Sand mold making for metal additive casting

By using the casting mold layer formed by the sand mold in additive metal casting, and using replaceable material layers and molten metal replacement technology, the problems of multiple thermal cycles and rapid customization of the casting mold are solved, achieving efficient and rapid production. The additive metal casting process improves process efficiency and part quality.

CN117597208BActive Publication Date: 2024-10-18MAGNUS METALS LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202280046292.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-14
Publication Date
2024-10-18
Estimated Expiration
2042-04-14

AI Technical Summary

Technical Problem

In the existing additive metal casting technology, the casting mold needs to withstand multiple thermal cycles and is difficult to quickly customize, resulting in low process efficiency. Moreover, traditional sand casting has shortcomings in efficient and rapid additive metal casting.

Method used

Using casting layers formed by sand molding, by embedding replaceable material layers in each production layer and replacing these layers with molten metal, combined with monitoring units and mechanical means, the efficient preparation and removal of the casting layers is achieved to form an efficient Additive casting system.

Benefits of technology

An efficient and fast additive metal casting process is achieved, which improves the transfer and use efficiency of casting mold layers, reduces the amount of metal used, and improves the quality and production speed of parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117597208B_ABST
    Figure CN117597208B_ABST
Patent Text Reader

Abstract

A casting system for casting an article, wherein the casting system may include: a mold system, an alternative material supply system, and a molten metal processing system. The casting system may be configured to produce multiple production layers in an additive manner, one currently produced production layer following another. For each currently produced production layer: (i) the mold system is configured to form one or more mold layers; (ii) the alternative material supply system is configured to provide one or more alternative material layers; (iii) the molten metal processing system is configured to form one or more current article regions of the currently produced production layer by providing molten metal that replaces the one or more alternative material layers.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] Additive metal casting is a casting process designed to improve upon traditional casting processes. Instead of pouring the molten metal into a mold in one continuous step, it is poured in layers. Additive metal casting allows for better control over the solidification process of the part, allowing for control over the metallurgical properties of the part. The molds are produced in steps to allow for the metal to be poured in layers. The benefits of additive metal casting include a shorter time from design to part manufacturing, as well as a reduction in the amount of metal required.

[0002] Molds used for additive metal casting must meet requirements that molds used for conventional casting cannot: Additive metal casting requires casting with an open mold, the mold must withstand multiple thermal cycles of metal heating, metal pouring, and cooling, and it may be necessary to prepare a custom mold on site for the part being cast.

[0003] Sand casting is a well-known technique that uses sand as a mold material. In addition to sand, a suitable binder (usually clay) is mixed or accompanied with the sand. The mixture is usually moistened with water, and sometimes with other substances, to enhance the strength and plasticity of the clay, making the aggregate suitable for molding. The sand is usually contained in a system of frames or mold boxes called flasks. The mold cavity is made by compacting the sand around a model called a pattern, by carving directly in the sand, or by 3D printing.

[0004] The foundry industry needs an additive metal casting apparatus and method that efficiently casts using a sand mold and quickly adopts additive metal casting. Summary of the invention

[0005] A casting system for casting an article may be provided, wherein the casting system may include: a mold system; an alternative material supply system; and a molten metal processing system. The casting system is configured to additively produce a plurality of production layers, one currently produced production layer following another. For each currently produced production layer: the mold system is configured to form one or more mold layers; the alternative material supply system is configured to provide one or more alternative material layers; and the molten metal processing system is configured to form one or more current article regions of the currently produced production layer by providing molten metal that replaces the one or more alternative material layers.

[0006] A method may be provided, which may include: producing multiple production layers by a casting system in an additive manner, one currently produced production layer following another; wherein, for each currently produced production layer: one or more mold layers are formed by a mold system of the casting system; one or more replaceable material layers are provided by a replaceable material providing system of the casting system; and one or more current article regions of the currently produced production layer are formed by a molten metal processing system of the casting system by providing molten metal that replaces the one or more replaceable material layers.

[0007] A non-transitory computer-readable medium for casting articles can be provided, wherein the instructions stored in the non-transitory computer-readable medium are used to: produce multiple production layers in an additive manner through a casting system, one currently produced production layer following another; wherein, for each currently produced production layer: one or more casting mold layers are formed by a casting system of the casting system; one or more replaceable material layers are provided by a replaceable material providing system of the casting system; and one or more current article regions of the currently produced production layer are formed by a molten metal processing system of the casting system by providing molten metal that replaces the one or more replaceable material layers. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] The subject matter regarded as the invention is particularly pointed out and distinctly claimed in the concluding portion of the specification. However, the organization and method of operation of the invention, together with objects, features, and advantages thereof, are best understood by reference to the following detailed description and accompanying drawings:

[0009] Figure 1A is an example of a gating system;

[0010] Figure 1B is an example of a casting system;

[0011] Figure 1C is an example of a method;

[0012] Figure 1D is an example of a method;

[0013] Figure 2A depicts an embedded pattern area before and after removal of a patterned article according to an embodiment of the present invention;

[0014] Figure 2B depicts concentric embedded pattern areas before and after removal of a patterned article in accordance with an embodiment of the present invention;

[0015] Figure 2C depicts an embedded pattern area with open areas in the pattern according to an embodiment of the present invention;

[0016] Figure 3Schematically illustrates metal additive casting using a sand mold with sand-based embedded areas and an ex-situ mold layer build-up structure according to an embodiment of the present invention;

[0017] Figure 3A Schematically illustrating metal additive casting using a sand mold with a sand-based embedded area and an in-situ mold layer build-up structure according to an embodiment of the present invention;

[0018] Figure 3B According to an embodiment of the present invention, Figure 3 A flowchart of an embodiment described in;

[0019] Figure 3C According to an embodiment of the present invention, Figure 3A A flowchart of an embodiment described in;

[0020] Figure 4 Schematically illustrates metal additive casting using a sand mold with sacrificial embedded regions and an ex situ mold layer build-up structure according to an embodiment of the present invention;

[0021] Figure 4A Schematically illustrates metal additive casting using a sand mold with a sacrificial embedded area and an in-situ mold layer build-up structure according to one embodiment of the present invention;

[0022] Figure 4B According to an embodiment of the present invention, Figure 4 A flowchart of an embodiment described in;

[0023] Figure 4C According to an embodiment of the present invention, Figure 4A Flowchart of the molding process 4000' of the embodiment described in;

[0024] Figure 5 Schematically illustrates the use of grooves and protrusions for connecting between various mold layers according to an embodiment of the present invention;

[0025] Figure 5A Schematically depicts a device for forming protrusions and / or grooves at the bottom of a casting layer according to an embodiment of the present invention;

[0026] Fig. 6A Schematically depicts metal additive casting using a sand mold with grooves to achieve transfer using an end effector with a fork arm according to an embodiment of the present invention;

[0027] Figure 6B Schematically depicts metal additive casting using a sand mold with grooves in different locations to enable transfer using an end effector with a fork arm according to an embodiment of the present invention;

[0028] Figure 7 A system according to an embodiment of the present invention is schematically described for preparing a mold layer in a mold preparation location and transferring it to a molding location for molding an article; and

[0029] Figure 8 Three different systems for preparing a casting layer according to embodiments of the present invention are schematically illustrated.

[0030] It is understood that, in order to make the illustration simple and clear, the elements shown in the figures are not necessarily drawn to scale. For example, for the sake of clarity, the size of some elements may be exaggerated relative to other elements. In addition, where appropriate, the reference numerals in the figures may be repeated to indicate corresponding or similar elements. DETAILED DESCRIPTION

[0031] In the following detailed description, many specific details are listed to facilitate a thorough understanding of the present invention. However, it will be appreciated by those skilled in the art that the present invention can be practiced without these specific details. In other cases, well-known methods, procedures, and components are not described in detail to avoid obscuring the present invention. As used herein, the term "ex-situ" refers to mold preparation outside the metal casting area, and the term "in-situ" refers to mold preparation in the metal casting area.

[0032] A casting system for casting an article may be provided. Casting includes forming one or more mold layers that are displaced by molten metal.

[0033] See also Figure 1A The casting system may include a casting mold system 111 , a replaceable material supply system 113 , a molten metal processing system 108 and a frame system 117 . Figure 1A Additional systems and / or units that may belong to the casting system or may be assigned to the casting process performed by the casting system are shown. These additional systems and / or units may include a motion system 107, a monitoring unit 103 that may include one or more sensors, a building unit 119, and a frame system 117.

