A method for preparing graphene / copper composite powder and composite material using microwave

Through microwave processing method, combined with organic coating and microwave power control, the problem of high energy consumption and complicated operation of high-temperature heat treatment in the preparation of graphene/copper composite materials has been solved, and high-quality graphene/copper composite powder and excellent performance have been obtained. Composite materials enable low-cost mass preparation and environmentally friendly production.

CN117604302BActive Publication Date: 2024-10-18HARBIN INST OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311536173.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-17
Publication Date
2024-10-18
Estimated Expiration
2043-11-17

AI Technical Summary

Technical Problem

Among the existing graphene/copper composite material preparation methods, high-temperature heat treatment equipment consumes high energy and is complex to operate, which affects the mechanical properties of the material, and the powder metallurgy method can easily destroy the graphene structure and reduce the strengthening effect.

Method used

Microwave processing is used to mix copper powder with organic molecules to form a coating layer. Microwave power and time are controlled by microwave equipment to optimize the graphene growth process to obtain high-quality graphene/copper composite powder, which is then sintering and deformed. Processed to obtain composite materials with excellent properties.

Benefits of technology

It achieves rapid and low-energy acquisition of high-quality graphene/copper composite powder, simplifies the preparation process, reduces energy consumption and environmental pollution, and provides a low-cost mass preparation solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117604302B_ABST
    Figure CN117604302B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing graphene / copper composite powder and composite materials by using microwaves; it belongs to the field of inorganic synthesis and powder metallurgy technology. The present invention aims to solve the problem that the existing graphene / copper composite powder preparation process needs to go through vacuum heat treatment equipment, which is time-consuming and energy-intensive. The method of the present invention is as follows: copper powder is uniformly wrapped with organic matter, then placed in a quartz container, filled with inert gas, placed in a microwave device, microwave power and microwave time are adjusted, and graphene / copper composite powder is obtained after the powder is cooled, and graphene / copper composite material is obtained after sintering and deformation treatment. The method of the present invention obtains high-quality graphene / copper composite powder and graphene / copper composite material with excellent mechanical and electrical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inorganic synthesis and powder metallurgy; specifically relates to a graphene / copper composite powder using microwaves and a preparation method thereof; a graphene / copper composite material using microwaves and a preparation method thereof. Background Art

[0002] Graphene / copper composite materials are a type of copper-based material with high electrical conductivity, high thermal conductivity, ultra-high strength, and excellent friction resistance. They are expected to be widely used in electronic packaging, new energy power generation, power transmission, automobile and shipbuilding industries. At present, many methods for preparing graphene / copper composite materials have been developed, among which the more commonly used methods are chemical vapor deposition, electrodeposition, powder metallurgy, etc.

[0003] Chemical vapor deposition is a common method for preparing graphene / copper composite materials. By controlling the reaction conditions, copper metal layers and graphene layers are deposited alternately to obtain graphene / copper composite materials (Nat Commun, 2013, 4: 2114). This method can obtain high-quality graphene / copper composite materials with a compressive strength of up to 1.5 GPa, but the preparation process requires strict control of the reaction conditions, and the prepared composite materials are small in size, which is not suitable for low-cost mass production.

[0004] Electrodeposition is another commonly used method for preparing graphene / copper composite materials. The preparation process mainly involves uniformly mixing metal copper salts with carbon sources such as graphene oxide solutions, using electrochemical deposition methods, and obtaining graphene / copper composite powders after heat treatment and reduction, and then sintering to prepare graphene / copper composite materials (Journal Of Alloys And Compounds, 2022, 924). This method can prepare a large number of graphene / copper composite materials, but the preparation process requires both electrochemical deposition and heat treatment and reduction, and the entire preparation process is relatively complicated.

[0005] Powder metallurgy is a method of mixing graphene powder and copper powder by ball milling, etc., first obtaining graphene / copper composite powder, and then densifying it by pressing and sintering to obtain graphene-reinforced copper-based composite materials (RscAdvances, 2015, 5: 51193-51200). Its advantage is that there is basically no restriction on the content, size, shape, etc. of the matrix powder and the reinforcement, and it has high designability. The problem with this method is that the mixing process is easy to destroy the integrity of the graphene structure, reducing the strengthening effect of graphene.

