Dye / salt separation loose nanofiltration membrane based on aminated nano-diamond-polyphenol-metal network as well as preparation method and application of dye / salt separation loose nanofiltration membrane

By aminating the loose nanofiltration membrane of the nanodiamond-polyphenol-metal network, the synergistic effect of nanodiamond and polyphenol-metal bilayer networks is solved, and the problem of poor dye/salt separation is achieved. Highly efficient dye/salt separation and high permeability flux, expanding the application of nanodiamond in the field of wastewater treatment.

CN118904119APending Publication Date: 2024-11-08NANJING SENFENG TECH CO LTD +2
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411078697.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional dense nanofiltration membranes have poor effect on dye/salt separation, and the water flux of ultrafiltration membranes with added inorganic nanoparticles decreases, making it difficult to achieve efficient dye/salt separation.

Method used

Using a loose nanofiltration membrane of aamlated nanodiamond-polyphenol-metal network, a high permeability flux and selective layer are formed through the synergistic effect of polyethyleneimine-modified nanodiamond and polyphenol-metal bilayer network to achieve dye Effective separation of /salt.

Benefits of technology

High organic dye retention rate, low inorganic salt retention rate and high permeability flux are achieved, which significantly improves the dye/salt separation effect and enhances the mechanical properties of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904119A_ABST
    Figure CN118904119A_ABST
Patent Text Reader

Abstract

The invention discloses a dye / salt separation loose nanofiltration membrane based on an aminated nano-diamond-polyphenol-metal network as well as a preparation method and application thereof, and belongs to the field of membrane separation of textile wastewater. The preparation method comprises the following steps: preparing a polyimide ultrafiltration base membrane by taking polyethyleneimine modified nano-diamond as an additive, sequentially soaking the polyimide ultrafiltration base membrane in a polyphenol solution and a metal salt solution, and assembling on the surface of the polyimide ultrafiltration base membrane to form an amino-polyphenol-metal double-layer network; the polyimide-based loose nanofiltration membrane containing the polyethyleneimine modified nano-diamond is prepared. The mechanical property and pure water flux of the prepared loose nanofiltration membrane are improved, the loose nanofiltration membrane has high dye retention rate and low inorganic salt retention rate, and efficient separation of dye and salt is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a dye / salt separation loose nanofiltration membrane based on an amino nanodiamond-polyphenol-metal network and a preparation method and application thereof, and belongs to the field of textile wastewater membrane separation. Background Art

[0002] The development of the textile industry inevitably brings about wastewater pollution problems. The discharge of a large amount of dye and salt wastewater will cause serious pollution to water bodies, affecting ecological balance and human health. Therefore, the separation of dyes / salts is conducive to resource recycling and is in line with the concept of green and sustainable development. Membrane separation technology is used due to its advantages such as simple operation and low energy consumption. Among them, nanofiltration is often used to separate organic dyes and multivalent ions, but traditional dense nanofiltration membranes are usually prepared by interfacial polymerization, which has a high retention of salt ions and cannot effectively separate dyes / salts. Therefore, the research and development of loose nanofiltration membranes for their application in dye / salt separation has attracted widespread attention.

[0003] Ultrafiltration membranes prepared by adding inorganic nanoparticles do not have an effective separation effect on dyes / salts due to their large pore size; coating and self-assembly deposition on the surface of ultrafiltration base membranes can effectively adjust the pore size of the membrane surface, forming a dense selective layer, and achieving effective dye / salt separation, but with a decrease in water flux. Therefore, using ultrafiltration membranes added with inorganic nanoparticles as a substrate and self-assembly depositing metal-polyphenol networks on the surface can, on the one hand, use hydrophilic nanoparticles to increase the hydrophilicity of the membrane, improve water flux, and enhance mechanical properties; on the other hand, it can also achieve excellent dye / salt separation, improve the trade-off between permeability and selectivity, and significantly increase permeation flux while improving selectivity.