[0034] The casting system is configured to produce multiple production layers in an additive manner, one currently produced production layer following another. Additive means that one production layer is produced after another. The formation of one production layer after another improves the quality of the produced object.

[0035] Where, for each currently produced production layer:

[0036] i. The mold system is configured to form one or more mold layers. The one or more mold layers may form one or more patterns.

[0037] ii. The replaceable material providing system is configured to provide one or more replaceable material layers.

[0038] iii. The molten metal processing system is configured to form one or more current article regions of a current production layer by providing molten metal that replaces the one or more replaceable material layers.

[0039] When molten metal is provided, the layer of replaceable material may be replaced. For example, the replaceable material may decompose due to heat and / or contact with the molten metal.

[0040] It may be beneficial that the replaceable material may decompose even in the presence of molten metal that has begun to cool (e.g., even several minutes after the molten metal has been deposited) because this may prevent the formation of islands of undecomposed replaceable material within the metal. For example, the replaceable material may dissolve even at temperatures below 600 degrees Celsius, above 580 degrees Celsius, etc.

[0041] The layer of replaceable material may be removed prior to providing the molten metal.

[0042] The casting system may include an alternative material removal system 115 configured to remove at least one of the one or more alternative material layers prior to at least one of the one or more molten metal layers forming one or more current article regions being formed.

[0043] The replaceable material removal system 115 can use any removal element shown in the specification. For example, the replaceable material removal system 115 may include at least one of a suction unit 1151, a mechanical removal unit 1152, a temperature-based removal unit 1153 (which can be heated and / or frozen or cooled), a chemical-based removal unit 1154 (e.g., an etching unit), etc.

[0044] The frame system 117 is configured to generate frame areas that define frames (sandbox layers) that divide production layers. The frame may be in contact with one or more mold areas.

[0045] The frame may be generated by the frame system 117. Alternatively, the frame may be generated by a system other than the casting system and positioned by the frame system 117 at the casting location.

[0046] Each production layer may obtain (generate or receive and place) one or more frame areas. Alternatively, multiple production layers may also obtain (generate or receive and place) one or more frame areas.

[0047] The frame region may be made of a heat resistant material—because the frame region may be located near the molten metal (although the molten region separates the frame from the molten layer). For example, the frame region may be made of wood, steel, 3D printable materials, non-3D printable materials, etc.

[0048] The replaceable material providing system 113 may be configured to generate one or more replaceable material layers. Alternatively, the replaceable material providing system may be configured to receive the one or more replaceable material layers and position the one or more replaceable material layers in a casting position.

[0049] The molding system 111 may be configured to perform at least one of the following:

[0050] i. Distributing the mold material to form one or more mold layers. The mold material may be a ceramic mold material.

[0051] ii. Forming one or more casting mold layers by sand molding.

[0052] iii. Forming one or more casting mold layers comprising sand and one or more binders.

[0053] iv. forming one or more mold layers including sand and a plurality of binders. The removal processes of at least two binders may be different. For example, one binder may be removed by heat and another binder may be removed by a mechanical removal process.

[0054] Examples of replaceable material layers include a hardened sand layer that can be removed by one or more of grinding, vibration, air flow, suction or other mechanical means, a compacted sand that can be mechanically removed by one or more of grinding, vibration, air flow, suction or other mechanical means, a binder-hardened sand that can be removed by one or more of heating, grinding, vibration, air flow, suction or other mechanical means, and a disposable material configured to evaporate when the molten metal is cast.

[0055] The replaceable material layer may be removed from the mold layer by at least one pattern removal means selected from the group consisting of heating, grinding, vibration, air flow, suction, or other mechanical means.

[0056] The mold system may include a mold powder supply system ( Figure 1B denoted by 102), a casting adhesive dispensing system ( Figure 1B 104) and a mold powder removal system ( Figure 1B denoted by 106).

[0057] For each currently producing production tier:

[0058] i. The mold powder providing system 102 is configured to provide one or more current mold powder layers.

[0059] ii. the mold binder dispensing system 104 is configured to form one or more current mold regions within each of the one or more current mold powder layers by selectively dispensing particles of one or more binders that bind some of the mold powder particles in the current mold powder layer; and

[0060] iii. The mold powder removal system 106 is configured to remove mold powder particles located within a certain area of ​​each layer in the one or more current mold powder layers, the certain area being defined by at least some of the one or more current mold regions.

[0061] The metal processing system 108 may be configured to perform at least one of the following:

[0062] i. forming one or more current article regions in a production layer currently being produced by depositing molten metal at a cavity created in a mold layer and applying at least one of a pre-deposition process and a post-deposition process.

[0063] ii. forming one or more current article regions in the current production layer by depositing molten metal at the cavities created in the mold layer and applying at least one of a pre-deposition process and a post-deposition process, such that the pre-deposition process and the post-deposition process include heating, wherein the deposition unit, the pre-deposition process unit, and the post-deposition process unit are physically coupled and share a common motion arrangement (referred to herein as preparation and deposition and post (PDP) processing). (In other words, the preparation and deposition and post (PDP) processing are applied to replace the one or more replaceable material layers).

[0064] iii. Application in a localized manner (as part of PDP processing) Preparation, deposition and post-processing Localized manner - can be performed in an area not exceeding a few centimeters in width or length.

[0065] iv. Applying (as part of the PDP process) at least two of preparation, deposition and post-treatment in a spatially distributed manner. Spatially distributed means over a distance of more than 10 or 20 cm.

[0066] v. Heating the environment in the current area of ​​the item. The environment may be more than 10 cm across the deposition location of the molten metal.

[0067] The monitoring unit 103 may be configured to monitor one or more aspects of the casting process performed by the casting system. For example, the monitoring unit 103 may monitor the operation of one or more of the mold system 111, the replaceable material supply system 113, the replaceable material removal system 115, the molten metal processing system 108, the frame system 117, and the motion system 107.

[0068] The monitoring unit 103 includes one or more sensors of one or more types, including passive sensors, active sensors, optical sensors, infrared sensors, vibration sensors, motion sensors, torque sensors, accelerometers, thermal sensors, X-ray sensors, electron beam sensors, ion beam sensors, spectrometers, etc.

[0069] The monitoring unit 103 may include one or more processors for processing the sensed information and providing alerts, suggestions on how to modify any aspect of the casting process, and the like.

[0070] For example, the monitoring unit 103 (or one or more controllers 105 which may be external to the monitoring unit) may be configured to control the provision of the one or more replaceable material layers based on the monitoring.

[0071] Figure 1C is an example of a method 130 for casting an article.

[0072] The method 130 may include a step 140 of additively producing a plurality of production layers, one currently produced production layer following another.

[0073] Step 140 may include steps 142 , 144 , 146 , and 150 .

[0074] Step 142 may include starting to manufacture the production layers currently being produced, wherein, for each production layer currently being produced:

[0075] Step 142 is followed by step 144 of forming one or more mold layers by a mold system of the casting system.

[0076] i. dispensing a casting mold material to form the one or more casting mold layers. The casting mold material may be a ceramic casting mold material.

[0077] ii. forming the one or more casting mold layers by sand molding.

[0078] iii. forming the one or more casting mold layers comprising sand and one or more binders.

[0079] iv. forming the one or more mold layers comprising sand and a plurality of binders. At least two binders differ from each other in their removal processes. For example, one binder may be removed by heat and another binder may be removed by a mechanical removal process.

[0080] v. forming the one or more mold layers by a mold system, which may include a mold powder providing system, a mold binder dispensing system, and a mold powder removing system.

[0081] vi. For each production layer currently being produced: (i) a mold powder providing system provides one or more current mold powder layers; (ii) a mold binder dispensing system selectively dispenses particles of one or more binders that bind some of the mold powder particles in the current mold powder layer to form one or more current mold regions in the one or more current mold powder layers; and (iii) a mold powder removal system removes mold powder particles within a certain area of ​​each layer of the one or more current mold powder layers, wherein the certain area is defined by at least some of the one or more current mold regions.

[0082] Step 144 is followed by step 146 of providing one or more layers of alternative material by an alternative material providing system of the casting system.

[0083] Step 146 may include generating the one or more replaceable material layers by a replaceable material providing system.

[0084] Alternatively, step 146 may include receiving one or more layers of replaceable material by an replaceable material providing system and positioning the one or more layers of replaceable material in a casting location.

