A boron nitride / silica aerogel and its preparation method
By preparing boron nitride/silica aerogel, the problem of the hydrophilicity of silica aerogel limiting its application in the field of lightweight thermal insulation was solved, realizing the preparation of low-cost, high-performance hydrophobic thermal insulation materials suitable for thermal insulation coatings.
Patent Information
- Application Number
- CN202311470670.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-07
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-07
AI Technical Summary
The hydrophilicity of existing silica aerogels limits their application in lightweight thermal insulation, especially in thermal insulation coatings.
High-purity BN nanosheets were prepared using ammonia borane as the dopant phase. Water glass was used as the silicon source, and boron nitride/silica aerogels were prepared through a two-step solvent method and atmospheric pressure drying process. Combined with a hydrophobic modifier, a three-dimensional porous network structure was formed.
A low-cost, high-performance boron nitride/silica aerogel was prepared, exhibiting excellent hydrophobicity and thermal insulation properties, making it suitable for industrial production and wide application.
Smart Images

Figure CN117582898B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lightweight thermal insulation materials and relates to a boron nitride / silica aerogel and its preparation method. Background Technology
[0002] Aerogels possess superior properties due to their unique structure, giving them unparalleled advantages in the field of thermal insulation. Currently, the main preparation methods for silica aerogels include those using organosilicon sources (such as methyl orthosilicate, tetraethyl orthosilicate, and alkoxysilanes) and inorganic silicon sources (such as water glass and fly ash), employing different preparation methods such as supercritical drying and atmospheric pressure drying processes.
[0003] However, currently, high-performance silica aerogels are mostly prepared using costly and environmentally unfriendly organosilicon sources and expensive, complex supercritical drying processes, which hinders process optimization and cost control for large-scale industrial production. Improving the preparation process using inorganic silicon sources combined with atmospheric pressure drying remains a key focus and research area for scaling up aerogel production and reducing production costs. Furthermore, although silica aerogels undergo hydrophobic modification during preparation, the inherent hydrophilicity of the prepared aerogels significantly limits their application in lightweight thermal insulation fields (especially in thermal insulation coatings). Therefore, the hydrophobic properties of the prepared materials can be improved by incorporating lightweight, hydrophobic components while maintaining their original excellent properties. Summary of the Invention
[0004] In view of this, in order to solve the problem that the hydrophilicity of silica aerogel itself limits its application in the field of lightweight thermal insulation, the present invention provides a boron nitride / silica aerogel and its preparation method. High-purity BN nanosheets prepared by ammonia borane are used as the doping phase, water glass is used as the silicon source, and a high-performance boron nitride / silica aerogel is prepared by a two-step solvent method and atmospheric pressure drying. This method can achieve high-performance boron nitride / silica aerogel with low cost and high efficiency.
[0005] To achieve the above objectives, the present invention provides the following technical solution:
[0006] A method for preparing boron nitride / silica aerogel includes the following steps:
[0007] Synthesis of S1 and BN nanosheet powders
[0008] Sodium borohydride reacts with ammonium sulfate in an organic solvent to produce ammonia borane. The prepared ammonia borane is then decomposed at high temperature into BN nanosheet powder with a length of 100±5 nm and a thickness of 20±2 nm.
[0009] S2. Prepare water glass diluent.
[0010] While stirring the water glass solution, slowly add deionized water to prepare a water glass dilution solution of the required concentration;
[0011] S3. Preparation of active silicic acid solution
[0012] The water glass diluent prepared in step S2 is exchanged with an acidic cation exchange resin to prepare an active silicic acid solution;
[0013] S4. Preparation of hydrogel
[0014] While thoroughly stirring the active silica solution prepared in step S3, slowly and repeatedly add small amounts of BN nanosheet powder synthesized in step S1, and simultaneously add an alkaline solution to catalyze the formation of boron nitride / silica hydrogel.
[0015] S5. Preparation of alcohol gel
[0016] The boron nitride / silica hydrogel prepared in step S4 was added to ethanol and aged and solvent-displaced at 20-50°C to obtain boron nitride / silica alcohol gel.
[0017] S6. Preparation of wet gel
[0018] The boron nitride / silica alcohol gel prepared in step S5 was modified by adding a surface modifier to obtain a boron nitride / silica wet gel.
