Modified asphalt coating material, preparation method thereof and asphalt waterproofing roll material

By using calcium-iron-aluminum-based layered hydroxide for modification in asphalt waterproofing membranes, the problem of insufficient UV resistance and salt-alkali resistance of asphalt waterproofing membranes in marine environments is solved, achieving better waterproof performance and use life.

CN117586699BActive Publication Date: 2024-10-18NANTONG KESHUN NEW BUILDING MATERIALS CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311485191.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-08
Publication Date
2024-10-18
Estimated Expiration
2043-11-08

AI Technical Summary

Technical Problem

Existing asphalt waterproofing membranes have insufficient UV resistance and salt-alkali resistance in marine environments, making it difficult to meet the long-term use requirements under complex marine conditions.

Method used

Calcium-iron-aluminum-based layered hydroxide is used to modify the modified asphalt coating material. The multi-layer shielding and absorption effect of calcium-iron-aluminum-based layered hydroxide improves the UV resistance, and through its protection against chloride ions and sulfate radicals The adsorption capacity of ions enhances the salt-alkali resistance.

Benefits of technology

It significantly improves the UV resistance and salt-alkali resistance of the asphalt waterproofing membrane, extends its service life, prevents salt spray erosion, and meets the needs of waterproofing materials under marine working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The technical solution of the present application discloses a modified asphalt coating material, a preparation method thereof and an asphalt waterproofing coiled material, wherein the asphalt waterproofing coiled material comprises the following components by weight: 40 parts of base asphalt; 3.5-10 parts of asphalt modifier; 2-5 parts of polyisoprene; 5-10 parts of rubber powder; 1-5 parts of naphthenic oil; 10-20 parts of calcium iron aluminum layered hydroxide; 0.1-0.3 parts of vulcanizing agent; and 20-40 parts of filler. The asphalt coating material can utilize the unique hierarchical structure of the material itself to realize shielding, reflection and absorption of ultraviolet rays, thereby improving the anti-ultraviolet ability of the waterproofing coiled material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of building waterproof materials, and in particular to a modified asphalt coating material and a preparation method thereof, and an asphalt waterproofing membrane. Background Art

[0002] Marine engineering construction refers to construction projects carried out at sea, on the seabed or on the coast for marine production, transportation, protection and other purposes, and construction materials are the basis of marine engineering construction and marine development. Due to the complex marine environment, related construction materials are extremely susceptible to environmental influences such as salt spray, high temperature, high humidity, tides, freeze-thaw, etc., which in turn cause the deterioration of the material structure and performance.

[0003] As far as building waterproof materials are concerned, the research on material performance under marine conditions not only needs to meet the requirements of conventional waterproof materials, but also needs to have good sea resistance to meet the needs of long-term use in complex marine environments. Asphalt waterproofing membrane is a low-cost waterproof material. After modification, it has the characteristics of high tensile strength, high elongation, and good high and low temperature resistance, and occupies a dominant position in waterproof materials. However, the asphalt substrate itself has poor UV resistance and is not resistant to salt and alkali, which greatly limits its application in marine construction projects. Summary of the invention

[0004] In response to the problems existing in the prior art, the embodiments of the present application provide a modified asphalt coating, a preparation method thereof and an asphalt waterproofing membrane, aiming to provide an asphalt waterproofing membrane with good UV resistance and salt-alkali resistance, which can adapt to the complex marine environment and meet the requirements for waterproof material performance under marine working conditions.

[0005] In a first aspect, an embodiment of the present application provides a modified asphalt coating material, comprising the following components by weight:

[0006] 40 parts of base asphalt;

[0007] 3.5-10 parts of asphalt modifier;

[0008] 2-5 parts of polyisoprene;

[0009] 5-10 parts of rubber powder;

[0010] 1-5 parts of naphthenic oil;

[0011] 10-20 parts of calcium iron aluminum layered hydroxide;

[0012] Vulcanizing agent 0.1-0.3 parts;

[0013] 20 to 40 parts of filler.

[0014] In the embodiment of the present application, calcium iron aluminum-based layered hydroxide is used to modify the asphalt coating material. The plate layer of calcium iron aluminum-based layered hydroxide is composed of positively charged metal cations, which has multi-layer shielding and reflection effects on ultraviolet rays. The interlayer anions make the layered hydroxide as a whole electrically neutral, and have a certain absorption effect on ultraviolet rays. Therefore, through the modification of calcium iron aluminum-based layered hydroxide and asphalt coating material, the unique hierarchical structure of the material itself can be used to achieve shielding, reflection and absorption of ultraviolet rays, thereby improving the anti-ultraviolet ability of the waterproof membrane. In addition, calcium iron aluminum-based layered hydroxide has dihydroxyl, is an anionic layered compound with exchangeable interlayer anions, has a strong adsorption capacity for chloride ions, and can also adsorb a certain amount of sulfate ions, so it can absorb harmful ions such as chloride ions and sulfate ions that penetrate into seawater, thereby preventing further erosion of the concrete structure by salt spray, and improving the salt and alkali resistance of the waterproof membrane.