[0085] Step 146 may be followed by step 150 of forming, by a molten metal processing system of the casting system, one or more current article regions of the production layer currently being produced by providing molten metal that replaces one or more layers of replaceable material.

[0086] Step 150 may include at least one of the following:

[0087] i. Forming one or more current article regions of a current production layer by applying preparation, deposition and post (PDP) processing to replace the one or more replaceable material layers.

[0088] ii. Application in a localized manner (as part of PDP processing) Preparation, deposition and post-processing Localized manner - can be performed in areas up to a few centimeters in width or length.

[0089] iii. At least two of preparation, deposition and post-treatment are applied (as part of the PDP process) in a spatially distributed manner. Spatially distributed means over a distance of more than 10 or 20 cm.

[0090] iv. Heating the environment in the current area of ​​the item. The environment may be more than 10 cm across the deposition location of the molten metal.

[0091] When molten metal is provided, the layer of replaceable material may be displaced—for example, the layer of replaceable material may decompose due to heat and / or contact with the molten metal.

[0092] It may be beneficial that the replaceable material may decompose even when the molten metal has begun to cool (e.g., even a few minutes after the start of molten metal deposition) because this may prevent the formation of islands of undecomposed replaceable material in the metal. For example, the replaceable material may dissolve even when the temperature is below 600 degrees Celsius or above 580 degrees Celsius, etc.

[0093] Step 150 is followed by step 152 : determining whether another production layer needs to be made, and if so, jumping to step 142 , otherwise ending the production layer formation, as shown by end step 156 .

[0094] The method 130 may include a step 158 of forming a frame. The forming of the frame may be performed per production layer - and in this case, step 158 may include multiple iterations 159, and during each iteration, one or more frame regions (associated with the production layer) are formed - each iteration 159 is performed between steps 142 and 144. Alternatively, the forming of the frame may include forming one or more frame regions for multiple production layers at a time. Also, in another example, the frame may be formed for each item at a time.

[0095] The method 130 may further include step 160: monitoring one or more aspects of the casting process performed by the casting system—for example, monitoring steps 144 and / or 146 and / or 150. The monitoring step may provide one or more monitoring results. The monitoring results may be sensing information or the result of processing the sensing information.

[0096] Monitoring may be performed by a monitoring unit 103, which may include one or more sensors of one or more types—passive sensors, active sensors, optical sensors, infrared sensors, vibration sensors, motion sensors, torque sensors, accelerometers, thermal sensors, X-ray sensors, electron beam sensors, ion beam sensors, spectrometers, etc.

[0097] Monitoring results may include alerts, suggestions on how to modify any aspect of the casting process, etc.

[0098] Step 160 may include controlling any aspect of the casting process based on one or more monitoring results. For example - step 160 may include controlling the provision of the one or more alternative material layers based on the monitoring.

[0099] Figure 1D is an example of a method 131 for casting an article.

[0100] The method 131 may include a step 140 of additively producing a plurality of production layers, one currently produced production layer following another.

[0101] Step 140 may include step 142 : starting to manufacture the production layer currently being produced, wherein for each production layer currently being produced.

[0102] Step 142 is followed by step 144 of forming one or more mold layers by a mold system of the casting system.

[0103] Step 144 is followed by step 146 of providing one or more layers of alternative material by an alternative material providing system of the casting system.

[0104] Step 146 may be followed by step 148 of removing at least one of the one or more molten metal layers by a replaceable material removal system of the casting system before at least one of the one or more molten metal layers forming the one or more current article regions is formed.

[0105] Step 148 may be performed by at least one of a suction unit, a mechanical removal unit, a temperature-based removal unit, or a chemical-based removal unit.

[0106] Step 148 is followed by step 150 of forming, by a molten metal processing system of the casting system, one or more current article regions of the current production layer by providing molten metal that replaces one or more layers of replaceable material.

[0107] Step 150 is followed by step 152 : determining whether another production layer needs to be manufactured, and if so, jumping to step 142 , otherwise ending the formation of the production layer, as shown in end step 156 .

[0108] Method 131 may include a step 158 of forming a frame. The forming of the frame may be performed per production layer—in which case step 158 may include multiple iterations 159, and during each iteration, one or more frame regions (associated with the production layer) are formed—and each iteration 159 is performed between steps 142 and 144. Alternatively, the forming of the frame may include forming one or more frame regions for multiple production layers at a time. Additionally, in another example, the frame may be formed for each item at a time.

[0109] The method 131 may also include step 160 of monitoring one or more aspects of a casting process performed by the casting system.

[0110] One layer of the mold area can form a pattern. For example, sand molds can be used with embedded pattern items.

[0111] The removal operation may be performed by a chemical-based removal unit.

[0112] One or more layers of replaceable material are decomposable in the presence of molten metal.

[0113] The method may include generating one or more replaceable material layers by a replaceable material providing system.

[0114] The method may include receiving one or more layers of replaceable material by a replaceable material providing system and positioning the one or more layers of replaceable material in a casting location.

[0115] The method may include forming one or more mold layers by sand molding from a mold system.

[0116] The one or more casting mold layers may include sand and one or more binders.

[0117] The one or more casting mold layers may include sand and a binder, wherein at least two binders differ from each other by their removal process.

[0118] For each currently produced production layer, the method may include: providing one or more current mold powder layers by a mold powder providing system of the mold system; forming one or more current mold regions in each of the one or more current mold powder layers by selectively distributing particles of one or more binders that bond some mold powder particles in the current mold powder layer by a mold binder dispensing system of the mold system; and removing mold powder particles located in a certain area of ​​each of the one or more current mold powder layers by a mold powder removal system of the mold system, wherein the certain area is defined by at least some of the one or more current mold regions.

[0119] For each currently produced production layer, the method may include dispensing a mold material by the mold system to form one or more mold layers.

[0120] The method may include forming, by a metal processing system, one or more current article regions of a current production layer by applying preparation, deposition, and post (PDP) processing to replace one or more replaceable material layers.

[0121] The operation of applying PDP treatments may include applying preparation, deposition, and post-treatment in a localized manner.

[0122] The operation of applying the PDP treatment may include applying at least two of preparation, deposition, and post-treatment in a spatially distributed manner.

[0123] The method may include heating, by the metal processing system, an environment in the current article area.

[0124] The method may comprise monitoring, by a monitoring unit, the provision of one or more replaceable material layers.

[0125] The method may include controlling, by a controller, provision of one or more replaceable material layers based on the monitoring.

[0126] One or more of the alternative material layers may be configured to decompose at temperatures exceeding 590 degrees Celsius.

[0127] One or more of the alternative material layers may be configured to decompose at a temperature reached by the molten layer within a maximum of a few minutes from deposition.

[0128] The method may include generating a frame region from a frame system of the gating system, the frame region defining a frame surrounding one or more mold regions.

[0129] A method for forming a mold for additively casting a metal article can be provided, comprising: preparing a mold layer comprising at least one removable pattern embedded in the mold layer; positioning the mold layer in a casting position; casting molten metal into at least one casting pattern article, removing at least one embedded removable casting pattern in the mold layer and replacing it with molten metal, and then repeating the previous steps with at least one additional mold layer, wherein the at least one additional mold layer is placed on top of the previous mold layer.

[0130] In some embodiments, at least one casting mold layer is formed by sand molding.

[0131] In some embodiments, at least one casting pattern is formed by embedding the model article in the casting mold layer prior to or simultaneously with sand molding.

[0132] In some embodiments, at least one patterned article is made of at least one of the following materials: loose sand within a hardened sand mold layer that is removable by one or more of grinding, vibration, air flow, suction or other mechanical means; compacted sand that is mechanically removable by one or more of grinding, vibration, air flow, suction or other mechanical means; binder-hardened sand that is removable by one or more of heating, grinding, vibration, air flow, suction or other mechanical means; and a disposable material configured to evaporate when molten metal is cast.

[0133] In some embodiments, at least one pattern item is removed from the mold layer before casting the casting material. In some further embodiments, the at least one pattern item is removed from the mold layer by at least one of pattern removal means consisting of heating, grinding, vibration, air flow, suction or other mechanical means.

[0134] In some embodiments, the at least one pattern item is removed from the mold layer during casting of the casting material.

[0135] In some embodiments, the mold layer is prepared by filling the mold layer frame with sand and hardening the sand with a hardening material.

[0136] In some embodiments, the method further comprises positioning the at least one cast pattern item in a corresponding position of the pattern item in the mold layer frame prior to filling the mold layer frame with sand.