[0004] Among inorganic nanoparticles, nanodiamond combines the properties of diamond and derived nanomaterials, has high chemical stability, hardness and large specific surface area, and the surface can be functionalized with various functional groups, making it more competitive in wastewater treatment. The research on the wastewater treatment application of nanodiamond is scarce and in its infancy, so it is of development significance to study the use of nanodiamond in the treatment of dye wastewater. Summary of the invention

[0005] The purpose of the present invention is to provide a loose nanofiltration membrane for dye / salt separation based on an amino nanodiamond-polyphenol-metal network, and a preparation method and application thereof, and to obtain a loose nanofiltration membrane with high organic dye retention rate, low inorganic salt retention rate and high permeation flux by utilizing the synergistic effect of the amino-polyphenol and polyphenol-metal double-layer networks of nanodiamond.

[0006] The technical solution to achieve the purpose of the present invention is:

[0007] In a first aspect, the present invention provides a method for preparing a dye / salt separation loose nanofiltration membrane based on an amino nanodiamond-polyphenol-metal network, comprising the following steps:

[0008] The first step is the preparation of polyethyleneimine-modified nanodiamonds: adding nanodiamonds into a polyethyleneimine aqueous solution, ultrasonicating for a certain period of time, stirring for a certain period of time, washing the obtained product with water, and drying to obtain polyethyleneimine-modified nanodiamonds;

[0009] The second step is the preparation of nano-diamond / polyimide ultrafiltration base membrane: polyethyleneimine-modified nano-diamond is dispersed in an organic solution, followed by adding diamine and dianhydride monomers to react for a certain period of time, and then adding a catalyst and a dehydrating agent to react by catalysis and dehydration to obtain a polyimide solution, and then degassing to obtain a casting solution, and then applying the obtained casting solution on a glass plate, and obtaining a nano-diamond / polyimide ultrafiltration base membrane by non-solvent-induced phase separation;

[0010] In the third step, the ultrafiltration base membrane obtained in the second step is immersed in a polyphenol solution and a metal salt solution in turn, and the immersion is repeated for a period of time, and then taken out and washed with water to obtain a loose nanofiltration membrane for dye / salt separation based on an amino nanodiamond-polyphenol-metal network.

[0011] Furthermore, in the first step, the nanodiamond uses oxidized nanodiamond with a particle size of 5-200nm, and the mass ratio of nanodiamond to polyethyleneimine is 1:1-1:20; ultrasonic treatment is performed for 10-60min, and stirring is performed at 50-80°C for 10-24h; the drying temperature is 70-100°C, and the drying time is 10-24h.

[0012] Furthermore, in the second step, the organic solution is one of N,N-dimethylacetamide, N,N-dimethylformamide, and N-methylpyrrolidone, preferably N,N-dimethylacetamide; the dianhydride monomer is one of hexafluorodianhydride, biphenyltetracarboxylic acid dianhydride, and benzophenonetetracarboxylic acid dianhydride, preferably hexafluorodianhydride; the diamine monomer is one of 4,4-diaminodiphenyl ether and p-phenylenediamine, preferably 4,4-diaminodiphenyl ether; and the molar ratio of dianhydride to diamine is (0.97-1.05):1.

[0013] Furthermore, in the second step, the total mass of the dianhydride and the diamine accounts for 11-21% of the mass of the polyimide solution; the mass of the polyethyleneimine-modified nanodiamond accounts for 0.1-5%, preferably 0.1-1%, of the total mass of the dianhydride and the diamine.

[0014] Furthermore, in the second step, the dehydrating agent is acetic anhydride, the catalyst is pyridine, the volume ratio of the dehydrating agent to the catalyst is (1-3):1, preferably 2:1; the molar ratio of the catalyst to the diamine is (1.5-2.5):1.

[0015] Furthermore, in the second step, diamine and dianhydride monomers are added to react for 12 hours; catalysis and dehydration reactions are carried out for 12 hours.