[0015] In some embodiments of the present application, the calcium-iron-aluminum-based layered hydroxide is prepared by a co-precipitation reaction of a metal salt solution containing calcium ions, iron ions, and aluminum ions and an alkaline solution.

[0016] In some embodiments of the present application, the molar ratio of calcium ions, iron ions, and aluminum ions in the metal salt solution is 10:(0.5-2):(3-5).

[0017] In some embodiments of the present application, the interlayer anions of the calcium iron aluminum layered hydroxide include nitrate ions.

[0018] In some embodiments of the present application, the modified asphalt coating further includes 5 to 10 parts of biochar and 0.5 to 2 parts of dispersant.

[0019] In some embodiments of the present application, the base asphalt includes one or more combinations of petroleum asphalt, natural asphalt, and coal tar asphalt.

[0020] In some embodiments of the present application, the asphalt modifier includes one or more combinations of styrene-butadiene-styrene block copolymer, styrene-isoprene-styrene block copolymer, and styrene-butadiene rubber.

[0021] In some embodiments of the present application, the rubber powder includes tire rubber powder and / or miscellaneous rubber powder.

[0022] In some embodiments of the present application, the filler includes one or more combinations of calcium carbonate, heavy calcium carbonate, and organic montmorillonite.

[0023] In a second aspect, an embodiment of the present application provides a method for preparing a modified asphalt coating, the method comprising:

[0024] The step of preparing molten asphalt comprises mixing base asphalt, cyclohexane oil and polyisoprene, and heating the mixture to react to obtain molten asphalt;

[0025] The step of preparing modified asphalt comprises mixing the molten asphalt, asphalt modifier, rubber powder, vulcanizing agent, calcium iron aluminum layered hydroxide, and heating the mixture to react to obtain modified asphalt;

[0026] The step of preparing the modified asphalt coating material comprises mixing the modified asphalt and filler, and heating the mixture for reaction to obtain the modified asphalt coating material.

[0027] In some embodiments of the present application, the step of preparing molten asphalt includes mixing base asphalt, cyclohexane oil, and polyisoprene, and heating the mixture to 130-140° C. to obtain molten asphalt;

[0028] The step of preparing modified asphalt comprises heating the molten asphalt to 150-160° C., adding an asphalt modifier, adding rubber powder and a vulcanizing agent after the asphalt modifier is completely dissolved, and then sequentially adding biochar, calcium iron aluminum layered hydroxide, and a dispersant after the asphalt modifier is dissolved, and reacting for 1-2 hours at a temperature keeping the temperature high to obtain the modified asphalt;

[0029] The step of preparing the modified asphalt coating material comprises heating the modified asphalt to 170-180° C., adding fillers, and keeping the temperature for reaction for 2-3 hours to obtain the modified asphalt coating material.

[0030] In a third aspect, an embodiment of the present application provides an asphalt waterproofing membrane, comprising:

[0031] Tire base;

[0032] A coating layer is provided on both side surfaces of the tread base layer, wherein the coating layer comprises the modified asphalt coating according to the embodiment of the first aspect of the present application or the modified asphalt coating obtained according to the preparation method of the second aspect of the present application;

[0033] An upper isolation layer is provided on the surface of the coating material layer on one side;

[0034] The lower isolation layer is arranged on the surface of the coating material layer on the other side.

[0035] In some embodiments of the present application, the upper isolation layer includes a PET polyester isolation film layer or a fine sand layer.

[0036] In some embodiments of the present application, the thickness of the upper isolation layer is 35-50 μm.

[0037] In some embodiments of the present application, the lower isolation layer includes a polyethylene isolation film layer.

[0038] In some embodiments of the present application, the thickness of the lower isolation layer is 0.2 to 0.5 mm. DETAILED DESCRIPTION

[0039] The features and exemplary embodiments of various aspects of the present application will be described in detail below. In the detailed description below, many specific details are proposed to provide a comprehensive understanding of the present application. However, it is obvious to those skilled in the art that the present application can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present application by illustrating the examples of the present application. In the following description, at least part of the known structures and technologies are not shown to avoid unnecessary ambiguity in the present application; and, for clarity, the size of some structures may be exaggerated. In addition, the features, structures or characteristics described below may be combined in one or more embodiments in any suitable manner.

[0040] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish an entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In the description of the present application, it should be noted that, unless otherwise specified, the meaning of "multiple" is more than two. Moreover, the term "include", "comprise" or any other variant thereof is intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements not only include those elements, but also include other elements not clearly listed, or also include elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements limited by the sentence "include..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements.