[0137] In some embodiments, the positioning of the at least one additional mold layer on top of the previous mold layer is done by using alignment means comprising grooves and / or protrusions.

[0138] According to one aspect of the invention, embodiments of the invention consist of a multi-step additive molten metal casting process in which a sand mold layer is used with an embedded patterned article. According to another aspect of the invention, in one embodiment, the mold layer can be a completely uniform sand mold layer, and the mold opening can be made by removing sand from the mold layer in the shape of the article (e.g., by grinding), without using a patterned article. The casting process can be for one part or for multiple parts in the mold.

[0139] Special software can receive a computer-aided design (CAD) file of a part and can generate a stacked representation scheme, which, when the stacked representation schemes are stacked on each other, forms a designed part. Each layered portion of the designed part ("pattern object") can be embedded in casting sand to form a mold layer that is open at the top, open at the bottom or closed (except for the first layer, the bottom of which can be closed). The pattern objects that can be embedded in each layer can be made of various removable or sacrificial or disposable materials, including polystyrene, sand or other materials. The pattern objects can be created by additive deposition, can be created directly in the mold layer, or can be placed in the mold layer after external printing. Multiple pattern objects can be embedded in each layer. The mold layer can be formed in a frame, which helps to improve the rigidity of the mold layer, especially when it is necessary to transfer the mold layer (also referred to as a sand box layer in this article). The mold layer can be created on a previous mold layer in the casting area, or it can be created on a separate build table. The mold layer can be made using casting sand with an adhesive, which is well known in the art.

[0140] The patterned article area can serve as support between the components of the molded area to prevent the loss of rigidity that might otherwise be caused by pattern holes in the molded layer. In some cases, especially for sufficiently rigid structures with small patterned areas, the embedded patterned area may be free of material.

[0141] A first mold layer may be formed or placed in a casting position; an optional pattern article removal step may be performed to create a casting pattern; and the mold may then be filled by pouring a layer of molten metal. A second mold layer may be formed ex situ or in situ, or placed on top of a previously metal filled mold layer; an optional pattern article removal step may then be performed to create a casting pattern; and the mold may then be filled with a second layer of molten metal. Additional cycles of mold layers and casting layers may also be performed. Reference Figure 2A , which depicts a mold layer with a patterned object therein (a) and the mold layer after the patterned object is removed (b).

[0142] In one embodiment, the mold layer can be fabricated in situ on the same build table used to fabricate the casting layer. An advantage of this embodiment is that there is no need to transfer the mold layer; therefore, mechanical constraints on the rigidity of the mold layer may be lower than if the mold layer were prepared in a separate location. In addition, in situ construction can accommodate defects in previous layers (e.g., excess / missing material).

[0143] In another embodiment, the mold layer can be produced ex situ, i.e., produced at a location separate from the location used for casting, moved to a casting build table, and placed in an appropriate place, such as on top of a previous mold layer. The advantage of the embedded pattern article layer present in the mold layer is that it provides additional rigidity to achieve the transfer of the mold layer. Another advantage of the present invention is that the temperature of the ex situ mold layer is significantly lower. In order to ensure sufficient accuracy of the alignment of the new mold layer relative to its previous mold layer, the new mold layer can be preheated before it is placed on the previous mold layer to minimize the differential expansion effects related to the temperature difference between the mold layers.

[0144] In one embodiment, the first layer, i.e., the bottom mold layer, can be a complete layer without the embedded pattern article area. The complete first mold layer can serve as a bottom cover for subsequent mold layers. The bottom mold layer can be formed without the use of an adhesive material, with a top surface containing an adhesive material, or with a material that completely contains an adhesive.

[0145] In one embodiment, the first layer, i.e., the bottom mold layer, can be filled to a partial height with sand before placing or forming the embedded patterned article area. The partially filled first mold layer can serve as a bottom covering for subsequent mold layers. The bottom mold layer can be formed without a binder material, with a binder material on the top surface, or completely with a binder material.

[0146] In one embodiment, when forming the mold layer, both the mold area and the patterned article area are made of sand, whereby the mold layer is completely filled with sand. The mold area can be formed by selectively placing sand coated with an adhesive in the mold area, or by selectively coating the sand in the mold area with an adhesive, or by the additive deposition of sand. The embedded patterned article area can be formed by compacted sand or sand coated with an adhesive, or selectively using adhesive coated sand to form the embedded patterned article area, wherein the adhesive material in the patterned article area has different properties from the adhesive material in the mold area. The sand coated with an adhesive can be hardened by heating, activated air flow or other means. The adhesive material can be composed of the following hardening materials, including: various types of clay, various types of silicates, various types of resins, various types of oils or other hardening materials. The patterned article can be created by the additive deposition of sand, can be created directly in the mold layer, or can be placed in the mold layer after external printing. The embedded patterned article area can be formed in the mold layer before the mold area is formed by sand molding or while the mold area is formed by sand molding.

[0147] Another advantage of forming a mold layer with embedded patterned articles (one or more) in the casting area is that it can create molded patterns that would not be transferable without the embedded pattern. Figure 2B , which depicts a mold layer with a patterned article (a) and the mold layer after the patterned article has been removed (b). As depicted, for example, a mold layer with a pattern consisting of concentric rings to be cast by metal cannot be transferred as a whole piece if the mold layer is formed without retaining the embedded pattern. Without the embedded pattern, multiple mold parts would need to be transferred and accurately placed in the casting area. Retaining the embedded patterned article enables the mold layer to be transferred as a continuous part.

[0148] In some embodiments, the removed patterned article may be suitable for additional casting cycles and thus may be transferred to a mold preparation location for reuse. In some embodiments, the cycle of removal and transfer to a mold preparation location may be automated by appropriate means.

[0149] exist Figure 2CIn one embodiment shown, the embedded patterned article area 210 in the mold layer 200, which is intended to be used to manufacture a circular metal shape, can be selectively coated with an adhesive. For example, when forming the mold layer 200, both the mold area 205 and the patterned area 210 are made of sand, whereby the mold layer 200 is completely filled with sand. The patterned area 210 can be formed by selectively placing sand coated with an adhesive in the mold area or selectively coating the sand in the mold area with an adhesive. The applied patterned area 250 plays a supporting role between the components of the mold area 205 to achieve sufficient rigidity for the mold layer 200 to be transferred from the mold layer manufacturing area. In some cases, particularly for structures with sufficient rigidity, the embedded patterned area can be partially free of material.

[0150] When loose sand (i.e., the portion of sand that does not form mold region 205 and pattern region 260) is removed, cavity 260 is created. Regions 250 and 260 together form the region of the circular object to be deposited. When molten metal is deposited into regions 250 and 260, it becomes easier to subsequently remove the patterned object by decomposition.

[0151] According to another embodiment, the embedded pattern area can be formed of compacted sand or formed of binder-coated sand, or by selectively using binder-coated sand to form the embedded pattern area, wherein the binder material in the pattern area (e.g., area 210 shown in FIG. 2) has different properties from the binder material in the mold area (e.g., area 205 shown in FIG. 2). For example, the binder-coated sand in area 205 can be cured by heat or activated air flow or other means, while the material in area 210 is decomposed.

[0152] In one embodiment, the binder of the embedded patterned article may be broken down and then the sand removed from the patterned area to create the casting pattern. In another embodiment, the embedded patterned article may be made of compacted sand, which may be mechanically extracted or broken / broken down by grinding, vibration, airflow, or other mechanical means prior to sand removal, wherein the sand in the mold area is resistant to mechanical means. The sand may be removed by performing vacuum suction. After removing the embedded patterned article, the mold layer may also undergo other process steps prior to casting the molten metal to increase the strength of the mold layer.

[0153] In one embodiment, the mold layer may be a completely uniform sand mold and the mold openings may be made by removing sand from the mold layer in the form of an object, such as by grinding, without the use of a patterned object.

[0154] The binder material in the embedded pattern area can be decomposed by heating the sand mold as a whole, locally heating the sand in the embedded pattern area, locally illuminating the sand in the embedded pattern area, by the flow of decomposing gas or liquid, or other methods. During and after decomposition, the sand in the embedded pattern area can be removed by vacuum suction or by a combination of compressed gas flow and vacuum suction.