[0006] The in-situ self-generated method for preparing graphene / copper composite materials developed in recent years has the advantages of strong interface bonding and good controllability, and is a promising preparation method. The in-situ growth method is to select a suitable carbon source as a precursor in the preparation stage of the composite powder, and then grow graphene in situ under the catalytic action of the copper surface after high-temperature carbonization treatment, which can significantly improve the interface bonding strength between the graphene reinforcement and the copper matrix (Nat Commun, 2020, 11: 2775). However, there are still problems with the in-situ growth method. The preparation of graphene / copper composite powders requires long-term treatment in high-temperature treatment equipment, which consumes high energy and has a long experimental cycle. It is easy to cause the copper powder grains to grow during the heat treatment process, which seriously affects the mechanical properties of the graphene / copper composite materials prepared subsequently. Summary of the invention

[0007] The present invention proposes a simple method for preparing graphene / copper composite powder and composite material with excellent graphene quality by using microwaves. The present invention uses copper powder and organic molecules as raw materials, and forms a layer of organic molecule coating on the surface of copper powder by mixing copper powder with organic molecules, thereby obtaining organic / copper composite powder, which is conducive to the uniform production of graphene and prevents the copper powder from being oxidized during the microwave process. Then, the coated organic / copper composite powder is placed in a quartz container, filled with inert gas and sealed, and then placed in a microwave device for microwave treatment. During the microwave treatment process, the growth process of graphene is optimized by regulating the microwave power and treatment time, so as to obtain a graphene / copper composite powder with good quality. Subsequently, sintering and deformation treatment are performed to obtain a graphene / copper composite material with excellent performance. The present invention aims to solve the problem that the existing graphene / copper composite powder preparation process needs to go through a vacuum heat treatment furnace equipment, which is time-consuming and energy-intensive. High-quality graphene / copper composite powder can be obtained through common microwave equipment, thereby providing a graphene / copper composite powder raw material for preparing a graphene / copper composite material with excellent performance.

[0008] In order to solve the above technical problems, the present invention provides a method for preparing a graphene / copper composite material using microwaves. The specific preparation method is carried out according to the following operations:

[0009] First, the organic matter is uniformly mixed with copper powder in a certain proportion; then it is placed in a quartz container, filled with inert gas, sealed with a lid, placed in a microwave device, and the microwave power and microwave time are adjusted. After the powder is cooled, a graphene / copper composite powder is obtained. The graphene / copper composite powder can then be sintered, or sintered and deformed to obtain a graphene / copper composite material with excellent performance.

[0010] It is further defined that the organic matter is mainly an organic matter whose elemental composition is carbon and hydrogen; carbon, hydrogen and oxygen; carbon, hydrogen and nitrogen; and it is further defined that the organic matter is a combination of one or more of the macromolecular organic matter represented by polyacrylonitrile and polymethyl methacrylate, and the small molecular organic matter represented by oleic acid and oleylamine in any ratio.

[0011] It is further defined that the mass ratio of the organic matter to the copper powder is 1:(1-1000).

[0012] It is further defined that the particle size of the copper powder is 20 mesh to 15000 mesh.

[0013] It is further defined that the mixing method of the organic / copper composite powder includes ball milling, rotary evaporation, and mechanical stirring.

[0014] It is further defined that the solvent used for rotary evaporation is N,N-dimethylformamide, cyclohexane or anhydrous ethanol.

[0015] It is further defined that the ball-to-material ratio is (10-20):1, the ball mill speed is 100 r / min to 600 r / min, and the ball milling time is 1 h to 10 h.

[0016] It is further defined that the inert gas is one of argon and nitrogen.

[0017] It is further defined that the quartz container includes a quartz boat with a cover, a quartz crucible, a corundum boat, and a corundum crucible.

[0018] It is further defined that the microwave equipment includes a microwave heating machine, a microwave heating box, and a household microwave oven.

[0019] It is further defined that the microwave heating power ranges from 100 watts to 200,000 watts, and the microwave heating time ranges from 1 minute to 30 minutes.

[0020] It is further defined that the sintering is spark plasma sintering, vacuum hot pressing sintering, and vacuum sintering.

[0021] It is further defined that the sintering is carried out at a temperature of 400°C to 1050°C and a pressure of 0 MPa to 200 MPa.

[0022] It is further defined that the deformation process is performed by rolling or extrusion.

[0023] It is further defined that the deformation temperature is controlled at 0-900° C. and the deformation ratio is 0-95%.