[0041] As described in the background technology, at present, the development of waterproofing rolls adapted to marine working conditions is insufficient, specifically, the development of the durability of the rolls under strong ultraviolet and high salinity conditions is insufficient, and it is difficult to meet the requirements of marine working conditions. In the waterproof material market, modified asphalt waterproofing rolls occupy a dominant position, but asphalt itself, which is the base material of the modified asphalt rolls, has poor anti-ultraviolet ability, so most of the modified asphalt rolls are constructed in a non-exposed manner, so that their waterproofing effect can be extended under the protection of concrete. In the prior art, various types of antioxidants, anti-ultraviolet agents and other additives are added to the asphalt rubber to improve its anti-ultraviolet ability, but on the one hand, the related additives are expensive, and on the other hand, many additives have poor compatibility with the asphalt system, and are prone to segregation during long-term storage and use, which seriously affects the performance of the asphalt waterproofing roll.

[0042] Currently, there are some modified asphalt waterproof membranes on the market that can be exposed for construction. They use a weather-resistant film on the upper layer of the rubber to achieve weather resistance by reflecting sunlight. However, this solution also has practical application problems. First, the weather-resistant film is more expensive than ordinary polyester / polyethylene isolation film. Secondly, the asphalt rubber and the film are very easy to peel off under long-term exposure. After being blown by the wind, the film and the membrane are completely peeled off and cannot play a weather-resistant role. In addition, the weather-resistant film is mainly white, which will cause serious white pollution on the construction site.

[0043] In terms of salt and alkali resistance, there are currently few reliable technical solutions. Under marine conditions, the environment contains a large number of harmful ions, such as: Cl - 、SO4 2- Mg 2+ Some of these ions will even penetrate the waterproof layer into the concrete, corrode the steel bars under the electrochemical action, and endanger the safety of the building structure.

[0044] Based on this, the inventors have conducted a lot of research, aiming to provide an asphalt waterproofing membrane with good UV resistance, while enhancing the salt and alkali resistance of the modified asphalt waterproofing membrane, which can effectively prevent the erosion of salt spray.

[0045] In order to solve the problems of the prior art, the embodiments of the present application provide a modified asphalt coating material, a preparation method thereof and an asphalt waterproofing membrane.

[0046] Modified asphalt coating

[0047] An embodiment of the first aspect of the present application provides a modified asphalt coating, comprising the following raw materials in parts by weight: base asphalt, 40 parts; asphalt modifier, 3.5-10 parts; polyisoprene, 2-5 parts; rubber powder, 5-10 parts; cycloparaffin oil, 1-5 parts; calcium iron aluminum layered hydroxide, 10-20 parts; vulcanizing agent, 0.1-0.3 parts; filler, 20-40 parts.

[0048] As can be understood by those skilled in the art, layered hydroxide refers to a special type of layered material, which is composed of several positively charged layers and anions present between the layers for balancing the charge. The anions in the middle have weak interactions with the layers and are usually exchangeable.

[0049] According to the embodiments of the present application, the plate layer of the calcium iron aluminum layered hydroxide is composed of positively charged calcium ions, aluminum ions and iron ions, which have multi-layer shielding and reflection effects on ultraviolet rays, and the interlayer anions of the calcium iron aluminum layered hydroxide have a certain absorption effect on ultraviolet rays. Therefore, the calcium iron aluminum layered hydroxide can use its unique hierarchical structure to achieve shielding, reflection and absorption of ultraviolet rays. After applying it to the modified asphalt coating material, it can effectively improve the anti-ultraviolet ability of the asphalt waterproofing membrane. In addition, the calcium iron aluminum layered hydroxide has a dihydroxy structure and is an anionic compound with exchangeable interlayer anions. It can absorb harmful ions such as chloride ions that penetrate into seawater, protect the waterproof layer from erosion and damage by salt and alkali, and then prevent salt fog from further eroding the concrete structure, and improve the salt and alkali resistance of the asphalt waterproofing membrane.

[0050] According to the embodiments of the present application, polyisoprene can cross-link with asphalt molecules to form a three-dimensional network structure. This cross-linked structure can increase the elasticity and flexibility of asphalt and improve the strength and durability of asphalt substrates. The polyisoprene molecular chain has a strong polarity. When polyisoprene interacts with the molecules in asphalt, an attraction will be generated between the polar groups, thereby increasing the adhesion of asphalt, allowing asphalt to better adhere to the surface of other materials and reduce peeling and shedding. In addition, polyisoprene has good antioxidant properties. After adding polyisoprene to asphalt, its molecular chain can react with oxygen molecules to inhibit the oxidation reaction, which can effectively delay the aging process of asphalt and reduce the quality decline and performance degradation caused by oxidation. In some embodiments, the average molecular weight of polyisoprene is 40,000 to 80,000.

[0051] According to the embodiments of the present application, naphthenic oil can be dissolved in asphalt and form a mixture therewith, thereby enhancing the softness and plasticity of asphalt, and the chain structure of the naphthenic oil molecules can fill the gaps between asphalt molecules, increase the distance between its molecules, and make the asphalt softer. In addition, naphthenic oil has a lower viscosity, and by adding an appropriate amount of naphthenic oil to asphalt, the fluidity of asphalt can be improved, making it easier to process and operate. In some embodiments, the saturated hydrocarbon content of the naphthenic oil can be 83% to 87%.