[0019] S7. Preparation of aerogel
[0020] Hexane was added to the boron nitride / silica wet gel prepared in step S6 for a second solvent replacement. The gel was then dried at room temperature (30–150 °C) to obtain boron nitride / silica aerogel.
[0021] Furthermore, in step S1, the molar ratio of sodium borohydride to ammonium sulfate is 1:2 to 2:1, the added organic solvent is one of ethanol, tetrahydrofuran or n-hexane, the reaction temperature is 30 to 50°C, the reaction time is 3 to 5 hours, and the temperature for preparing BN nanosheet powder by cracking the generated ammonia borane is 1000 to 1300°C.
[0022] Furthermore, in step S2, the mass ratio of water glass diluted with water glass to deionized water is 1:4 to 1:10.
[0023] Furthermore, in step S3, the flow rate of the acidic cation exchange resin for preparing the active silica solution is 15–30 m / h.
[0024] Furthermore, in step S4, the mass ratio of BN nanosheet powder to water glass is 1:19 to 1:4; and the concentration of ammonia water added as an alkaline catalyst is 0.01 to 2 mol / L.
[0025] Furthermore, in step S6, the surface modifier is trimethylchlorosilane / n-hexane, with a mass ratio of 1:2 to 2:1.
[0026] Furthermore, in step S7, the time for adding n-hexane for the second solvent replacement is 10-14 hours; after drying at normal pressure for 2 hours, boron nitride / silica aerogel is obtained.
[0027] The present invention also provides a boron nitride / silica aerogel prepared by the above-described method for preparing boron nitride / silica aerogel.
[0028] Furthermore, the boron nitride / silica aerogel is a three-dimensional porous network structure formed by uniformly dispersing boron nitride nanosheets in an amorphous silica matrix.
[0029] Furthermore, boron nitride / silica aerogels are hydrophobic, with a porosity of 5–95%, a density of 10–90 mg / mL, and a thermal conductivity of 30–45 mW / m·K.
[0030] The beneficial effects of this invention are as follows:
[0031] 1. The boron nitride / silica aerogel disclosed in this invention is prepared by reacting sodium borohydride and ammonium sulfate in an organic solvent to generate ammonia borane, and then preparing BN nanosheet powder through high-temperature pyrolysis. A water glass diluent of the required concentration is prepared, and an active silicic acid solution is prepared by exchanging the solution with an acidic cation exchange resin. The prepared BN nanosheet powder is uniformly dispersed in the active silicic acid solution, and then a boron nitride / silica hydrogel is obtained by catalysis with the addition of an alkaline solution. The boron nitride / silica hydrogel is then aged and solvent-displaced in ethanol at a certain temperature, modified with a modifier, and then solvent-displaced again with n-hexane. Finally, it is dried at a certain temperature and atmospheric pressure to obtain a boron nitride / silica aerogel with uniform structure and excellent performance. This preparation method uses water glass as the silicon source, employs a two-step solvent displacement and hydrophobic modification process, and prepares boron nitride / silica aerogel by atmospheric pressure drying. This method has the advantages of wide availability of raw materials, low cost, suitability for industrial production, and excellent performance.
[0032] 2. The boron nitride / silica aerogel disclosed in this invention uses boron nitride nanosheet powder prepared by high-temperature pyrolysis of self-made ammonia borane as a dopant to further regulate the hydrophobic properties of the prepared boron nitride / silica aerogel. The boron nitride / silica aerogel with excellent comprehensive properties such as structural strength is prepared by two-step solvent replacement and atmospheric pressure drying, which has broad prospects for industrialization and market application.
