 g of liquefied bismaleimide monomer 3 and 2.5 g of diluent; stir evenly under vacuum;

[0129] 3) Weigh 20g of molten silicon powder and 0.5g of 3-aminopropyltriethoxysilane (KH-550), and stir evenly under vacuum;

[0130] 4) Weigh 5 g of curing agent triphenylphosphine and 20 g of 2-methylimidazole, stir them evenly in vacuum to obtain a standby sample named BMIP3;

[0131] 5) Pour BMIP3 into an aluminum mold, put it into an oven, heat it to 150°C, keep it warm for 2 hours, then heat it to 200°C, keep it warm for 3 hours, and cool it naturally to obtain bismaleimide polymer sample three.

[0132] The performance test results of bismaleimide polymer sample 3 are shown in Table 4 below.

[0133] Table 4 Performance test results of bismaleimide polymer sample 3

[0134] Inspection items unit Test value hardness D 90 Glass transition temperature (Tg) ℃ 340 Coefficient of thermal expansion CTE (10-50℃) <![CDATA[10 -6 K -1 ]]> 35 Coefficient of thermal expansion CTE (150-200℃) <![CDATA[10 -6 K -1 ]]> 50 Bending Strength MPa 300 Flexural modulus MPa 9500

[0135] The coefficient of thermal expansion of the bismaleimide polymer samples prepared in Preparation Examples 1-3 was tested. The CTE after heat resistance was first subjected to a heat resistance test, and then the CTE test was performed on the samples after the heat resistance. The heat resistance test in the present invention is to repeatedly heat the samples at a high temperature of 200°C for 200 times. The specific method is: put the sample into an oven, heat it directly from room temperature to 90°C, and then heat it to 200°C at a rate of 10°C every 10 minutes, keep it warm for 3 hours and then naturally cool it to room temperature, repeat it 200 times, and then perform a CTE test on the samples after the heat resistance, repeat the test 3 times for each sample, and calculate the average value. The test results are shown in Table 5.

[0136] Table 5 High temperature resistance test results of bismaleimide polymer samples

[0137]

[0138]

[0139] It can be seen from Table 5 that after repeated high temperature resistance tests, the thermal expansion coefficients of the bismaleimide polymer samples prepared in Preparation Examples 1-3 did not change, indicating that the bismaleimide polymer samples of the present invention have excellent repeated high temperature resistance dimensional stability.

[0140] Sample Example 1

[0141] This sample example provides a method for preparing aviation heat-resistant mold plates.

[0142] 1. Carbon fiber non-woven fabric impregnation: Pour the liquid BMIP1 containing bismaleimide onto the carbon fiber non-woven fabric and let it stand for 10 minutes until the liquid soaks all the carbon fiber non-woven fabric; the weight ratio of the carbon fiber non-woven fabric to BMIP1 is 0.5:1.

[0143] 2. Turn on the vacuum and slowly draw the vacuum to -0.01Mpa in 30 minutes, then maintain the vacuum for 2 hours.

[0144] 3. Heating and curing: gradually raise the temperature in the heating furnace to 150°C and keep it for 3 hours, then raise the temperature to 200°C, keep it for 2 hours, and finally gradually cool it down to room temperature to produce aviation heat-resistant mold plates.

[0145] The performance test results of the aviation heat-resistant mold plate prepared in Sample Example 1 are shown in Table 6 below.

[0146] Table 6 Performance test results of aviation heat-resistant mold plates

[0147]

[0148]

[0149] Sample Example 2

[0150] This sample example provides a method for preparing aviation heat-resistant mold plates.

[0151] 1. Carbon fiber non-woven fabric impregnation: Pour the liquid BMIP1 containing bismaleimide onto the carbon fiber non-woven fabric and let it stand for 10 minutes until the liquid has soaked all the carbon fiber non-woven fabric; the weight ratio of the carbon fiber non-woven fabric to BMIP1 is 1:1.

[0152] 2. Turn on the vacuum and slowly draw the vacuum to -0.01Mpa in 30 minutes, then maintain the vacuum for 2 hours.