[0052] According to the embodiment of the present application, the vulcanizing agent can undergo a cross-linking reaction with the asphalt molecules to form a cross-linked structure of sulfide, which can enhance the elasticity and flexibility of the asphalt, thereby improving the strength and durability of the asphalt material and its resistance to thermal oxidation aging. In addition, the addition of the vulcanizing agent can change the temperature characteristics of the asphalt, making the asphalt material less likely to soften and flow at high temperatures, while maintaining good elasticity and flexibility at low temperatures, thereby improving the high and low temperature resistance of the asphalt material.

[0053] In some embodiments, the vulcanizing agent may be selected from benzoyl peroxide, dicumyl peroxide, 2,4-dichlorobenzoyl peroxide, or a combination thereof.

[0054] In some embodiments, the calcium iron aluminum layered hydroxide is prepared by a co-precipitation reaction of a metal salt solution containing calcium ions, iron ions, and aluminum ions and an alkaline solution.

[0055] In some embodiments, the molar ratio of calcium ions, iron ions, and aluminum ions in the metal salt solution is 10:(0.5-2):(3-5).

[0056] According to the embodiments of the present application, the contents of calcium ions, iron ions and aluminum ions in the metal salt solution are controlled within the above range, so that the calcium-iron-aluminum-based layered hydroxide has a higher purity and has better shielding and reflection effects on ultraviolet rays.

[0057] In some embodiments, the interlayer anions of the calcium iron aluminum based layered hydroxide include nitrate ions.

[0058] According to the embodiment of the present application, the plate layer of the calcium iron aluminum layered hydroxide is composed of positively charged calcium ions, iron ions and aluminum ions, and the interlayer anions are nitrate ions. According to the SO4 2- >NO3 - >Cl - >OH - , calcium iron aluminum layered hydroxide to Cl - It has strong adsorption capacity and can also adsorb a certain amount of SO4 2- >, so it can achieve effective anti-salt and alkali effect and improve the salt and alkali resistance of waterproof membrane.

[0059] In some embodiments, the metal salt solution includes an aqueous solution of nitrate corresponding to calcium ions, iron ions, and aluminum ions, and the alkaline solution includes an aqueous solution of sodium hydroxide and sodium nitrate. The metal salt solution provides cations of the calcium iron aluminum layered hydroxide, and the nitrate solution can provide nitrate ions, thereby obtaining a calcium iron aluminum layered hydroxide with a stable structure.

[0060] In some embodiments, the coprecipitation reaction for preparing calcium iron aluminum layered hydroxide specifically includes: dissolving Ca(NO3)2·4H2O, Fe(NO3)3·9H2O and Al(NO3)3·9H2O in deionized water according to a ratio to prepare solution A; dissolving NaOH and NaNO3 in deionized water to prepare solution B. The A and B solutions are dripped into a three-necked flask containing alcohol and NaOH drop by drop, and magnetically stirred for 2 to 3 hours, and then placed in an autoclave for crystallization for 18 to 20 hours. After the reaction, the solution is centrifuged and washed to neutrality for multiple times, and the obtained solid material is placed in a vacuum drying oven at 80 to 90°C for 12 to 15 hours, and then ground into powder after drying to obtain calcium iron aluminum layered hydroxide.

[0061] In some embodiments, the modified asphalt coating further includes 5 to 10 parts of biochar and 0.5 to 2 parts of dispersant.

[0062] Not limited to any theory and explanation, the calcium iron aluminum layered hydroxide structure has two hydroxyls, and its hydrophilicity is strong, and its compatibility with hydrophobic asphalt is poor. And biochar is a highly aromatic organic matter, it has good compatibility with asphalt, and its internal loose porous structure can be well used as a carrier of calcium iron aluminum layered hydroxide, so that calcium iron aluminum layered hydroxide is filled in the internal pores of biochar, thereby improving the compatibility between calcium iron aluminum layered hydroxide and asphalt. And the addition of dispersant can further improve the dispersion effect between calcium iron aluminum layered hydroxide and biochar, and better promote calcium iron aluminum layered hydroxide to be loaded on biochar. In some embodiments, the dispersant can be polyvinyl pyrrolidone (PVP).

[0063] In some embodiments, the base asphalt includes one or more combinations of petroleum asphalt, natural asphalt, and coal tar asphalt.

[0064] In some embodiments, the base asphalt may be petroleum asphalt, and the petroleum asphalt may be selected from 70# petroleum asphalt and / or 90# petroleum asphalt.

[0065] In some embodiments, the asphalt modifier includes one or more combinations of styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), and styrene-butadiene rubber (SBR).

[0066] According to the embodiments of the present application, asphalt modifier refers to a natural or synthetic organic or inorganic material added to asphalt or asphalt mixture, which can be melted or dispersed in asphalt to improve or enhance the performance of asphalt. As asphalt modifier can effectively prevent the phase separation between the components in the coating material due to the polarity difference, asphalt modifier can make the asphalt waterproofing membrane composed of asphalt coating material have excellent overall performance such as adhesion, low temperature flexibility and durability.