[0155] In one embodiment, the sand in the embedded pattern area is decomposed above a certain temperature, which is lower than the decomposition temperature of the binder material in the mold area. The local pattern object removal module can utilize a heating unit to heat the sand in the pattern area, for example, using a pipe for supplying heated gas or using an illuminated heating unit. The local pattern object removal module may include a vacuum suction unit that operates in the embedded pattern area and extracts the decomposed sand and other residues from the exposed surfaces of the previous mold layer and the casting layer. The heating unit and the vacuum suction unit can work simultaneously to gradually remove the sand layer by layer (the removed layer may be different from the mold layer and is typically significantly thinner than the mold layer). The local pattern object removal module can repeatedly scan the embedded pattern area in various motion modes, including a grid mode, a contour following mode, or other options.

[0156] In one embodiment, the sand in the embedded pattern area may be decomposed when exposed to illumination of a specific wavelength and / or intensity, while the binder material of the sand in the mold area is less sensitive to illumination. The local pattern object removal module may include a lighting unit instead of a heating unit, and the lighting unit may work together with a vacuum suction unit. The lighting unit and the vacuum suction unit may work simultaneously to gradually remove the sand layer by layer (the removed layer may be different from the mold layer and is typically significantly thinner than the mold layer). The local pattern object removal module may repeatedly scan the embedded pattern area in various motion modes, including a grid mode, a contour following mode, or other options. The illumination light source may be a laser, an illumination array (lamp, LED), or other.

[0157] The decomposition step may be performed under local underpressure / negative pressure conditions to accelerate the vertical flow of fumes that may be emitted from the embedded pattern area, thereby minimizing possible contamination of the underlying metal surface. The decomposition step may be performed in the presence of a gas that is susceptible to reacting with gases that may be emitted from the embedded pattern area, thereby minimizing possible contamination of the underlying metal surface. After removing the sacrificial material (e.g., sand) in the embedded pattern area and creating the casting pattern, molten metal may be poured into the casting pattern. The next mold layer may then be placed on top of the previous mold layer, and the above process repeated. After the casting of all layers is completed, the stacked mold layers with at least one cast part are placed in a demolding station, the sand is removed, and the at least one part is retrieved.

[0158] Now refer to Figure 3 , Figure 3A , Figure 3B , Figure 3C Depicted is layer-by-layer metal additive casting using a sand mold layer with sand-based embedded areas. Figure 3 Schematic illustration of metal additive casting using sand mold layers with sand-based embedded areas and ex situ mold layers to build a structure according to an embodiment of the present invention. Figure 3 In the embodiment shown in , metal additive casting may include the following steps for each layer (310-340): (a) a sand-based embedded pattern (net-shaped shading) (e.g., 322) may be formed in a frame (sand box layer) (black, solid) (respectively 310f-340f) on a build table (possibly except for the first layer) surrounded by casting sand (dotted lines); (b) a newly prepared mold layer may be transferred to the casting area and placed on top of the previously cast mold layer; (c) the sand-based pattern may be removed (e.g., 322A), and (d) metal (grey, solid) is cast to fill the embedded pattern (e.g., 322B). The above process may be repeated as many layers as desired.

[0159] Now refer to Figure 3A Depicted is the layer-by-layer molding and casting of three separate layers and a bottom layer using metal additive casting using a sand mold with sand-based embedded areas and an in-situ mold layer building structure according to an embodiment of the present invention. Figure 3A In the embodiment shown in , metal additive casting may include the following steps for each layer: (a) using a casting layer frame (black, solid) with one or more embedded sand-based patterns (net shading), wherein the one or more embedded sand-based patterns are embedded in a sand-based casting mold (dotted line) formed in a frame (sand box layer) (black, solid) in the casting area (possibly except for the first layer); (b) the sand-based pattern (one or more) (white, solid) may be removed, (c) metal (gray, solid) is cast to fill the embedded pattern (one or more). The above process may be repeated as many layers as required.

[0160] Now refer to Figure 3B According to an embodiment of the present invention, for example Figure 3Flowchart of the additive casting process 3000 shown. The additive casting process 3000 is performed partially in the mold preparation site 3000A and partially in the casting site 3000B. The additive casting process 3000 can be started in the mold preparation site 3000A by placing the mold layer frame on the mold layer building table (step 3010). If the mold layer is the first layer (step 3020, layer number = 1), the frame can be filled with sand by casting (step 3012), then transferred to the casting site (step 3014), and placed in the casting position in the casting building table (step 3016). If the process involves any other mold layer (as determined in step 3020), after its frame is placed on the building table (3010), the step of forming / placing the pattern object (one or more) can be performed, by filling the area around the formed / placed pattern object by hardening sand (step 3030), and transferring the prepared mold layer to the casting site (step 3040). At the casting site, the mold layer may be placed in place, for example, on top of a previous mold layer on a casting build table (step 3050), and the embedded pattern item may be removed (step 3060); molten metal is then poured into the one or more cavities created by the mold layer (step 3070). At the mold preparation site 3000A, steps 3030-3040 may be repeated for each successive mold layer, and at the casting site 3000B, steps 3050-3070 may be repeated for each such successive mold layer, respectively.

[0161] Now refer to Figure 3C According to an embodiment of the present invention, for example Figure 3A Flowchart of the additive casting process 3000' shown. The additive casting process 3000' can be performed entirely at the casting site. The process 3000' can start by placing a mold layer frame in the casting area (step 3500). If the mold layer is the first layer (step 3510, layer number = 1), the frame can be filled with sand by casting (step 3512). If the process involves any other mold layer (as determined in step 3510), the pattern item (one or more) formation / placement steps can be performed, and the area around the placed pattern items can be filled with hardened sand (step 3520); the embedded pattern can be removed from the mold layer (step 3530), and then the molten metal is poured into the mold layer (step 3540).

[0162] In one embodiment, a mold layer is formed wherein the mold region is made of sand and the embedded pattern region is made of a sacrificial / disposable material. The mold region may be formed by selectively placing sand coated with a binder, or by selectively coating the sand in the mold region with a binder, or by compacting the sand. The embedded pattern region may be formed of polystyrene or other organic or other inorganic material that decomposes at high temperatures or when in contact with molten metal.

[0163] Now refer to Figure 4 Depicted is the layer-by-layer shaping and casting of three separate layers and a bottom layer using metal additive casting using a sand mold with a sacrificial embedded area and an ex-situ mold layer assembly structure. For each layer, the metal additive casting may include the following steps: (a) a sacrificial embedded pattern (diagonal line, shaded) may be placed or formed in a layer frame (sand box layer) (black, solid) on a build table (possibly with the exception of the first layer); (b) the vacancies in the mold layer frame are filled with sand (dotted line) by casting; (c) a newly prepared mold layer is transferred to the casting area and placed on top of the previously cast mold layer; and (d) molten metal (grey, solid) is cast by pouring to decompose and replace the embedded pattern. The process can be repeated as many layers as desired. According to an embodiment of the present invention, this example shows solid features (layer 1), horizontal channels (layer 2), vertical axes (layer 3, black line, dashed line), and sub-layer features and undercuts (layer 3).

[0164] Now refer to Figure 4A Depicts the layer-by-layer shaping and casting of three separate layers and a bottom layer using metal additive casting using a sand mold with a sacrificial embedded area and an in-situ mold layer building structure according to an embodiment of the present invention. Metal additive casting may include the following steps for each layer: (a) a sacrificial embedded pattern (diagonal line, shaded) is placed or formed in a layer frame (sand box layer) (black, solid) on a casting build table (not shown) in the casting area (possibly except for the first layer); (b) the vacancies in the layer frame are filled with sand (dotted line) by casting; (c) molten metal (grey, solid) is cast by pouring to decompose and replace the embedded pattern. The process can be repeated as many layers as desired. This example shows solid features (layer 1), horizontal channels (layer 2), vertical axes (layer 3, black lines, dashed lines), and sub-layer features and undercuts (layer 3).