[0153] 3. Heating and curing: gradually raise the temperature in the heating furnace to 150°C and keep it for 3 hours, then raise the temperature to 200°C, keep it for 2 hours, and finally gradually cool it down to room temperature to produce aviation heat-resistant mold plates.

[0154] The performance test results of the aviation heat-resistant mold plate prepared in Sample Example 2 are shown in Table 7 below.

[0155] Table 7 Performance test results of aviation heat-resistant mold plates

[0156] unit Test value density <![CDATA[g / cm 3 ]]> 1.68 Thermal expansion coefficient CTE horizontal (10-50℃) <![CDATA[10 -6 K -1 ]]> 15 Thermal expansion coefficient CTE transverse (150-200℃) <![CDATA[10 -6 K -1 ]]> 17 Thermal expansion coefficient CTE vertical (10-50℃) <![CDATA[10 -6 K -1 ]]> 34 Thermal expansion coefficient CTE vertical (150-200℃) <![CDATA[10 -6 K -1 ]]> 35 Bending Strength MPa 550 Flexural modulus MPa 12000 Impact strength <![CDATA[KJ / m 2 ]]> 149 Glass transition temperature (Tg) ℃ 300

[0157] Sample Example 3

[0158] This sample example provides a method for preparing aviation heat-resistant mold plates.

[0159] 1. Carbon fiber non-woven fabric impregnation: Pour the liquid BMIP2 containing bismaleimide onto the carbon fiber non-woven fabric and let it stand for 10 minutes until the liquid has soaked all the carbon fiber non-woven fabric; the weight ratio of the carbon fiber non-woven fabric to BMIP2 is 0.5:1.

[0160] 2. Turn on the vacuum and slowly draw the vacuum to -0.01Mpa in 30 minutes, then maintain the vacuum for 2 hours.

[0161] 3. Heating and curing: gradually raise the temperature in the heating furnace to 150°C and keep it for 3 hours, then raise the temperature to 200°C, keep it for 2 hours, and finally gradually cool it down to room temperature to produce aviation heat-resistant mold plates.

[0162] The performance test results of the aviation heat-resistant mold plate prepared in Sample Example 3 are shown in Table 8 below.

[0163] Table 8 Performance test results of aviation heat-resistant mold plates

[0164] Inspection items unit Test value density <![CDATA[g / cm 3 ]]> 1.61 Thermal expansion coefficient CTE horizontal (10-50℃) <![CDATA[10 -6 K -1 ]]> 15 Thermal expansion coefficient CTE transverse (150-200℃) <![CDATA[10 -6 K -1 ]]> 17 Thermal expansion coefficient CTE vertical (10-50℃) <![CDATA[10 -6 K -1 ]]> 32 Thermal expansion coefficient CTE vertical (150-200℃) <![CDATA[10 -6 K -1 ]]> 35 Bending Strength MPa 480 Flexural modulus MPa 11500 Impact strength <![CDATA[KJ / m 2 ]]> 140 Glass transition temperature (Tg) ℃ 320

[0165] Sample Example 4

[0166] This sample example provides a method for preparing aviation heat-resistant mold plates.

[0167] 1. Carbon fiber non-woven fabric impregnation: Pour liquid BMIP2 containing bismaleimide onto the carbon fiber non-woven fabric and let it stand for 10 minutes until the liquid has soaked all the carbon fiber non-woven fabric; the weight ratio of the carbon fiber non-woven fabric to BMIP2 is 1:1.

[0168] 2. Turn on the vacuum and slowly draw the vacuum to -0.01Mpa in 30 minutes, then maintain the vacuum for 2 hours.

[0169] 3. Heating and curing: gradually raise the temperature in the heating furnace to 150°C and keep it for 3 hours, then raise the temperature to 200°C, keep it for 2 hours, and finally gradually cool it down to room temperature to produce aviation heat-resistant mold plates.

[0170] The performance test results of the aviation heat-resistant mold plate prepared in Sample Example 4 are shown in Table 9 below.