[0067] In some embodiments, the asphalt modifier includes a combination of styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), and styrene butadiene rubber (SBR).

[0068] In some embodiments, the weight average molecular weight of SBS and SIS is 150,000 to 450,000, and the styrene content is 20% to 30%.

[0069] In some embodiments, the styrene-butadiene-styrene block copolymer is a star-shaped structure. The star-shaped SBS can improve the stability of asphalt, delay the aging process of asphalt, and reduce quality decline and performance degradation.

[0070] In some embodiments, the filler includes one or more combinations of calcium carbonate, heavy calcium carbonate, and organic montmorillonite.

[0071] According to the embodiments of the present application, the above-mentioned filler can play a role as a skeleton to enhance the stability and structural strength of the modified asphalt coating.

[0072] In some embodiments, the rubber powder includes tire rubber powder, miscellaneous rubber powder, or a combination thereof.

[0073] In some embodiments, the particle size of the rubber powder may be 60-80 meshes.

[0074] In some embodiments, the rubber content in the rubber powder may be 25% to 55%, and may be 30% to 40%.

[0075] According to the application examples, adding rubber powder with the above-mentioned particle size and rubber content into the modified asphalt coating can reduce the needle penetration of the modified asphalt, increase the softening point, enhance the ductility of the modified asphalt at low temperatures, and extend the service life of the coating.

[0076] Preparation method of modified asphalt coating material

[0077] An embodiment of the second aspect of the present application provides a method for preparing a modified asphalt coating, comprising the following steps S10 to S30.

[0078] S10, a step of preparing molten asphalt, comprising mixing base asphalt, cyclohexane oil and polyisoprene, and heating the mixture to react to obtain molten asphalt.

[0079] S20, a step of preparing modified asphalt, comprising mixing molten asphalt, asphalt modifier, rubber powder, vulcanizing agent, biochar, calcium iron aluminum layered hydroxide, and dispersant, and heating the mixture to react to obtain modified asphalt;

[0080] S30, a step of preparing a modified asphalt coating material, comprising mixing the modified asphalt and a filler, and heating the mixture to react, so as to obtain the modified asphalt coating material.

[0081] The preparation method of the modified asphalt coating provided in the embodiment of the present application is simple to operate, can be realized without changing the original production process of the modified asphalt coil, has low requirements on equipment, is well compatible with existing processes, and has great potential for large-scale application.

[0082] In some embodiments, the step of preparing molten asphalt includes mixing base asphalt, cyclohexane oil, and polyisoprene, and heating the mixture to 130-140° C. to obtain molten asphalt.

[0083] According to the embodiment of the present application, the mixing is carried out at 130-140° C., so that the asphalt can be fully melted, and the cycloalkane oil and polyisoprene are fully mixed with the asphalt to form a cross-linked network structure.

[0084] In some embodiments, the step of preparing modified asphalt includes heating the molten asphalt to 150-160°C, adding an asphalt modifier, adding rubber powder and a vulcanizing agent after the asphalt modifier is completely dissolved, and then adding biochar, calcium iron aluminum layered hydroxide, and a dispersant in sequence after the dissolution, and keeping the reaction warm for 1-2 hours to obtain modified asphalt.

[0085] According to the embodiment of the present application, rubber powder and vulcanizer are added after the asphalt modifier is completely dissolved, and biochar, calcium iron aluminum layered hydroxide and dispersant are added after the rubber powder is completely dissolved, which can ensure that the raw materials are evenly dispersed in the asphalt and improve the uniformity of mixing of the raw materials.

[0086] In some embodiments, the step of preparing the modified asphalt coating comprises heating the modified asphalt to 170-180° C., adding fillers, and reacting at the temperature for 2-3 hours to obtain the modified asphalt coating.

[0087] Asphalt waterproof membrane

[0088] The third aspect of the present application provides an asphalt waterproofing membrane, comprising:

[0089] Tire base;

[0090] A coating layer is provided on both side surfaces of the tread base layer, wherein the coating layer comprises the modified asphalt coating provided according to the embodiment of the first aspect of the present application or the modified asphalt coating obtained by the preparation method according to the embodiment of the second aspect of the present application;

[0091] The upper isolation layer is arranged on the surface of the coating material layer on one side.

[0092] The lower isolation layer is arranged on the surface of the coating layer on the other side.

[0093] In some embodiments, the upper isolation layer includes PET polyester isolation film or fine sand.

[0094] In some embodiments, the thickness of the upper isolation layer is 35-50 μm.

[0095] In some embodiments, the lower release layer comprises a polyethylene release film.

[0096] In some embodiments, the thickness of the lower isolation layer is 0.2-0.5 mm.