[0016] Furthermore, in the second step, the obtained casting solution is scraped onto a glass plate with a coating thickness of 0.1-0.5 mm; non-solvent induced phase separation refers to placing the glass plate coated with the casting solution in air for 1-60 seconds and then immersing it in a deionized water coagulation bath until a film is formed.

[0017] Furthermore, in the third step, the polyphenol is one of tannic acid, catechol, and quercetin, preferably tannic acid, and the concentration of the polyphenol solution is 1-50 mg / L; the metal salt is one of ferrous chloride tetrahydrate, ferric chloride hexahydrate, and nickel chloride, preferably ferric chloride hexahydrate, and the concentration of the metal salt solution is 5-500 mg / L; the molar ratio of the polyphenol to the metal salt is 1:(1-100).

[0018] Furthermore, in the third step, the immersion is repeated 1-3 times, and the immersion time is 1-60 min, preferably 10-30 min.

[0019] In a second aspect, the present invention also provides a dye / salt separation loose nanofiltration membrane based on amino nanodiamond-polyphenol-metal network prepared by the method described in the first aspect.

[0020] In a third aspect, the present invention also provides the use of a dye / salt separation loose nanofiltration membrane based on an amino nanodiamond-polyphenol-metal network prepared by the method described in the first aspect, and the loose nanofiltration membrane is used for separation of dyes and salts.

[0021] Furthermore, the salt includes one or more of sodium chloride, sodium sulfate, magnesium chloride, and magnesium sulfate, preferably sodium chloride; the dye includes one or more of Congo red, methyl blue, methylene blue, indigo carmine, and brilliant blue R, preferably Congo red.

[0022] Compared with the prior art, the advantages of the present invention are as follows: (1) The polyethyleneimine-modified nanodiamond reduces the aggregation of the original nanodiamond, improves the dispersion stability in the solution, and the introduced amino group cross-links with the polyimide to form an amide bond, thereby enhancing the mechanical properties. (2) By utilizing the "intrinsic driving force" caused by the surface energy mismatch, the polyethyleneimine-modified nanodiamond migrates to the base membrane interface, exposing the amino group, providing a binding site for tannic acid, and there is a hydrogen bond or electrostatic interaction. (3) The polyimide base membrane containing nanodiamonds attracts more tannic acid deposition, and the selective layer formed by coordination with metal ions is more dense and hydrophilic, and the water flux is greatly improved. (4) The presence of polyethyleneimine-modified nanodiamonds is unique and can effectively form an amino-modified nanodiamond-polyphenol-metal double-layer network to achieve excellent separation of dyes and salts, with a high retention rate of organic dyes and a low retention rate of inorganic salts, while carbon nanotubes cannot be formed, which has a negative effect on the polyimide nanofiltration membrane and cannot achieve separation of dyes and salts. (5) The prepared loose nanofiltration membrane has good application prospects and expands the research on nanodiamonds in the field of wastewater treatment.

[0023] It should be understood that all combinations of the aforementioned concepts and the additional concepts described in more detail below can be considered as part of the inventive subject matter of the present application as long as such concepts are not mutually contradictory. In addition, all combinations of the claimed subject matter are considered as part of the inventive subject matter of the present application.

[0024] The foregoing and other aspects, embodiments and features of the present invention can be more fully understood from the following description in conjunction with the accompanying drawings. Other additional aspects of the present invention, such as the features and / or beneficial effects of the exemplary embodiments, will be apparent from the following description or learned from the practice of the specific embodiments according to the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a TEM image of the original nanodiamond of the present invention.

[0026] Figure 2 This is a TEM image of polyethyleneimine-modified nanodiamond prepared in Example 1 of the present invention.

[0027] Figure 3 This is a comparison diagram of the dye / salt separation loose nanofiltration membrane based on amino nanodiamond-polyphenol-metal network prepared in Example 6 of the present invention before and after separation of dye / salt solution.

[0028] Figure 4 This is a comparison diagram of the dye / salt separation loose nanofiltration membrane based on amino carbon nanotube-polyphenol-metal network prepared in Comparative Example 3 of the present invention before and after separation of dye / salt solution. DETAILED DESCRIPTION

[0029] The present application is further described below in conjunction with specific embodiments.