[0171] Table 9 Performance test results of aviation heat-resistant mold plates

[0172] Inspection items unit Test value density <![CDATA[g / cm 3 ]]> 1.68 Thermal expansion coefficient CTE horizontal (10-50℃) <![CDATA[10 -6 K -1 ]]> 15 Thermal expansion coefficient CTE transverse (150-200℃) <![CDATA[10 -6 K -1 ]]> 17 Thermal expansion coefficient CTE vertical (10-50℃) <![CDATA[10 -6 K -1 ]]> 33 Thermal expansion coefficient CTE vertical (150-200℃) <![CDATA[10 -6 K -1 ]]> 35 Bending Strength MPa 580 Flexural modulus MPa 12500 Impact strength <![CDATA[KJ / m 2 ]]> 144 Glass transition temperature (Tg) ℃ 320

[0173] Sample Example 5

[0174] This sample example provides a method for preparing aviation heat-resistant mold plates.

[0175] 1. Carbon fiber non-woven fabric impregnation: Pour liquid BMIP3 containing bismaleimide onto the carbon fiber non-woven fabric and let it stand for 10 minutes until the liquid soaks all the carbon fiber non-woven fabric; the weight ratio of carbon fiber non-woven fabric to BMIP3 is 0.5:1.

[0176] 2. Turn on the vacuum and slowly draw the vacuum to -0.01Mpa in 30 minutes, then maintain the vacuum for 2 hours.

[0177] 3. Heating and curing: gradually raise the temperature in the heating furnace to 150°C and keep it for 3 hours, then raise the temperature to 200°C, keep it for 2 hours, and finally gradually cool it down to room temperature to produce aviation heat-resistant mold plates.

[0178] The performance test results of the aviation heat-resistant mold plate prepared in Sample Example 5 are shown in Table 10 below.

[0179] Table 10 Performance test results of aviation heat-resistant mold plates

[0180]

[0181]

[0182] Sample Example 6

[0183] This sample example provides a method for preparing aviation heat-resistant mold plates.

[0184] 1. Carbon fiber non-woven fabric impregnation: Pour liquid BMIP3 containing bismaleimide onto the carbon fiber non-woven fabric and let it stand for 10 minutes until the liquid has soaked all the carbon fiber non-woven fabric; the weight ratio of the carbon fiber non-woven fabric to BMIP3 is 1:1.

[0185] 2. Turn on the vacuum and slowly draw the vacuum to -0.01Mpa in 30 minutes, then maintain the vacuum for 2 hours.

[0186] 3. Heating and curing: gradually raise the temperature in the heating furnace to 150°C and keep it for 3 hours, then raise the temperature to 200°C, keep it for 2 hours, and finally gradually cool it down to room temperature to produce aviation heat-resistant mold plates.

[0187] The performance test results of the aviation heat-resistant mold plate prepared in Sample Example 6 are shown in Table 11 below.

[0188] Table 11 Performance test results of aviation heat-resistant mold plates

[0189]

[0190]

[0191] Sample Example 7

[0192] This sample example provides a method for preparing aviation heat-resistant mold plates.

[0193] 1. Infiltration of glass fiber non-woven fabric: Pour the liquid BMIP1 containing bismaleimide onto the glass fiber non-woven fabric and let it stand for 10 minutes until the liquid soaks all the glass fiber non-woven fabric; the weight ratio of glass fiber non-woven fabric to BMIP1 is 0.5:1.

[0194] 2. Turn on the vacuum and slowly draw the vacuum to -0.01Mpa in 30 minutes, then maintain the vacuum for 2 hours.

[0195] 3. Heating and curing: gradually raise the temperature in the heating furnace to 150°C and keep it for 3 hours, then raise the temperature to 200°C, keep it for 2 hours, and finally gradually cool it down to room temperature to produce aviation heat-resistant mold plates.

[0196] The performance test results of the aviation heat-resistant mold plate prepared in Sample Example 7 are shown in Table 12 below.

[0197] Table 12 Performance test results of aviation heat-resistant mold plates

[0198] Inspection items unit Test value density <![CDATA[g / cm 3 ]]> 1.91 Thermal expansion coefficient CTE horizontal (10-50℃) <![CDATA[10 -6 K -1 ]]> 23 Thermal expansion coefficient CTE transverse (150-200℃) <![CDATA[10 -6 K -1 ]]> 25 Thermal expansion coefficient CTE vertical (10-50℃) <![CDATA[10 -6 K -1 ]]> 35 Thermal expansion coefficient CTE vertical (150-200℃) <![CDATA[10 -6 K -1 ]]> 37 Bending Strength MPa 350 Flexural modulus MPa 9000 Impact strength <![CDATA[KJ / m 2 ]]> 109 Glass transition temperature (Tg) ℃ 300

[0199] Sample Example 8

[0200] This sample example provides a method for preparing aviation heat-resistant mold plates.