[0097] Preparation of asphalt waterproofing membrane

[0098] The preparation method of the asphalt waterproofing membrane comprises the following steps:

[0099] S10, preparing asphalt coating material;

[0100] S20, pre-impregnating the tire base to obtain a pre-impregnated tire base;

[0101] S30, applying the modified asphalt coating material to the surfaces of both sides of the prepreg tire base respectively to obtain a tire base layer and a coating material layer;

[0102] S40, covering the surface of the coating material layer on one side with a PET polyester isolation film or fine sand to obtain an upper isolation layer; covering the surface of the coating material layer on the other side with a polyethylene isolation film to obtain a lower isolation layer, thereby preparing an asphalt waterproofing membrane.

[0103] Example

[0104] The present invention is described below with reference to specific examples. It should be noted that the examples described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are conventional products that can be obtained commercially without specifying the manufacturer. Unless otherwise specified, the parts in the following examples all refer to parts by weight.

[0105] The sources or models of some raw materials in the following examples are as follows:

[0106] SBS: LG411;

[0107] SIS: Baling Petrochemical Co., Ltd., 1105;

[0108] SBR: Shandong Gaoshi Science and Technology Industry and Trade Co., Ltd., 095;

[0109] Polyisoprene: Shandong Kepler Biotechnology Co., Ltd., kpl-436521;

[0110] Tire rubber powder: Sichuan Zhongyu Rubber & Plastic New Material Technology Co., Ltd.;

[0111] Naphthenic oil: Naphthenic oil 4006, Shandong Taichang Petrochemical Technology Co., Ltd.;

[0112] Biochar: Henan Lize Environmental Protection Technology Co., Ltd., LZ04-05.

[0113] Example 1

[0114] Preparation of modified asphalt coating

[0115] A modified asphalt coating material, comprising the following raw materials in parts by weight:

[0116] 90# asphalt 40 parts;

[0117] SBS 1.5 parts;

[0118] SIS 0.5 part;

[0119] SBR 2 parts;

[0120] 2 parts of polyisoprene;

[0121] 8 parts of tire rubber powder;

[0122] 5 parts of naphthenic oil;

[0123] 10 parts of calcium iron aluminum layered hydroxide;

[0124] Biochar 5 parts;

[0125] Dispersant (PVP) 1 part;

[0126] Curing agent (benzoyl peroxide) 0.1 part;

[0127] Filler (200 mesh heavy calcium) 33 parts.

[0128] Calcium iron aluminum layered hydroxide was prepared by the following method:

[0129] S10, take 13.5 parts of Ca(NO3)2·4H2O, 3.3 parts of Fe(NO3)3·9H2O and 7.9 parts of Al(NO3)3·9H2O and dissolve them in 100 parts of deionized water to prepare solution A, and control the mass concentration of Fe(NO3)3 in solution A to be 2%;

[0130] S20, take 2 parts of NaOH and 4.25 parts of NaNO3 and dissolve them in 100 parts of deionized water to prepare solution B, and control the mass concentration of NaOH in solution B to be 2%;

[0131] S30, dripping the A and B solutions into a three-necked flask containing alcohol and NaOH drop by drop, stirring magnetically for 2 hours, and then placing in an autoclave for crystallization for 18 hours. After the reaction, the solution is centrifuged and washed several times until neutral, and the obtained solid material is placed in a vacuum drying oven at 80° C. and dried for 12 hours, and then ground into powder after drying to obtain calcium iron aluminum layered hydroxide.

[0132] The modified asphalt coating is prepared by the following method:

[0133] S10, put 90# petroleum asphalt, cycloparaffin oil and polyisoprene in a metal aluminum can, use a heating jacket to raise the temperature to 130°C, put in a stirring head (speed 1500r / min) and stir and mix evenly;

[0134] S20, heating to 160°C, adding styrene-butadiene-styrene block copolymer (SBS), styrene-butadiene rubber (SBR), styrene-isoprene-styrene block copolymer (SIS), after the modifier is completely dissolved in the asphalt, adding tire rubber powder and vulcanizing agent, and adding biochar, calcium iron aluminum layered hydroxide and polyvinyl pyrrolidone (PVP) in sequence after continuing to completely dissolve, controlling the temperature at 160°C, and keeping the reaction for 1 hour;

[0135] S30, continue to raise the temperature to 180°C, add filler, and keep the temperature to react for 2 hours to obtain a modified asphalt coating material.

[0136] Asphalt waterproof membrane

[0137] An asphalt waterproofing membrane comprises a base layer, a coating layer coated on both sides of the base layer, an upper insulating layer pressed on one side of the coating layer surface and a lower insulating layer pressed on the other side of the coating layer surface, wherein the upper insulating layer is a 50 μm thick PET polyester insulating film and the lower insulating layer is a 0.4 mm thick high-density polyethylene insulating film. The asphalt waterproofing membrane is prepared by the following method:

[0138] S10, passing the tire base through a prepreg pool for prepreg treatment, and squeezing out excess prepreg through a pair of rollers;

[0139] S20, applying the modified asphalt coating material to the upper and lower surfaces of the tire base respectively, and then extruding the modified asphalt coating material into a fixed thickness through a fixed roller to obtain a tire base layer and a coating layer;

[0140] S30, pressing a layer of PET polyester isolation film on the surface of the upper surface coating layer, pressing a layer of high-density polyethylene isolation film on the surface of the lower surface coating layer, and then cooling with cooling pool water, pulling, measuring thickness, and rolling up to obtain a modified asphalt coil.