[0165] Now refer to Figure 4B According to an embodiment of the present invention, Figure 4Flow chart of an additive casting process 4000, for example, performed by the embodiment. The additive casting process 4000 is performed partially in a mold preparation site 4000A and partially in a casting site 4000B. The additive casting process 4000 can be started in the mold preparation site 4000A by placing a mold layer frame on a mold building table (step 4010). If the mold layer is the first layer (step 4020, layer = 1), the layer frame can be filled with casting sand (step 4012), then transferred to the casting site (step 4014), and placed in a casting position in the casting site (step 4016). If the process involves any other mold layers (as determined in step 4020), after the corresponding layer frame is placed on the mold building table (4010), the step of placing or forming the pattern objects can be performed (step 4030), the area around the placed pattern objects (one or more) can be filled with hardened sand (step 4040), and the prepared mold layer can be transferred to the casting site (step 4050). At the casting site, the mold layer can be placed on the previous mold layer on the casting building table (step 4060), and the embedded pattern objects can be removed (step 4070), and then molten metal is poured into the mold layer (step 4080). Steps 4070 and 4080 can be performed simultaneously, whereby pouring molten metal onto the embedded pattern causes the pattern to decompose or evaporate. At the mold preparation site 4000A, steps 4030-4050 may be repeated for each successive mold layer, and at the casting site 4000B, steps 4060-4080 may be repeated for each such successive mold layer, respectively.

[0166] Now refer to Figure 4C According to an embodiment of the present invention, Figure 4A A flow chart of, for example, an additive casting process 4000' performed by the embodiment. The additive casting process 4000' can be performed entirely at the casting site. The additive casting process 4000' can be started by placing a mold layer frame on a casting build table (not shown) in the casting area (step 4500). If the mold layer is the first layer (step 4510, layer = 1), the layer frame can be filled with sand by casting (step 4512). If the process involves any other mold layer (as determined in step 4510), a step of placing or forming a pattern item (one or more) can be performed (step 4520), the area around the placed pattern item can be filled with hardened sand (step 4530), and then molten metal is poured into the mold layer (step 4540), whereby the molten metal decomposes or evaporates the embedded pattern.

[0167] In one embodiment, the component consisting of the embedded pattern area can be placed or formed in one or more positions by the pattern object placement unit within the required placement accuracy. For example, the placement accuracy can be 0.5 mm or less. The surrounding mold area in the mold layer is then filled with sand, which optionally contains a binder material and is treated by compaction or the flow of heat or activated gas to make it hard, thereby making the mold layer completely filled with material.

[0168] In one embodiment, the embedded pattern article material is covered with a coating that can withstand high temperatures and maintain the surface quality of the embedded pattern article, thereby providing a smoother surface finish than a sand casting mold. In a specific embodiment, the embedded pattern article is coated by investment casting a slurry before the sand casting mold is formed.

[0169] The formation of the sand mold layer can be carried out in situ on the top of the previously cast sand mold layer, or it can be carried out in ex situ, being located in a separate location. In the case of ex situ mold production, the sand mold layer is transferred and placed on the previous layer. In the case of in situ mold production, the next mold layer is produced on the top of the existing mold layer. Once the current mold layer is in place, molten metal is poured into the embedded pattern area, and the embedded pattern item decomposes and evaporates. Then place the next mold layer on the top of the previous mold layer (if it is ex situ production) or form the next mold layer on the top of the previous mold layer (if it is in situ production), and repeat the above process. After completing the casting of all layers, the stacked mold layer with at least one cast part is placed in a demoulding station, the sand is removed, and at least one part is retrieved.

[0170] In one embodiment, a binder material is applied to at least a portion of the bottom of the mold layer prior to placement on the previous mold layer. The binder layer may be applied during initial placement of the sand in the mold area of ​​the mold layer, or the binder material may be applied to the exterior of the bottom of the mold layer prior to placement in the casting area.

[0171] The height that the mold material is formed can be greater than the height of the mold layer frame. Excess height can protrude above and / or below the layer frame. After the mold layer is placed on the previous mold layer, pressure can be applied to the top surface of the mold layer to promote compaction and merging of the interlayer interface. Excess height can be in the range of 0.1mm to 1mm. Pressure can be applied by a plate placed on the top of the mold layer.

[0172] In one embodiment, a clamp may be applied to the layer frame to hold the layer frame in place during the molten metal casting process.

[0173] The mold layer may be formed with grooves and protrusions on the top and bottom surfaces to serve as connection and alignment means between the layers. The formation of the grooves and protrusions allows alignment between successive mold layers and prevents horizontal movement between the mold layers. The placement of the mold layer on the casting area can be aligned differently as required for parts of different shapes. Multiple sets of features can be positioned on the surface of the casting area to enable the first mold layer to be attached at various locations depending on the size and layout of the embedded patterned article within the mold frame.

[0174] In one embodiment, grooves and protrusions may be located in a layer frame around a mold layer (flask layer). The grooves and protrusions provided in the frame part of the mold layer create a connection to serve as an alignment element between the building table and the mold frame and between consecutive mold layers.

[0175] Now refer to Figure 5 Described is the accurate placement and alignment between mold layers and mold layers using grooves and protrusions according to an embodiment of the present invention. Three mold layers 510, 520 and 530 show the use of protrusions and grooves. Grooves 510A and protrusions 510B can be prepared at the bottom and top of mold layer 510, respectively. Similarly, grooves and protrusions can also be prepared at the bottom and top of mold layers 520 and 530, respectively, so that the grooves of one mold layer match the size and position of the corresponding protrusions of its previous mold layer. View (a) shows each mold layer 510-530 during its manufacture, respectively. View (b) depicts that after the metal deposition step of layer 510, mold layer 520 is placed on top of mold layer 510. View (c) depicts that after the continuous metal deposition step of layer 520, mold layer 530 is placed on top of mold layer 520.

[0176] Now refer to Figure 5A A device 5000 for forming protrusions and / or grooves at the bottom of a mold layer according to an embodiment of the present invention is schematically depicted. The device 5000 may include a plurality of movable pins 5110-5160, which are arranged in a plate (also referred to herein as a workbench) 5010 so that each pin 5110-5160 can be moved upward from the upper side of the plate 5010 to form a protrusion, or moved downward from the upper side of the plate 5010 to form a groove. A combination of grooves and protrusions can be formed by a combination of plates. The pins and holes can be circular, elliptical, or other possible shapes. In Figure 5AIn the example of , pins 5110 and 5160 are moved to form a protrusion relative to plate 5010, and pins 5120 and 5150 are moved to form a groove at the top of plate 5010. When plate 5010 is placed at the bottom of mold layer 5100, pins 5110 and 5160 form a groove in the mold layer, and pins 5120 and 5150 form a protrusion in the mold layer. Figure 5A In the example of , the grooves and protrusions are formed only in the sand portion 5100A of the mold layer 5100, while the area of ​​the plate 5010 facing the bottom of the mold part 5100B remains flat. The grooves can be formed on the top of the mold layer by creating an area without adhesive material, which is then removed by suction or similar means. The protrusions can be formed on the top of the mold layer by forming hard sand. In some embodiments, the movement of the pins 5110-5160 (which pin will move in which direction and the degree of movement) can be controlled by a controller, which can be adapted to provide movement control signals to corresponding actuators (not shown).

[0177] In one embodiment, the pins of device 5000 are used to form protrusions on the bottom of the mold layer and grooves can be formed on the top of the mold layer by creating areas without adhesive material, which are then removed by suction or similar means.

[0178] In another embodiment, the connection between the mold layers may consist of hard sand parts in the mold area. In addition or alternatively, the connection between the mold layers may also be a complementary part that is inserted into a groove in the first mold layer and bonded thereto, so that when the second mold layer is connected to the first mold layer, the additional part is assembled into a matching groove in the second mold layer and bonded thereto. The connection in the frame and the connection in the sand-filled area can be used in combination. The position of the connection can vary from layer to layer depending on the shape of the embedded parts in each layer.

[0179] In one embodiment, the inserted complementary part may comprise a binder material which forms a rigid bond between successive mould layers. Such a material may be sand mixed with a bonding material and / or a binder material.

[0180] In one embodiment, grooves may be formed on the top and / or bottom surfaces by creating areas where no binder material is added to the sand, whereby loose sand may be removed to create the cavities that form the grooves.

[0181] In one embodiment, groove is formed at the bottom of the mold layer, and projection is formed on the top of the mold layer. Groove can be formed by creating an area without adhesive material in the bottom of the mold area, and when the mold layer is lifted from the build platform, the area without adhesive material is easy to decompose. The position and shape of the groove are aligned with the projection on the top of the previous mold layer. The projection on the top of the mold layer is formed in the mold area in a manner that the position and shape of the projection are aligned with the groove in the subsequent mold layer. In a specific embodiment, the inner surface of the groove can include such material, and when the material contacts the projection of the previous layer, bonding can be produced.