[0201] 1. Infiltration of glass fiber non-woven fabric: Pour the liquid BMIP1 containing bismaleimide onto the glass fiber non-woven fabric and let it stand for 10 minutes until the liquid soaks all the glass fiber non-woven fabric; the weight ratio of glass fiber non-woven fabric to BMIP1 is 1:1.

[0202] 2. Turn on the vacuum and slowly draw the vacuum to -0.01Mpa in 30 minutes, then maintain the vacuum for 2 hours.

[0203] 3. Heating and curing: gradually raise the temperature in the heating furnace to 150°C and keep it for 3 hours, then raise the temperature to 200°C, keep it for 2 hours, and finally gradually cool it down to room temperature to produce aviation heat-resistant mold plates.

[0204] The performance test results of the aviation heat-resistant mold plate prepared in Sample Example 8 are shown in Table 13 below.

[0205] Table 13 Performance test results of aviation heat-resistant mold plates

[0206] Inspection items unit Test value density <![CDATA[g / cm 3 ]]> 1.99 Thermal expansion coefficient CTE horizontal (10-50℃) <![CDATA[10 -6 K -1 ]]> 21 Thermal expansion coefficient CTE transverse (150-200℃) <![CDATA[10 -6 K -1 ]]> 24 Thermal expansion coefficient CTE vertical (10-50℃) <![CDATA[10 -6 K -1 ]]> 34 Thermal expansion coefficient CTE vertical (150-200℃) <![CDATA[10 -6 K -1 ]]> 36 Bending Strength MPa 380 Flexural modulus MPa 9500 Impact strength <![CDATA[KJ / m 2 ]]> 112 Glass transition temperature (Tg) ℃ 300

[0207] Sample Example 9

[0208] This sample example provides a method for preparing aviation heat-resistant mold plates.

[0209] 1. Infiltration of glass fiber non-woven fabric: Pour the liquid BMIP2 containing bismaleimide onto the glass fiber non-woven fabric and let it stand for 10 minutes until the liquid soaks all the glass fiber non-woven fabric; the weight ratio of glass fiber non-woven fabric to BMIP2 is 0.5:1.

[0210] 2. Turn on the vacuum and slowly draw the vacuum to -0.01Mpa in 30 minutes, then maintain the vacuum for 2 hours.

[0211] 3. Heating and curing: gradually raise the temperature in the heating furnace to 150°C and keep it for 3 hours, then raise the temperature to 200°C, keep it for 2 hours, and finally gradually cool it down to room temperature to produce aviation heat-resistant mold plates.

[0212] The performance test results of the aviation heat-resistant mold plate prepared in Sample Example 9 are shown in Table 14 below.

[0213] Table 14 Performance test results of aviation heat-resistant mold plates

[0214] Inspection items unit Test value density <![CDATA[g / cm 3 ]]> 1.91 Thermal expansion coefficient CTE horizontal (10-50℃) <![CDATA[10 -6 K -1 ]]> 22 Thermal expansion coefficient CTE transverse (150-200℃) <![CDATA[10 -6 K -1 ]]> 25 Thermal expansion coefficient CTE vertical (10-50℃) <![CDATA[10 -6 K -1 ]]> 34 Thermal expansion coefficient CTE vertical (150-200℃) <![CDATA[10 -6 K -1 ]]> 35 Bending Strength MPa 380 Flexural modulus MPa 9200 Impact strength <![CDATA[KJ / m 2 ]]> 119 Glass transition temperature (Tg) ℃ 320

[0215] Sample Example 10

[0216] This sample example provides a method for preparing aviation heat-resistant mold plates.

[0217] 1. Infiltration of glass fiber non-woven fabric: Pour liquid BMIP2 containing bismaleimide onto the glass fiber non-woven fabric and let it stand for 10 minutes until the liquid soaks all the glass fiber non-woven fabric; the weight ratio of glass fiber non-woven fabric to BMIP2 is 1:1.