[0030] It should be noted that all technical and scientific terms used in this document have the same meaning as those commonly understood by technicians in the technical field of this application; the term "and / or" used in this document includes any and all combinations of one or more related listed items.

[0031] As used herein, the term "at least one of" is intended to be synonymous with "one or more of." For example, "at least one of A, B, and C" expressly includes only A, only B, only C, and combinations of each thereof.

[0032] Concentration, amount and other numerical data can be presented in range format herein.It should be understood that such range format is only used for convenience and simplicity, and should be flexibly interpreted as not only including the numerical value clearly described as range limit, but also including all single numerical values ​​or sub-ranges contained in the range, just as each numerical value and sub-range are clearly described.For example, the numerical range of about 1 to about 4.5 should be interpreted as not only including the limit value of 1 to about 4.5 clearly described, but also including single numerals (such as 2,3,4) and sub-ranges (such as 1 to 3,2 to 4, etc.).The same principle is applicable to the scope of only narrating a numerical value, such as "less than about 4.5", which should be interpreted as including all the above-mentioned values ​​and ranges.In addition, no matter how the breadth of the described range or feature is, this explanation should be applicable.

[0033] If the specific conditions are not specified in the examples, the conventional conditions or the conditions recommended by the manufacturer are used. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. Among them, the nanodiamond particle size used in the examples is 5nm.

[0034] The invention discloses a method for preparing a loose nanofiltration membrane for dye / salt separation based on an amino nanodiamond-polyphenol-metal network. The nanofiltration membrane comprises a polyimide ultrafiltration base membrane doped with polyethyleneimine-modified nanodiamond and a polyphenol-metal selective layer. The nanodiamond is subjected to surface polyethyleneimine grafting to obtain polyethyleneimine-modified nanodiamond. The polyethyleneimine-modified nanodiamond is blended with diamine and dianhydride monomers to prepare a polyimide-based ultrafiltration membrane through chemical imidization. Polyphenol and metal salt are deposited on the surface of the ultrafiltration membrane to construct an amino-polyphenol-metal double-layer network, and a loose nanofiltration membrane for dye / salt separation based on an amino nanodiamond-polyphenol-metal network is prepared. The method specifically comprises the following steps:

[0035] The first step is the preparation of polyethyleneimine modified nanodiamonds: polyethyleneimine is dissolved in deionized water and stirred until the solution is uniform; the nanodiamonds are added to the polyethyleneimine aqueous solution, ultrasonicated for 10-60 minutes, and stirred at 50-80°C for 10-24 hours. The obtained product is washed with water and dried to obtain polyethyleneimine modified nanodiamonds.

[0036] The second step is the preparation of nano-diamond / polyimide ultrafiltration base membrane: polyethyleneimine-modified nano-diamond is dispersed in an organic solution, followed by the addition of diamine and dianhydride monomers for a certain period of time, and then a catalyst and a dehydrating agent are added for catalytic and dehydration reactions to obtain a polyimide solution, which is then degassed to obtain a casting liquid, which is then scraped onto a glass plate with a thickness of 0.1-0.5 mm, allowed to stand in the air for 1-60 seconds, and then immersed in a deionized water coagulation bath, until the membrane is completely detached, and then soaked in deionized water for preservation to obtain a nano-diamond / polyimide ultrafiltration base membrane.

[0037] In the third step, the ultrafiltration base membrane obtained in the second step is soaked in a polyphenol solution and a metal salt solution in turn, and the soaking is repeated for a period of time. The base membrane is taken out and washed with water to obtain a dye / salt separation loose nanofiltration membrane based on an amino nanodiamond-polyphenol-metal network, referred to as a nanodiamond loose nanofiltration membrane.