[0141] Example 2

[0142] The preparation of calcium iron aluminum layered hydroxide, the preparation of modified asphalt coating material, and the asphalt waterproofing membrane in this embodiment are the same as those in Example 1, except that the contents of the components in the modified asphalt coating material are different. The modified asphalt coating material includes the following components in parts by weight:

[0143] 90# asphalt 40 parts;

[0144] SBS 1.2 parts;

[0145] SIS2.3 copies;

[0146] SBR 2 parts;

[0147] 2 parts of polyisoprene;

[0148] 6 parts of tire rubber powder;

[0149] 5 parts of naphthenic oil;

[0150] 15 parts of calcium iron aluminum layered hydroxide;

[0151] Biochar 5 parts;

[0152] Dispersant (PVP) 1 part;

[0153] Curing agent (benzoyl peroxide) 0.1 part;

[0154] Filler (200 mesh heavy calcium) 28 parts.

[0155] Example 3

[0156] The preparation of calcium iron aluminum layered hydroxide, the preparation of modified asphalt coating material, and the asphalt waterproofing membrane in this embodiment are the same as those in Example 1, except that the contents of the components in the modified asphalt coating material are different. The modified asphalt coating material includes the following components in parts by weight:

[0157] 90# asphalt 40 parts;

[0158] 1 copy of SBS;

[0159] SIS1 copy;

[0160] SBR 2 parts;

[0161] 2 parts of polyisoprene;

[0162] 4 parts of tire rubber powder;

[0163] 5 parts of naphthenic oil;

[0164] Calcium iron aluminum layered hydroxide 20 parts;

[0165] Biochar 5 parts;

[0166] Dispersant (PVP) 1 part;

[0167] Curing agent (benzoyl peroxide) 0.1 part;

[0168] Filler (200 mesh heavy calcium) 23 parts.

[0169] Example 4

[0170] The preparation of calcium iron aluminum layered hydroxide, the preparation of modified asphalt coating material, and the asphalt waterproofing membrane in this embodiment are the same as those in Example 1, except that the composition ratio of the modified asphalt coating material is different. The modified asphalt coating material includes the following components in parts by weight:

[0171] 90# asphalt 40 parts;

[0172] SBS 1.5 parts;

[0173] SIS1.5 copies;

[0174] SBR 2 parts;

[0175] 2 parts of polyisoprene;

[0176] 8 parts of tire rubber powder;

[0177] 5 parts of naphthenic oil;

[0178] 10 parts of calcium iron aluminum layered hydroxide;

[0179] Curing agent (benzoyl peroxide) 0.1 part;

[0180] Filler (200 mesh heavy calcium) 33 parts.

[0181] Example 5

[0182] The preparation of calcium iron aluminum layered hydroxide, the preparation of modified asphalt coating material and asphalt waterproofing membrane in this embodiment are the same as those in Example 1, except that the composition of the asphalt modifier is different, and the asphalt modifier is 4 parts of SBS.

[0183] Comparative Example 1

[0184] The preparation of the modified asphalt coating material and the asphalt waterproofing membrane in this comparative example are the same as those in Example 1, except that the composition ratio of the modified asphalt coating material is different. The modified asphalt coating material includes the following components in parts by weight:

[0185] 90# asphalt 40 parts;

[0186] SBS 1.5 parts;

[0187] SIS 0.5 part;

[0188] SBR 2 parts;

[0189] 2 parts of polyisoprene;

[0190] 8 parts of tire rubber powder;

[0191] 5 parts of naphthenic oil;

[0192] Curing agent (benzoyl peroxide) 0.1 part;

[0193] Filler (200 mesh heavy calcium) 33 parts.

[0194] Comparative Example 2

[0195] The preparation of the modified asphalt coating material and the asphalt waterproofing membrane in this comparative example are the same as those in Example 1, except that the composition ratio of the modified asphalt coating material is different. The modified asphalt coating material includes the following components in parts by weight:

[0196] 90# asphalt 40 parts;

[0197] SBS 1.5 parts;

[0198] SBR 2 parts;

[0199] 8 parts of tire rubber powder;

[0200] 5 parts of naphthenic oil;

[0201] Curing agent (benzoyl peroxide) 0.1 part;

[0202] Filler (200 mesh heavy calcium) 33 parts.

[0203] Comparative Example 3

[0204] The preparation of the modified asphalt coating and the asphalt waterproofing membrane in this comparative example are the same as those in Example 1, except that the calcium iron aluminum layered hydroxide is replaced by an equal amount of magnesium aluminum layered hydroxide (Jiangsu Xianfeng Nanotechnology Co., Ltd., MgAl-LDH two-dimensional layered double metal hydroxide, 102911).