[0218] 2. Turn on the vacuum and slowly draw the vacuum to -0.01Mpa in 30 minutes, then maintain the vacuum for 2 hours.

[0219] 3. Heating and curing: gradually raise the temperature in the heating furnace to 150°C and keep it for 3 hours, then raise the temperature to 200°C, keep it for 2 hours, and finally gradually cool it down to room temperature to produce aviation heat-resistant mold plates.

[0220] The performance test results of the aviation heat-resistant mold plate prepared in Sample Example 10 are shown in Table 15 below.

[0221] Table 15 Performance test results of aviation heat-resistant mold plates

[0222]

[0223]

[0224] Sample Example 11

[0225] This sample example provides a method for preparing aviation heat-resistant mold plates.

[0226] 1. Infiltration of glass fiber non-woven fabric: Pour the liquid BMIP3 containing bismaleimide onto the glass fiber non-woven fabric and let it stand for 10 minutes until the liquid soaks all the glass fiber non-woven fabric; the weight ratio of glass fiber non-woven fabric to BMIP3 is 0.5:1.

[0227] 2. Turn on the vacuum and slowly draw the vacuum to -0.01Mpa in 30 minutes, then maintain the vacuum for 2 hours.

[0228] 3. Heating and curing: gradually raise the temperature in the heating furnace to 150°C and keep it for 3 hours, then raise the temperature to 200°C, keep it for 2 hours, and finally gradually cool it down to room temperature to produce aviation heat-resistant mold plates.

[0229] The performance test results of the aviation heat-resistant mold plate prepared in Sample Example 11 are shown in Table 16 below.

[0230] Table 16 Performance test results of aviation heat-resistant mold plates

[0231]

[0232]

[0233] Sample Example 12

[0234] This sample example provides a method for preparing aviation heat-resistant mold plates.

[0235] 1. Infiltration of glass fiber non-woven fabric: Pour liquid BMIP3 containing bismaleimide onto the glass fiber non-woven fabric and let it stand for 10 minutes until the liquid soaks all the glass fiber non-woven fabric; the weight ratio of glass fiber non-woven fabric to BMIP3 is 1:1.

[0236] 2. Turn on the vacuum and slowly draw the vacuum to -0.01Mpa in 30 minutes, then maintain the vacuum for 2 hours.

[0237] 3. Heating and curing: gradually raise the temperature in the heating furnace to 150°C and keep it for 3 hours, then raise the temperature to 200°C, keep it for 2 hours, and finally gradually cool it down to room temperature to produce aviation heat-resistant mold plates.

[0238] The performance test results of the aviation heat-resistant mold plate prepared in Sample Example 12 are shown in Table 17 below.

[0239] Table 17 Performance test results of aviation heat-resistant mold plates

[0240] Inspection items unit Test value density <![CDATA[g / cm 3 ]]> 1.99 Thermal expansion coefficient CTE horizontal (10-50℃) <![CDATA[10 -6 K -1 ]]> 21 Thermal expansion coefficient CTE transverse (150-200℃) <![CDATA[10 -6 K -1 ]]> 24 Thermal expansion coefficient CTE vertical (10-50℃) <![CDATA[10 -6 K -1 ]]> 30 Thermal expansion coefficient CTE vertical (150-200℃) <![CDATA[10 -6 K -1 ]]> 34 Bending Strength MPa 480 Flexural modulus MPa 12500 Impact strength <![CDATA[KJ / m 2 ]]> 112 Glass transition temperature (Tg) ℃ 340

[0241] From the test results of Preparation Example 1-3 and Sample Example 1-12, it can be seen that the modification of bismaleimide (BMI) by base fabric (carbon fiber non-woven fabric, glass fiber non-woven fabric) can further improve the comprehensive performance of the product, especially the lateral CTE has been greatly reduced. At the same time, due to the high temperature resistance of bismaleimide, the temperature resistance of the board prepared by Sample Example 1-12 is greatly improved compared with that of boards made of other resins, and can easily meet the long-term temperature resistance requirement of 200°C.