[0033] Other advantages, objectives, and features of the invention will be set forth in part in the description which follows, and in part will be apparent to those skilled in the art from the following examination, or may be learned from practice of the invention. The objectives and other advantages of the invention can be realized and obtained through the following description. Attached Figure Description
[0034] To make the objectives, technical solutions, and advantages of the present invention clearer, the preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings, wherein:
[0035] Figure 1 This is a flow chart of the boron nitride / silica aerogel preparation process of the present invention;
[0036] Figure 2 These are TEM and high-resolution images of BN nanosheet powder prepared by the pyrolysis of ammonia borane according to the present invention. Figure 2 (a) is a transmission electron microscope image of BN nanosheet powder at a resolution of 20 nm. Figure 2 (b) is a transmission electron microscope image of BN nanosheet powder at a resolution of 5 nm;
[0037] Figure 3 This is a photograph of the boron nitride / silica aerogel prepared in this invention. Figure 3 (a) is a microscopic photograph of the boron nitride / silica aerogel prepared in this invention. Figure 3 (b) is a macroscopic photograph of the prepared boron nitride / silica aerogel. Detailed Implementation
[0038] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0039] Example
[0040] like Figure 1 The method for preparing a boron nitride / silica aerogel includes the following steps:
[0041] Synthesis of S1 and BN nanosheet powders
[0042] Sodium borohydride (9.5 g, 0.25 mol) and ammonium sulfate (33 g, 0.25 mol) in a molar ratio of 1:1 were dissolved in 250 ml of tetrahydrofuran and reacted at 40 °C for 4 hours to obtain ammonia borane (BH3NH3). After filtration, 7.1 g of ammonia borane powder (yield 91%) was obtained. The ammonia borane powder was then pyrolyzed at 1200 °C to obtain 5.6 g of high-purity BN nanosheet powder (yield 75%). The obtained BN nanosheet powder had a length of 100 ± 5 nm and a thickness of 20 ± 2 nm.
[0043] S2. Prepare water glass diluent.
[0044] While stirring 100g of water glass solution, slowly add 400g of deionized water. The mass ratio of water glass to deionized water in the water glass dilution is 1:4, thus preparing a water glass dilution solution of the required concentration.
[0045] S3. Preparation of active silicic acid solution
[0046] The water glass diluent prepared in step S2 is exchanged with an acidic cation exchange resin to prepare an active silicic acid solution; the flow rate for preparing the active silicic acid solution by exchanging with the acidic cation exchange resin is 20 m / h, and the time for passing through the exchange column is 3 hours.
[0047] S4. Preparation of hydrogel
[0048] While thoroughly stirring the active silica solution prepared in step S3, slowly and repeatedly add 5.6g of BN nanosheet powder synthesized in step S1 in small amounts. The mass ratio of the added BN nanosheet powder to water glass is 1:10. At the same time, add 10ml of ammonia water with a concentration of 1mol / L as an alkaline catalyst to catalyze and obtain boron nitride / silica hydrogel.
[0049] S5. Preparation of alcohol gel
[0050] The boron nitride / silica hydrogel prepared in step S4 was immersed in ethanol at 35°C for 24 h and then in n-hexane for 12 h for solvent replacement to obtain boron nitride / silica alcohol gel.
[0051] S6. Preparation of wet gel
[0052] The boron nitride / silica alcohol gel prepared in step S5 was immersed in a trimethylchlorosilane / n-hexane modifier with a mass ratio of 1:1 for 24 hours to obtain boron nitride / silica wet gel.
[0053] S7. Preparation of aerogel
[0054] The boron nitride / silica wet gel prepared in step S6 was immersed in hexane at 35°C for a second solvent replacement for 12 hours. After multiple batches of drying at atmospheric pressure at 100°C for 2 hours, a total of 35g of boron nitride / silica aerogel was obtained.
[0055] Figure 2 (a) is a transmission electron microscope image of BN nanosheet powder at a resolution of 20 nm. Figure 2 (b) is a transmission electron microscope image of BN nanosheet powder at a resolution of 5 nm; it can be seen that BN nanosheets have good crystalline morphology.
[0056] Figure 3 (a) is a microscopic photograph of the boron nitride / silica aerogel prepared in this invention. It can be seen that the boron nitride nanosheets are uniformly dispersed in the amorphous silica matrix to form a three-dimensional porous network structure, which gives the boron nitride / silica aerogel a micro-nano structure and thus gives it good hydrophobicity. Figure 3 (b) is a macroscopic photograph of the prepared boron nitride / silica aerogel, which shows that it has good bulk integrity.
[0057] The boron nitride / silica aerogel prepared in this embodiment mainly consists of silicon, boron, nitrogen, and oxygen. Its internal microstructure comprises boron nitride nanosheets uniformly distributed as a dispersed phase within an amorphous silica matrix, forming a three-dimensional network structure. This boron nitride / silica aerogel possesses a three-dimensional lamellar porous network composed of boron nitride nanosheets and amorphous silica, with the boron nitride nanosheets uniformly distributed within the amorphous silica matrix. By using low-cost water glass as the silicon source and boron nitride nanosheets with a specific aspect ratio as reinforcement, the boron nitride / silica aerogel exhibits excellent chemical stability, good hydrophobicity, and low manufacturing cost.