[0182] The bottom surface of the mold layer may be formed with sunken grooves so that a mechanical robot end effector with a fork arm can be inserted into the sunken grooves to lift the mold layer from a flat surface and place it on a flat surface, for example, by a suitable forklift-like device. The sunken grooves can be created in the areas between the casting intervals in the mold layer. In one embodiment, the sunken grooves can be formed on the bottom surface by creating areas where no binder material is added to the sand, thereby removing loose sand to create the desired chambers. The position of the sunken grooves can vary depending on the shape of the embedded patterned article of the mold layer, and therefore, the relative end effector position of transferring the mold layer from the mold layer preparation site to the casting site can also vary accordingly.

[0183] In one embodiment, the recessed groove is tapered and is used in conjunction with the tapering of the end effector with the fork arm to enable insertion into the groove with minimal friction between the fork arm and the groove, so that contact occurs substantially only when the robotic end effector reaches its fully inserted position.

[0184] In one embodiment, the sunken groove is formed by placing a hollow rod on the building table before filling with sand. After filling the mold layer, the end effector with a fork arm is inserted into the hollow rod, and the mold layer is transferred to the casting area by lifting the mold layer with the hollow rod. In another embodiment, the hollow rod is tapered on the outside in the horizontal direction. In addition, the inner cavity of the hollow rod can also be tapered in the horizontal direction. When the mold layer is placed on the casting area, the end effector with a fork arm can be easily removed from the mold layer while extracting the hollow rod.

[0185] Now refer to Fig. 6A and Figure 6B The present invention shows that grooves for transferring the mold layer are formed in different positions at the bottom of the mold layer. The grooves according to the embodiment of the present invention can be formed by removable sand, by Figure 5A The lifting rod in the device 5000 shown in FIG. 5 is formed by the placement of a hollow rod, or by the pre-placement of an end effector with a fork arm. Fig. 6AIt is shown that grooves 602A-606A for transferring mold layers 602-606A are respectively made in the same position at the bottom of all mold layers. Figure 6B The figure shows that grooves 652A-656A for transferring mold layers 652-656 are respectively made at different positions at the bottom of the mold layer. Fig. 6A and Figure 6B In the drawings, the casting stages are labeled as (a)—forming a casting layer, (b)—placing a casting layer on top of its previous casting layer, and (c)—casting (removing the pattern item(s) and pouring the molten metal).

[0186] In order to perform the casting and molding methods described herein, a system can be formed. Figure 7 , which schematically describes an additive casting system 7000 for preparing a mold layer in a mold preparation site, transferring the mold layer to a casting site, and casting an article according to an embodiment of the present invention. Figure 7 An additive casting system 7000 is described, which includes a molding subsystem 7000A and a casting subsystem 7000B, which can be remotely located from each other. It will be apparent to one skilled in the art that the molding subsystem 7000A and the casting subsystem 7000B can be used to perform molding and casting at a single location, but modifications are apparent.

[0187] The molding subsystem 7000A may include a sand mold supply unit 7002, which is suitable for supplying sand to the mold layer 7104 in a controllable manner during the mold layer preparation stage. The molding subsystem 7000A may also include a unit 7004 for supplying pattern items (one or more) to the prepared mold layer. The mold layer in preparation can be placed on the mold building table 7102. When the mold layer 7104 is prepared, the mold layer 7104 can be transferred to the casting subsystem 7000B by the mold layer transfer unit 7008. In some embodiments, some or all of the units of the molding subsystem 7000A may be controlled and timed by a controller 7006. The controller 7006 may include any suitable controller, a programmable logic controller (PLC), or any other computing unit suitable for executing a controller readable program code. The program code may be stored on a non-transient computer readable storage unit (not shown) known in the art.

[0188] The casting subsystem 7000B may include a pattern article removal unit 7010 and a molten metal deposition unit 7012. The placement of the mold layer in the casting position (e.g., accurately positioned on top of the previous mold layer on the casting build table 7106) may be accomplished by the transfer and placement unit 7008'. Once the placement of the mold layer is completed (or after completing optional preparation steps, not shown), the molten metal deposition unit 7012 pours molten metal into one or more cavities created in the mold layer 7104.

[0189] The operation and timing of the patterned article removal unit 7010, the molten metal deposition unit 7012, and the transfer and placement unit 7008' may be accomplished by a controller 7006'. The controller 7006' may include any suitable controller, a programmable logic controller (PLC), or any other computing unit suitable for executing a controller-readable program code. The program code may be stored on a non-transitory computer-readable storage unit (not shown) known in the art.

[0190] In some embodiments, the mold layer transfer unit 7008 and the transfer and placement unit 7008' may be a single unit, particularly depending on the distance between the two locations. In some embodiments, the controller 7006 and the controller 7006' may be a single controller, particularly depending on the distance between the two locations.

[0191] According to the embodiments of the present invention, different methods can be used to prepare the mold layer. Figure 8 , which schematically shows three different mold layer preparation systems 8000, 8100 and 8200 according to embodiments of the present invention. The mold layer preparation system 8000 may include a mold sand and binder supply unit 8004 and a pattern item sand and binder supply unit 8020 disposed above a mold layer frame 8002, adapted to provide sand and binder materials for preparing pattern items (one or more) (unit 8020), and fill the remaining mold layer frame with sand and binder materials to form a mold (unit 8004). The operations of the pattern item sand and binder supply unit 8020 and the mold sand and binder supply unit 8004 may be controlled by a controller 8010.

[0192] The mold layer preparation system 8100 may include a mold binder supply unit 8104, a sand supply unit 8106, and a pattern binder supply unit 8120. The controller 8110 may control the operations of the mold binder supply unit 8104, the sand supply unit 8106, and the pattern binder supply unit 8120 to provide a suitable mixture for the pattern article(s) and a suitable mixture for the mold at a desired location.

[0193] The mold layer preparation system 8200 may include a pattern item placement or formation unit 8208, a mold binder supply unit 8204, and a sand supply unit 8206. The controller 8210 may control and coordinate the operations of the pattern item placement or formation unit 8208, the mold binder supply unit 8204, and the sand supply unit 8206 to first place the item(s) in a desired position in the mold frame 8202, then prepare the casting mixture, and fill the remaining mold frame with a mixture of sand and binder.

[0194] A method for forming a mold for additively casting a metal article may be provided. The method may include additively producing a plurality of production layers, one currently produced production layer following another; wherein, for each currently produced production layer: (i) forming one or more mold layers comprising at least one removable pattern; (ii) replacing the at least one removable casting pattern with one or more layers of molten metal.

[0195] A method for forming a mold for additively casting a metal article may be provided. The method may include: (i) preparing a mold layer including at least one removable pattern embedded in the mold layer; (ii) positioning the mold layer at a casting location; (iii) casting molten metal into at least one casting pattern article, removing at least one embedded removable casting pattern in the mold layer and replacing it with molten metal; (iv) repeating steps (i)-(iii) with at least one additional mold layer, wherein at least one additional mold layer may be placed on top of a previous mold layer.

[0196] The at least one casting mold layer may be formed by sand molding.

[0197] At least one casting pattern may be formed by embedding a pattern item in the casting layer before or simultaneously with forming the casting layer by sand molding.

[0198] At least one patterned article may be made of at least one of the following materials: loose sand within a hardened sand mold layer that is removable by one or more of milling, vibration, air flow, suction or other mechanical means; compacted sand that is mechanically removable by one or more of milling, vibration, air flow, suction or other mechanical means; binder-hardened sand that is removable by one or more of heating, milling, vibration, air flow, suction or other mechanical means; and disposable material configured to evaporate when molten metal is cast.

[0199] Before casting the casting material, at least one pattern item may be removed from the casting mold layer.

[0200] At least one pattern item can be removed from the mold layer by at least one of the following pattern removal means: heating, grinding, vibration, air flow, suction or other mechanical means.

[0201] During casting of the casting material, at least one pattern item may be removed from the casting mold layer.

[0202] The casting layer is prepared by filling the casting layer frame with sand and hardening the sand by means of a hardening material.

[0203] The hardening material may be selected from various types of clays, various types of silicates, various types of resin types, and various types of oils.

[0204] Before the casting layer frame is filled with sand, at least one casting pattern object is positioned in a corresponding position of the pattern objects in the casting layer frame.

[0205] The positioning of at least one additional moulding layer on top of a previous moulding layer may be done using alignment means comprising grooves and or protrusions.

[0206] Although some features of the present invention have been illustrated and described herein, many modifications, substitutions, changes and equivalents will now occur to those skilled in the art. Therefore, it should be understood that the appended claims are intended to cover all such modifications and changes that fall within the true spirit of the present invention.