Claims

1. A method for preparing an aviation heat-resistant mold plate, characterized in that: The following steps are involved: A modified solution containing a functional compound and a curing agent is provided. The preparation method of the functional compound is as follows: an alicyclic diol is mixed with a nitro acid compound, and the mixture is reacted to obtain a dinitro compound, and the dinitro compound is then mixed with hydrazine hydrate, and the mixture is reduced to obtain a diamino compound; Then the diamino compound is mixed with maleic anhydride, reacted to obtain a precursor compound, and finally the precursor compound is mixed with a dehydrating agent, dehydrated to obtain a functional compound; the nitro acid compound is p-nitrobenzoyl-β-alanine and 4-fluoro-2-nitrobenzoic acid, and the alicyclic diol is tricyclododecanedimethanol with a CAS number of 26896-48-0; the molar ratio of the diamino compound to the maleic anhydride is 1:(2-2.5); The modified solution is subjected to polymerization reaction to obtain an aviation heat-resistant mold plate; or the modified solution is used to treat a base fabric, so that the modified solution infiltrates the base fabric, heats it, and performs polymerization reaction to obtain an aviation heat-resistant mold plate; the molar ratio of the alicyclic diol to the nitro acid compound is greater than 0.5 and less than or equal to 0.6; the temperature of the reaction of the alicyclic diol with the nitro acid compound is 70-90° C.; the reaction time of the alicyclic diol with the nitro acid compound is 8-12 hours; dimethyl sulfoxide or thionyl chloride is also added to the reaction of the alicyclic diol with the nitro acid compound.

2. The method for preparing the aviation heat-resistant mold plate according to claim 1, characterized in that: The molar ratio of the dinitro compound to the hydrazine hydrate is 1:(2.5-3); an alcohol solvent is also added to the reduction reaction, and the reduction reaction is carried out under reflux conditions.

3. The method for preparing the aviation heat-resistant mold plate according to claim 1, characterized in that: The reaction temperature of the diamino compound and the maleic anhydride is 20-30°C; The reaction time of the diamino compound and the maleic anhydride is 2 to 4 hours.

4. The method for preparing the aviation heat-resistant mold plate according to any one of claims 1 to 3, characterized in that: The dehydrating agent is acetic anhydride; A catalyst is also added to the dehydration reaction, wherein the catalyst is at least one of magnesium acetate, sodium acetate, nickel acetate, cobalt acetate, magnesium chloride, cobalt chloride, magnesium sulfate, and cobalt sulfate; The temperature of the dehydration reaction is 60-80°C; The dehydration reaction time is 2 to 4 hours.

5. The method for preparing the aviation heat-resistant mold plate according to claim 1, characterized in that: The mass ratio of the functional compound to the curing agent is 100: (20-35); The curing agent is at least one of triphenylphosphine, 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, o-hydroxybenzyldimethylamine, 4,4'-dimethylaminodiphenylmethane, tri-(2-ethylacetic acid) salt of 2,4,6-tris(dimethylaminomethyl)phenol, trioleate of 2,4,6-tris(dimethylaminomethyl)phenol, 2-methylimidazole, 2-methyl-4-ethylimidazole, dibenzoyl peroxide, tert-butyl perbenzoate, azobisisobutyronitrile, and azobisisoheptylonitrile.

6. The method for preparing the aviation heat-resistant mold plate according to claim 1, characterized in that: The modified solution also includes a filler, a filler modifier and a diluent; the filler modifier is a silane coupling agent.

7. The method for preparing the aviation heat-resistant mold plate according to claim 1, characterized in that: The polymerization reaction temperature is 150-200°C.

8. The method for preparing the aviation heat-resistant mold plate according to any one of claims 1 and 5 to 7, characterized in that: The base fabric is at least one of carbon fiber non-woven fabric and glass fiber non-woven fabric; The weight ratio of the base fabric to the modified solution is (0.5-2):1.

Citation Information

Patent Citations

  • High-temperature resistance high-toughness bismaleimide resin as well as preparation method and application thereof

    CN108276578A

  • Bismaleimide prepolymer with high solubility and good temperature resistant performance as well as preparation method and application thereof

    CN108395534A