[0024] Graphene / copper composite powder and composite material prepared by any of the above methods.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] Compared with the traditional high-temperature furnace heat treatment method, microwave treatment has the advantages of fast reaction speed, large temperature rise and fall speed, and easy control of reaction conditions. In addition, the microwave treatment process does not require a high-temperature furnace, which can reduce energy consumption and environmental pollution, and achieve the purpose of green and environmentally friendly preparation of graphene / copper composite powders.

[0027] The present invention is expected to solve the problems of high energy consumption and complex operation of vacuum or atmosphere heat treatment furnace equipment in the preparation process of common graphene / copper composite powders. The present invention can obtain high-quality graphene / copper composite powders through a common microwave oven, providing a solution for the batch and low-cost preparation of graphene / copper composite materials with excellent performance.

[0028] In order to further understand the features and technical contents of the present invention, please refer to the following detailed description and drawings of the present invention. However, the attached drawings are only provided for reference and illustration and are not intended to limit the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 XRD diagram of graphene / copper composite powders prepared from copper powder raw materials and oleic acid with different mass fractions in Example 1;

[0030] Figure 2 This is the graphene Raman graph of the composite copper powder after microwave treatment and corrosion treatment in Example 1, a——0.2G M / Cu,b——0.5G M / Cu,c——1G M / Cu,d——2G M / Cu;

[0031] Figure 3 is the XPS graph of C1s of graphene in Example 2;

[0032] Figure 4 This is the Raman graph of graphene / copper composite powder prepared with different mass fractions of oleic acid in Comparative Example 1. DETAILED DESCRIPTION

[0033] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0034] Example 1: The method for preparing graphene / copper composite powder using microwaves in this example is carried out according to the following steps:

[0035] The copper powder was uniformly coated with oleic acid by ball milling process. The ball milling process parameters were as follows: ball-to-material ratio was 10:1, ball mill speed was 200r / min, and ball milling time was 1 hour. Oleic acid / copper composite powders containing different mass fractions of oleic acid were prepared. The mass fractions of oleic acid were 0.2wt.%, 0.5wt.%, 1.0wt.%, and 2.0wt.%, respectively, and were named 0.2G M / Cu, 0.5G M / Cu, 1G M / Cu and 2G M / Cu;

[0036] The obtained oleic acid / copper composite powder was then placed in a quartz crucible, filled with argon as a protective gas, and quickly processed in a microwave oven with a microwave power of 800 watts and a microwave time of 2 minutes. Five groups of powders were microwaved using the same process to obtain graphene / copper composite powders prepared with different oleic acid mass fractions.

[0037] The composite powder prepared in this example was tested, and the results were as follows: Figure 1-2 shown.

[0038] Depend on Figure 1 It can be seen that the XRD results of the graphene / copper composite powders prepared in this embodiment containing different mass fractions of oleic acid show that the composite powders and the copper powder raw materials have no oxide peaks, indicating that no oxidation occurs during the microwave treatment.

[0039] Depend on Figure 2 It can be seen that the graphene I prepared in this embodiment D / I G The values ​​are all lower than 1, indicating that the graphene prepared with different mass fractions of oleic acid under the conditions of this example has higher quality.

[0040] Example 2: The method for preparing graphene / copper composite powder using microwaves in this example is carried out according to the following steps:

[0041] The copper powder was uniformly coated with polyacrylonitrile by ball milling process, and the ball milling process parameters were as follows: ball-to-material ratio was 10:1, ball mill speed was 200r / min, and ball milling time was 1 hour, and polyacrylonitrile / copper composite powder containing 0.5wt.% polyacrylonitrile was prepared;

[0042] The obtained polyacrylonitrile / copper composite powder is then placed in a quartz crucible, filled with argon as a protective gas, and placed in a microwave oven for rapid treatment with a microwave power of 800 watts and a microwave time of 2 minutes to obtain a graphene / copper composite powder containing 0.5 wt.% polyacrylonitrile.

[0043] The composite powder prepared in this example was tested, and the results were as follows: Figure 3 shown.

[0044] Depend on Figure 3 It can be seen that the carbon atoms in the graphene in the graphene / copper composite powder prepared in this embodiment mainly exist in the form of SP2 (SP2 content is 73%), which shows that the prepared graphene / copper composite powder has a higher quality.