[0038] In the present invention, a nanodiamond loose nanofiltration membrane is used for the separation of dyes and salts, and the separation effect of the membrane is investigated by interception rate and water flux, wherein:

[0039] The retention rate is calculated by the following formula (1):

[0040]

[0041] R is the retention rate, C p is the concentration of dye or salt in the permeate, C f is the concentration of dye or salt in the stock solution.

[0042] The water flux is calculated by the following formula (2):

[0043]

[0044] Where J is the permeation flux, V is the permeation volume, A is the effective membrane area, and t is the permeation time.

[0045] The dye retention experiment was analyzed using a UV spectrophotometer, and the salt retention experiment was analyzed using a conductivity meter.

[0046] Embodiment 1:

[0047] The preparation of polyethyleneimine modified nanodiamond of the present invention comprises the following steps:

[0048] Take 20 mL of deionized water, dissolve 1 g of polyethyleneimine, and stir for 30 min until the solution is uniform; Figure 1 The obtained product was washed with water and dried at 80°C for 16 hours to obtain polyethyleneimine modified nanodiamonds. The TEM of the obtained product is as follows: Figure 2 shown.

[0049] Embodiment 2:

[0050] The preparation of the nano-diamond / polyimide ultrafiltration base membrane of the present invention comprises the following steps:

[0051] 30 mg of polyethyleneimine-modified nanodiamond (Example 1) was added to 38 g of N,N-dimethylacetamide solution, and ultrasonically dispersed for 30 min. Subsequently, 2.3 g of 4,4-diaminodiphenyl ether and 5.1 g of hexafluorodianhydride were added and reacted for 12 h. 3.7 mL of acetic anhydride and 1.85 mL of pyridine were added and catalyzed and dehydrated for 12 h to obtain a polyimide solution, which was then degassed to obtain a casting solution. The obtained casting solution was scraped onto a glass plate with a thickness of 0.5 mm, allowed to stand in the air for 30 s, and then immersed in deionized water. When the membrane was completely detached, it was soaked in deionized water for storage to obtain a nanodiamond / polyimide ultrafiltration base membrane.

[0052] Embodiment 3:

[0053] The method of this embodiment is the same as that of embodiment 2, except that the mass of the polyethyleneimine-modified nanodiamond added is 60 mg, and a nanodiamond / polyimide ultrafiltration base membrane is prepared.

[0054] Embodiment 4:

[0055] The method of this embodiment is the same as that of embodiment 2, except that the mass of the polyethyleneimine-modified nanodiamond added is 100 mg, and a nanodiamond / polyimide ultrafiltration base membrane is prepared.

[0056] Comparative Example 1:

[0057] 2.3 g of 4,4-diaminodiphenyl ether and 5.1 g of hexafluorodianhydride were added to 38 g of N,N-dimethylacetamide solution, and the reaction was carried out for 12 h. 3.7 mL of acetic anhydride and 1.85 mL of pyridine were added to react for 12 h to obtain a polyimide solution, which was then degassed to obtain a casting solution. The obtained casting solution was scraped onto a glass plate with a thickness of 0.5 mm, allowed to stand in the air for 30 s, and then immersed in deionized water. When the membrane was completely detached, it was soaked in deionized water for storage to obtain a polyimide ultrafiltration base membrane.

[0058] Embodiment 5:

[0059] The preparation of the dye / salt separation loose nanofiltration membrane based on the amino nanodiamond-polyphenol-metal network of the present invention comprises the following steps:

[0060] The nanodiamond / polyimide ultrafiltration base membrane obtained in Example 3 was soaked in 200 mL of 30 mg / L tannic acid and 350 mg / L ferric chloride hexahydrate salt solution in turn, each for 25 min. The membrane was soaked only once, taken out and washed with water to obtain a loose nanofiltration membrane for dye / salt separation based on an amino nanodiamond-polyphenol-metal network, which was stored in deionized water.

[0061] Example 6

[0062] The method of this embodiment is the same as that of embodiment 5, except that the immersion is repeated twice to obtain a loose nanofiltration membrane for dye / salt separation based on an amino-nanodiamond-polyphenol-metal network.