[0058] The boron nitride / silica aerogel prepared in this embodiment has certain hydrophobicity, a porosity of 5-95%, a density of 10-90 mg / mL, and a thermal conductivity of 30-45 mW / m·k.
[0059] In summary, the high-performance boron nitride / silica aerogel prepared by this invention not only has good thermal stability and heat insulation performance, but also allows for adjustment of the hydrophobic properties of the prepared aerogel material by adjusting the BN content, making it more advantageous for the application of silica aerogel powder material in heat insulation coatings.
[0060] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A method for preparing boron nitride / silica aerogel, characterized in that, Includes the following steps: Synthesis of S1 and BN nanosheet powders Sodium borohydride reacts with ammonium sulfate in an organic solvent to produce ammonia borane. The prepared ammonia borane is then decomposed at high temperature into BN nanosheet powder with a length of 100±5 nm and a thickness of 20±2 nm. The molar ratio of sodium borohydride to ammonium sulfate is 1:2 to 2:
1. The added organic solvent is one of ethanol, tetrahydrofuran, or n-hexane. The reaction temperature is 30 to 50 °C, the reaction time is 3 to 5 hours, and the temperature for preparing BN nanosheet powder by decomposition of the generated ammonia borane is 1000 to 1300 °C. S2. Prepare water glass diluent. While stirring the water glass solution, slowly add deionized water to prepare a water glass diluent of the required concentration; the mass ratio of water glass to deionized water in the water glass dilution is 1:4 to 1:
10. S3. Preparation of active silicic acid solution The water glass diluent prepared in step S2 is exchanged with an acidic cation exchange resin to prepare an active silicic acid solution; The flow rate for preparing active silicic acid solution by acidic cation exchange resin is 15~30 m / h; S4. Preparation of hydrogel While thoroughly stirring the active silicic acid solution prepared in step S3, slowly and repeatedly add small amounts of BN nanosheet powder synthesized in step S1, and simultaneously add an alkaline solution to catalyze the formation of boron nitride / silica hydrogel; the mass ratio of the added BN nanosheet powder to water glass is 1:19~1:4; the concentration of the added ammonia water as an alkaline catalyst is 0.01~2 mol / L; S5. Preparation of alcohol gel The boron nitride / silica hydrogel prepared in step S4 was added to ethanol and aged and solvent-displaced at 20~50℃ to obtain boron nitride / silica alcohol gel. S6. Preparation of wet gel The boron nitride / silica alcohol gel prepared in step S5 was modified by adding a surface modifier to obtain a boron nitride / silica wet gel. S7. Preparation of aerogel Hexane was added to the boron nitride / silica wet gel prepared in step S6 for a second solvent replacement, and the gel was dried at room pressure at a temperature of 30~150℃ to obtain boron nitride / silica aerogel.
2. The method for preparing boron nitride / silica aerogel as described in claim 1, characterized in that, In step S6, the surface modifier is trimethylchlorosilane / n-hexane, with a mass ratio of 1:2 to 2:
1.
3. The method for preparing boron nitride / silica aerogel as described in claim 1, characterized in that, In step S7, the time for adding n-hexane for the second solvent replacement is 10-14 hours; after drying at normal pressure for 2 hours, boron nitride / silica aerogel is obtained.
4. The boron nitride / silica aerogel prepared by the method for preparing boron nitride / silica aerogel according to any one of claims 1 to 3.
5. The boron nitride / silica aerogel as described in claim 4, characterized in that, Boron nitride / silica aerogel is a three-dimensional porous network structure formed by uniformly dispersing boron nitride nanosheets in an amorphous silica matrix.
6. The boron nitride / silica aerogel as described in claim 5, characterized in that, Boron nitride / silica aerogels are hydrophobic, with a porosity of 5–95%, a density of 10–90 mg / mL, and a thermal conductivity of 30–45 mW / m·K.
Citation Information
Patent Citations
Silicon dioxide aerogel material and preparation method thereof
CN104030301A
Sulfur and nitrogen codoped graphene-based aerogel and preparation method thereof
CN108439372A