Claims

1. A casting system for casting an article, wherein: The casting system includes: Moulding system; Alternative material supply systems; Molten metal processing systems; wherein the casting system is configured to additively produce a plurality of production layers, one currently produced production layer following another; Where, for each currently produced production layer: The mold system is configured to form one or more mold layers; The replaceable material providing system is configured to provide one or more replaceable material layers; and The molten metal processing system is configured to replace the one or more replaceable material layers by providing molten metal to form one or more current article regions of the production layer currently being produced.

2. The casting system according to claim 1, comprising: A replaceable material removal system is configured to remove at least one of the one or more replaceable material layers before at least one of the one or more molten metal layers that forms the one or more current article regions is formed.

3. The casting system according to claim 2, wherein: The replaceable material removal system comprises a suction unit for removing the at least one replaceable material layer.

4. The casting system according to claim 2, wherein: The replaceable material removal system comprises a mechanical removal unit for removing the at least one replaceable material layer.

5. The casting system according to claim 2, wherein: The replaceable material removal system comprises a temperature-based removal unit for removing the at least one replaceable material layer.

6. The casting system according to claim 2, wherein: The replaceable material removal system comprises a chemical-based removal unit for removing the at least one replaceable material layer.

7. The casting system according to claim 1, wherein: The one or more layers of replaceable material are decomposable in the presence of molten metal.

8. The casting system according to claim 1, wherein: The replaceable material providing system is configured to generate the one or more replaceable material layers.

9. The casting system according to claim 1, wherein: The replaceable material supply system is configured to receive the one or more replaceable material layers and position the one or more replaceable material layers in a casting position.

10. The casting system according to claim 1, wherein: The casting mold system is configured to form the one or more casting mold layers by sand molding.

11. The casting system according to claim 1, wherein: The one or more casting mold layers include sand and one or more binders.

12. The casting system according to claim 1, wherein: The one or more casting mold layers include sand and a binder, wherein at least two binders are different from each other due to their removal process.

13. The casting system according to claim 1, wherein: The mold system includes a mold powder providing system, a mold binder dispensing system and a mold powder removing system.

14. The casting system according to claim 13, wherein: For each currently producing production tier: The mold powder providing system is configured to provide one or more current mold powder layers; The mold binder dispensing system is configured to form one or more current mold regions within each of the one or more current mold powder layers by selectively dispensing particles of one or more binders that bind some of the mold powder particles in the current mold powder layer; as well as The mold powder removal system is configured to remove mold powder particles located within a certain area of ​​each layer of the one or more current mold powder layers, the certain area being defined by at least some of the one or more current mold regions.

15. The casting system according to claim 1, wherein: For each currently produced production layer, the molding system is configured to dispense molding material to form the one or more molding layers.

16. The casting system according to claim 1, wherein: The metal processing system is configured to form the one or more current article regions of the currently produced production layer by depositing molten metal at the cavity created in the mold layer to replace the one or more replaceable material layers and applying at least one of a pre-deposition process and a post-deposition process.

17. The casting system according to claim 16, wherein: Depositing molten metal at the cavity created in the mold layer and applying at least one of a pre-deposition treatment and a post-deposition treatment includes depositing molten metal at the cavity created in the mold layer and applying at least one of a pre-deposition treatment and a post-deposition treatment in a localized manner.

18. The casting system according to claim 16, wherein: Depositing molten metal at a cavity created in a casting layer and applying at least one of a pre-deposition treatment and a post-deposition treatment comprises applying at least two of the following: depositing molten metal at a cavity formed in a casting layer and applying at least one of a pre-deposition treatment and a post-deposition treatment in a spatially distributed manner.

19. The casting system according to claim 1, wherein: The metal processing system is configured to heat the environment in the area of ​​the current article.

20. The casting system according to claim 1, comprising a monitoring unit for monitoring the provision of the one or more replaceable material layers.

21. A casting system according to claim 20, comprising a controller for controlling the provision of the one or more replaceable material layers based on the monitoring.

22. The casting system according to claim 1, wherein: The one or more layers of replaceable material are configured to decompose at a temperature exceeding 590 degrees Celsius.

23. The casting system according to claim 1, wherein: The one or more layers of replaceable material are configured to decompose at a temperature that the molten layer reaches within a maximum of a few minutes from deposition.

24. The casting system of claim 1, comprising a frame system configured to create a frame region defining a frame surrounding one or more mold regions.

25. A method for casting an article, wherein: The method comprises: The casting system produces multiple production layers additively, one currently produced production layer following the next; Where, for each currently produced production layer: One or more mold layers are formed by a mold system of the casting system; providing one or more layers of replaceable material by a replaceable material providing system of the casting system; and One or more current article regions of a production layer currently being produced are formed from molten metal processing of the casting system by providing molten metal that replaces the one or more replaceable material layers.

26. The method according to claim 25, comprising: At least one of the one or more replaceable material layers is removed by the replaceable material removal system of the casting system before at least one of the one or more molten metal layers forming the one or more current article regions is formed.

27. The method according to claim 26, wherein: The removal is performed by a suction unit.

28. The method according to claim 26, wherein: Removal is performed by a mechanical removal unit.

29. The method according to claim 26, wherein: Removal is performed by a temperature-based removal unit.

30. The method of claim 26, wherein: Removal is performed by a chemical-based removal unit.

31. The method of claim 25, wherein: The one or more layers of replaceable material are decomposable in the presence of molten metal.

32. The method of claim 25, comprising generating the one or more replaceable material layers by a replaceable material providing system.

33. The method of claim 25, comprising receiving the one or more layers of replaceable material by a replaceable material supply system and positioning the one or more layers of replaceable material in a casting position.

34. The method of claim 25, comprising forming the one or more mold layers by sand molding with a mold system.

35. The method of claim 25, wherein: The one or more casting mold layers include sand and one or more binders.

36. The method of claim 25, wherein: The one or more casting mold layers include sand and a binder, wherein at least two binders differ from each other in their removal process.

37. The method of claim 25, wherein: For each currently producing production tier: The casting powder supply system of the casting system provides one or more current casting powder layers; forming one or more current mold regions in each of the one or more current mold powder layers by selectively dispensing particles of one or more binders that bind some of the mold powder particles in the current mold powder layer, by a mold binder dispensing system of the mold system; as well as A mold powder removal system of the mold system removes mold powder particles located within a certain area of ​​each layer in the one or more current mold powder layers, wherein the certain area is defined by at least some of the one or more current mold areas.

38. The method of claim 25, wherein: For each currently produced production layer, the molding material is distributed by the molding system to form one or more molding layers.

39. The method of claim 25, comprising: One or more current article regions of a current production layer are formed by the metal processing system by applying preparation and deposition and post (PDP) processing to replace the one or more replaceable material layers.

40. The method of claim 39, wherein: Applying PDP processing includes applying preparation, deposition and post-processing in a localized manner.

41. The method of claim 39, wherein: Applying the PDP process includes applying at least two of preparation, deposition, and post-processing in a spatially distributed manner.

42. The method of claim 25, comprising heating the environment of the current article area by the metal processing system.

43. The method of claim 25, comprising monitoring the provision of the one or more replaceable material layers by a monitoring unit.

44. The method of claim 43, comprising controlling, by a controller, the provision of the one or more replaceable material layers based on monitoring.

45. The method of claim 25, wherein: The one or more layers of replaceable material are configured to decompose at a temperature exceeding 590 degrees Celsius.

46. ​​The method of claim 25, wherein: The one or more layers of replaceable material are configured to decompose at a temperature that the molten layer reaches within a maximum of a few minutes from deposition.

47. The method of claim 25, comprising generating a frame region from a frame system of a gating system, the frame region defining a frame surrounding one or more mold regions.

48. A non-transitory computer readable medium for casting an article, wherein: The non-transitory computer readable medium stores instructions for: The casting system produces multiple production layers additively, one currently produced production layer following the next; Where, for each currently produced production layer: One or more mold layers are formed by a mold system of the casting system; providing one or more layers of replaceable material by a replaceable material providing system of the casting system; and One or more current article regions of a production layer currently being produced are formed from molten metal processing of the casting system by providing molten metal that replaces the one or more replaceable material layers.

Citation Information

Patent Citations

  • High-resolution rapid manufacturing

    CN101449295A

  • Method and system for direct casting of cast components by additive manufacturing of composite monolithic molds

    CN107848020A