[0063] Example 7

[0064] The method of this embodiment is the same as that of embodiment 5, except that the immersion is repeated three times to obtain a loose nanofiltration membrane for dye / salt separation based on an amino nanodiamond-polyphenol-metal network.

[0065] Comparative Example 2:

[0066] The polyimide ultrafiltration base membrane obtained in Comparative Example 1 was soaked in 200 mL of 30 mg / L tannic acid and 350 mg / L ferric chloride hexahydrate solution, respectively, for 25 min each, and the soaking was repeated twice. The membrane was taken out and washed with water to obtain a loose nanofiltration membrane of a polyphenol-metal network without nanodiamonds, which was stored in deionized water.

[0067] Comparative Example 3:

[0068] Take 20mL of deionized water, dissolve 1g of polyethyleneimine, stir for 30min until the solution is uniform; add 100mg of carbon nanotubes to the polyethyleneimine aqueous solution, ultrasonicate for 15min, and stir at 60℃ for 15h. The obtained product is washed with water and dried at 80℃ for 16h to obtain polyethyleneimine-modified carbon nanotubes. Add 60mg of polyethyleneimine-modified carbon nanotubes to 38g of N,N-dimethylacetamide solution, ultrasonically disperse for 30min, then add 2.3g of 4,4-diaminodiphenyl ether and 5.1g of hexafluorodianhydride, react for 12h, add 3.7mL of acetic anhydride and 1.85mL of pyridine to catalyze and dehydrate for 12h to obtain polyimide solution, then degas to obtain casting solution, and apply the obtained casting solution on a glass plate with a thickness of 0.5mm, stand in the air for 30s, immerse in deionized water, wait for the membrane to completely fall off, and soak in deionized water to obtain a carbon nanotube / polyimide ultrafiltration base membrane. The carbon nanotube / polyimide ultrafiltration base membrane was soaked in 200 mL of 30 mg / L tannic acid and 350 mg / L ferric chloride hexahydrate solution in turn, each for 25 min, and the soaking was repeated twice. The membrane was taken out and washed with water to obtain a loose nanofiltration membrane based on an amino carbon nanotube-polyphenol-metal network, referred to as a carbon nanotube loose nanofiltration membrane, which was stored in deionized water.

[0069] The polyimide ultrafiltration base membranes prepared in Examples 2-4 and Comparative Example 1 were subjected to an organic dye retention test by a cross-flow filtration device, and the test results are shown in Table 1. In the table, R (CR) is the retention rate of Congo red, and PWP is the pure water flux.

[0070] Table 1

[0071] <![CDATA[PWP / Lm -2 h -1 ]]> R(CR) / % Comparative Example 1 228.4 72.9 Example 2 235.9 74.4 Example 3 329.3 79.1 Example 4 315.9 83.3

[0072] The polyimide ultrafiltration base membranes prepared in Examples 2-4 and Comparative Example 1 were subjected to tensile performance tests. The test results are shown in Table 2.

[0073] Table 2

[0074]

[0075]

[0076] Combining the data in Table 1 and Table 2, the polyimide ultrafiltration base membrane prepared in Example 3 has the highest pure water flux and the largest tensile strength, and has the best performance, so the polyimide ultrafiltration base membrane of Example 3 is selected as the base membrane for preparing loose nanofiltration membranes in subsequent examples.

[0077] The nanodiamond loose nanofiltration membranes prepared in Examples 5-7 were tested by a cross-flow filtration device. The test results are shown in Table 3.

[0078] Table 3

[0079] <![CDATA[PWP / Lm -2 h -1 ]]> R(CR) / % Example 5 76.1 88.4 Example 6 42.6 99.5 Example 7 29.1 99.6

[0080] As can be seen from Table 3, although the pure water flux of the nanodiamond loose nanofiltration membrane prepared in Example 5 is large, the Congo red interception rate is low, and the high interception of organic dyes cannot be achieved; the pure water flux of the nanodiamond loose nanofiltration membrane prepared in Example 6 is large, and the Congo red interception rate is high; the Congo red interception rate of the nanodiamond loose nanofiltration membrane prepared in Example 7 is not significantly improved compared with that in Example 6, and the pure water flux is sacrificed. Therefore, the nanodiamond loose nanofiltration membrane of Example 6 is selected as the best sample membrane for separation of dyes and salts.