[0205] Detection part

[0206] 1. Basic performance: The performance of the waterproof membrane samples obtained in each embodiment and comparative example was tested according to the standard GB / T35467-2017 "Wet-laid waterproof membrane";

[0207] 2. UV aging test: Use a UV aging test chamber to perform UV aging resistance test at 85°C;

[0208] 3. Xenon lamp aging test: Perform xenon lamp accelerated aging test in accordance with GB / T 27789-2011;

[0209] 4. Salt / alkali resistance test: Soak the sample in a saturated sodium chloride / calcium hydroxide solution at 23°C for 168 hours, take it out and wipe the surface solution dry, and then test the low-temperature flexibility after curing under standard conditions for 24 hours.

[0210] The test results are shown in Table 1 below.

[0211] Table 1:

[0212]

[0213]

[0214] As can be seen from Table 1, in Examples 1-5, calcium iron aluminum layered hydroxides are added to modify the asphalt coating, and the obtained asphalt roll materials have good UV resistance and salt-alkali resistance. After UV aging, the product still maintains a good appearance, without powdering and cracking, and maintains good low-temperature flexibility. However, in Comparative Example 1, calcium iron aluminum layered hydroxides are not added to modify the asphalt coating, and the UV resistance of the obtained waterproof roll materials is significantly reduced. After aging tests, powdering and cracking phenomena occur, and the low-temperature flexibility is significantly deteriorated.

[0215] From Table 1, we can see that the addition of calcium iron aluminum layered hydroxide can effectively improve the UV resistance and salt-alkali resistance of the waterproof membrane, and other performance indicators meet the national standards and have excellent performance, which provides a strong guarantee for the construction and use of the waterproof membrane under marine working conditions.

[0216] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A modified asphalt coating material, characterized in that: The modified asphalt coating material is applied to waterproof coiled materials under marine working conditions, and comprises the following components by weight: 40 parts of base asphalt; 3.5~10 parts of asphalt modifier; 2-5 parts of polyisoprene; 5~10 parts of rubber powder; 1-5 parts of naphthenic oil; 10-20 parts of calcium iron aluminum layered hydroxide; Vulcanizing agent 0.1~0.3 parts; 20~40 parts of filler; 5-10 parts of biochar; Dispersant 0.5~2 parts; wherein, The calcium iron aluminum layered hydroxide has a dihydroxy structure; The modified asphalt coating material is prepared by the following method: The step of preparing molten asphalt comprises mixing base asphalt, cyclohexane oil and polyisoprene, and heating the mixture to 130-140° C. to obtain molten asphalt; The step of preparing modified asphalt comprises heating the molten asphalt to 150-160° C., adding an asphalt modifier, adding rubber powder and a vulcanizing agent after the asphalt modifier is completely dissolved, and then sequentially adding biochar, calcium iron aluminum layered hydroxide, and a dispersant after the asphalt modifier is dissolved, and reacting the mixture for 1-2 hours to obtain modified asphalt; The step of preparing the modified asphalt coating material comprises heating the modified asphalt to 170-180° C., adding fillers, and reacting the mixture for 2-3 hours to obtain the modified asphalt coating material.

2. The modified asphalt coating material according to claim 1, characterized in that: The calcium-iron-aluminum-based layered hydroxide is prepared by a coprecipitation reaction between a metal salt solution containing calcium ions, iron ions and aluminum ions and an alkaline solution.

3. The modified asphalt coating material according to claim 2, characterized in that: The molar ratio of calcium ion, iron ion and aluminum ion in the metal salt solution is 10:(0.5-2):(3-5).

4. The modified asphalt coating material according to claim 2 or 3, characterized in that: The interlayer anions of the calcium iron aluminum layered hydroxide include nitrate ions.

5. The modified asphalt coating material according to claim 1, characterized in that: The matrix asphalt includes one or more combinations of petroleum asphalt, natural asphalt, coal tar asphalt, and / or The asphalt modifier includes one or more combinations of styrene-butadiene-styrene block copolymer, styrene-isoprene-styrene block copolymer, styrene-butadiene rubber, and / or The rubber powder includes tire rubber powder, and / or The filler includes one or more combinations of calcium carbonate and organic montmorillonite.

6. An asphalt waterproofing membrane, characterized in that: include: Tire base; A coating layer is provided on both side surfaces of the tread base layer, wherein the coating layer comprises the modified asphalt coating according to any one of claims 1 to 5; An upper isolation layer is provided on the surface of the coating material layer on one side; The lower isolation layer is arranged on the surface of the coating material layer on the other side.

7. The asphalt waterproofing membrane according to claim 6, characterized in that: The upper isolation layer comprises a PET polyester isolation film layer or a fine sand layer, and / or The thickness of the upper isolation layer is 35-50 μm, and / or The lower isolation layer comprises a polyethylene isolation film layer, and / or The thickness of the lower isolation layer is 0.2~0.5mm.

Citation Information

Patent Citations

  • Preparation method and application of SBS / rubber compound modification asphalt

    CN105419364A

  • Anticorrosive paint based on modified graphene and preparation method thereof