[0081] The loose nanofiltration membranes prepared in Example 6, Comparative Example 2 and Comparative Example 3 were tested by a cross-flow filtration device, and the test results are shown in Table 4. R(CR) and R(NaCl) in the table are the retention rates of Congo red and sodium chloride, respectively, and PWP is the pure water flux. In addition, the comparison before and after separation of dye / salt solution in Example 6 is as follows: Figure 3 As shown, the comparison of comparative example 3 before and after separation of dye / salt solution is as follows Figure 4 shown.

[0082] Table 4

[0083] <![CDATA[PWP / Lm -2 h -1 ]]> R(CR) / % R(NaCl) / % Example 6 42.6 99.5 2.3 Comparative Example 2 21.9 99.4 2.7 Comparative Example 3 251.0 48.6 0.8

[0084] As can be seen from Table 4, Example 6 and Comparative Example 2 illustrate that the loose nanofiltration membrane with polyethyleneimine modified nanodiamond added has significantly improved the pure water flux compared to when not added, while maintaining high organic dye interception and low inorganic salt interception, and has excellent performance and good separation performance of dyes and salts. In the test, it was found that the nanofiltration membrane prepared in Comparative Example 3 was more fragile than Example 6 and Comparative Example 2, and could not withstand filtration for a long time, which was attributed to the addition of carbon nanotubes that destroyed the arrangement of polyimide molecular chains and increased the defective structure of polymer molecular chains, causing the membrane to be more easily damaged. Although the pure water flux of the loose nanofiltration membrane of carbon nanotubes in Comparative Example 3 was improved, the interception rate of organic dyes was greatly reduced, indicating that the polyethyleneimine modified carbon nanotubes were added into the polyimide ultrafiltration base membrane and played a negative impact, not only destroying the structure of the membrane, but also hindering the deposition of the metal-polyphenol network on the membrane surface, and it was impossible to form a dense, uniform and continuous selective layer, thereby affecting the interception rate, and it was impossible to achieve the separation of dyes and salts. Polyethyleneimine-modified carbon nanotubes had a negative impact on the loose nanofiltration membrane for separation of dyes and salts, while the nanodiamond loose nanofiltration membrane showed excellent performance in dye / salt separation.

[0085] The loose nanofiltration membranes prepared in Example 6 and Comparative Example 2 were subjected to a tensile property test. The test results are shown in Table 5.

[0086] Table 5

[0087]

[0088] As can be seen from Table 5, the mechanical properties of the loose nanofiltration membrane with the addition of polyethyleneimine-modified nanodiamonds are greatly improved compared with those without the addition.

[0089] The above-mentioned implementation cases are only preferred implementation cases in the present invention, but the implementation methods of the present invention are not limited to the above-mentioned implementation cases. For example, various forms of combinations of the schemes in the embodiments, any other changes, modifications, substitutions, and combinations made without departing from the spirit and principles of the present invention should be equivalent replacement methods and are within the protection scope of the present invention.

Claims

1. A method for preparing a dye / salt separation loose nanofiltration membrane based on an amino nanodiamond-polyphenol-metal network, comprising the following steps: The first step is the preparation of polyethyleneimine-modified nanodiamonds: adding nanodiamonds into a polyethyleneimine aqueous solution, ultrasonicating for a certain period of time, stirring for a certain period of time, washing the obtained product with water, and drying to obtain polyethyleneimine-modified nanodiamonds; The second step is the preparation of nano-diamond / polyimide ultrafiltration base membrane: polyethyleneimine-modified nano-diamond is dispersed in an organic solution, followed by adding diamine and dianhydride monomers to react for a certain period of time, and then adding a catalyst and a dehydrating agent to react by catalysis and dehydration to obtain a polyimide solution, and then degassing to obtain a casting solution, and then applying the obtained casting solution on a glass plate, and obtaining a nano-diamond / polyimide ultrafiltration base membrane by non-solvent-induced phase separation; In the third step, the ultrafiltration base membrane obtained in the second step is immersed in a polyphenol solution and a metal salt solution in turn, and the immersion is repeated for a period of time, and then taken out and washed with water to obtain a loose nanofiltration membrane for dye / salt separation based on an amino nanodiamond-polyphenol-metal network.

2. The method according to claim 1, characterized in that In the first step, the nanodiamond uses oxidized nanodiamond with a particle size of 5-200nm, and the mass ratio of nanodiamond to polyethyleneimine is 1:1-1:20; ultrasonic treatment is performed for 10-60min, and stirring is performed at 50-80℃ for 10-24h; the drying temperature is 70-100℃, and the drying time is 10-24h.

3. The method according to claim 1, characterized in that In the second step, the organic solution is one of N,N-dimethylacetamide, N,N-dimethylformamide, and N-methylpyrrolidone, preferably N,N-dimethylacetamide; the dianhydride monomer is one of hexafluorodianhydride, biphenyltetracarboxylic dianhydride, and benzophenonetetracarboxylic dianhydride, preferably hexafluorodianhydride; the diamine monomer is one of 4,4-diaminodiphenyl ether and p-phenylenediamine, preferably 4,4-diaminodiphenyl ether; and the molar ratio of dianhydride to diamine is (0.97-1.05):

1.

4. The method according to claim 1, characterized in that In the second step, the total mass of the dianhydride and the diamine accounts for 11-21% of the mass of the polyimide solution; the mass of the polyethyleneimine-modified nanodiamond accounts for 0.1-5%, preferably 0.1-1% of the total mass of the dianhydride and the diamine.

5. The method according to claim 1, characterized in that In the second step, the dehydrating agent is acetic anhydride, the catalyst is pyridine, the volume ratio of the dehydrating agent to the catalyst is (1-3):1, preferably 2:1; the molar ratio of the catalyst to the diamine is (1.5-2.5):

1.

6. The method according to claim 1, characterized in that In the second step, the obtained casting solution is scraped onto a glass plate with a coating thickness of 0.1-0.5 mm; non-solvent induced phase separation refers to placing the glass plate coated with the casting solution in the air for 1-60 seconds and then immersing it in a deionized water coagulation bath until a film is formed.

7. The method according to claim 1, characterized in that In the third step, the polyphenol is one of tannic acid, catechol, and quercetin, preferably tannic acid, and the concentration of the polyphenol solution is 1-50 mg / L; the metal salt is one of ferrous chloride tetrahydrate, ferric chloride hexahydrate, and nickel chloride, preferably ferric chloride hexahydrate, and the concentration of the metal salt solution is 5-500 mg / L; the molar ratio of the polyphenol to the metal salt is 1:(1-100).

8. The method according to claim 1, characterized in that In the third step, the soaking is repeated 1-3 times, and the soaking time is 1-60 min, preferably 10-30 min.

9. A dye / salt separation loose nanofiltration membrane based on an amino nanodiamond-polyphenol-metal network prepared according to any one of claims 1 to 8.

10. Use of a dye / salt separation loose nanofiltration membrane based on an amino nanodiamond-polyphenol-metal network prepared by the method according to any one of claims 1 to 8, characterized in that: The loose nanofiltration membrane was used for the separation of dyes and salts.

Citation Information

Cited By

  • Preparation method and application of modified polytetrafluoroethylene membrane

    CN119281129A

  • Preparation Method and Application of a Modified Polytetrafluoroethylene Membrane

    CN119281129B

  • Preparation method and application of novel LBL marine biomass hydrogel composite membrane

    CN119701662A

  • Preparation method and application of a novel LBL marine biomass hydrogel composite membrane

    CN119701662B