[0045] Example 3: The method for preparing graphene / copper composite powder using microwaves in this example is carried out according to the following steps:

[0046] The copper powder was uniformly coated with oleic acid by rotary evaporation, the solvent was cyclohexane, and the rotary evaporation temperature was 80 degrees Celsius, and an oleic acid / copper composite powder containing 0.5wt.% oleic acid was prepared;

[0047] The obtained polyacrylonitrile / copper composite powder was then placed in a quartz boat, filled with argon as a protective gas, and placed in a microwave oven for rapid treatment with a microwave power of 800 watts and a microwave time of 2 minutes to obtain a graphene / copper composite powder prepared with 0.5 wt.% oleic acid.

[0048] Example 4: The method for preparing graphene / copper composite powder using microwaves in this example is carried out according to the following steps:

[0049] The copper powder was uniformly coated with oleic acid by rotary evaporation, the solvent was anhydrous ethanol, and the rotary evaporation temperature was 80 degrees Celsius to prepare an oleic acid / copper composite powder containing 0.5wt.% oleic acid;

[0050] The obtained oleic acid / copper composite powder was then placed in a quartz boat, filled with argon as a protective gas, and placed in a household microwave oven for rapid treatment with a microwave power of 500 watts and a microwave time of 5 minutes to obtain a graphene / copper composite powder prepared with 0.5 wt.% oleic acid.

[0051] Example 5: The method for preparing graphene / copper composite powder using microwaves in this example is carried out according to the following steps:

[0052] The copper powder was uniformly coated with polyacrylonitrile by ball milling process, and the ball milling process parameters were as follows: ball-to-material ratio was 10:1, ball mill speed was 300r / min, and ball milling time was 100 hours, and polyacrylonitrile / copper composite powder containing 0.1wt.% polyacrylonitrile was prepared;

[0053] The obtained polyacrylonitrile / copper composite powder is then placed in a quartz crucible, filled with argon as a protective gas, and placed in a household microwave oven for rapid processing with a microwave power of 800 watts and a microwave time of 2 minutes to obtain a graphene / copper composite powder prepared with 0.5 wt.% polyacrylonitrile.

[0054] The preparation method of the graphene / copper composite material in this embodiment is carried out according to the following steps:

[0055] Step 1: subjecting the graphene / copper composite powder prepared by the method of this embodiment to a spark plasma sintering treatment, wherein the sintering process is 700° C. for 5 min and the sintering pressure is 40 MPa;

[0056] Step 2: Extruding the composite material after sintering in step 1, the extrusion process is hot extrusion, the extrusion temperature is 800° C., and the extrusion ratio is 25:1, to obtain a graphene / copper composite material.

[0057] The performance test of the composite material obtained by sintering showed that the tensile yield strength of the composite material was 337 MPa, the tensile strength was 360 MPa, and the electrical conductivity was 93.2% IACS (International Annealed Soft Copper Standard) at 20°C.

[0058] The performance test of the composite material obtained by extrusion was carried out, and the electrical conductivity of the extruded composite material was 99.6% IACS at 20°C.

[0059] Comparative Example 1: The preparation method of the graphene / copper composite powder of the comparative example is carried out according to the following steps;

[0060] The copper powder was uniformly coated with oleic acid by ball milling process. The ball milling process parameters were as follows: ball-to-material ratio was 10:1, ball mill speed was 200 r / min, and ball milling time was 1 hour. Oleic acid / copper composite powder containing 0.2 wt.% of oleic acid was prepared.

[0061] Then the obtained oleic acid / copper composite powder was evenly spread on a clean copper boat, and then the copper boat was placed in a tube furnace and subjected to high temperature carbonization treatment (CVD treatment) in a hydrogen (17 vol.%) and argon (83 vol.%) atmosphere: the heating rate was 10°C / min, and the mixture was heated to 700°C, 800°C, 900°C, and 1000°C, respectively, and kept warm for 2 minutes. The obtained graphene / copper composite powders were recorded as CVD700°C, CVD800°C, CVD900°C, and CVD1000°C, respectively. The composite powders treated with CVD at different temperatures were characterized by Raman and compared, as shown in Figure 2. Figure 4 shown.

[0062] Depend on Figure 4 The Raman spectra of CVD700℃, CVD800℃, CVD900℃, and CVD1000℃ show that

[0063] Prepared graphene / copper composite powder, I D / I G The values ​​of the composite powders were 0.97, 0.98, 1.15 and 1.16 respectively. In comparison, the composite powders 0.2G M I / CuD / I G =0.85, so it can be considered that under this condition, microwave treatment can obtain graphene / copper composite powders with excellent quality than CVD treatment. In the microwave rapid treatment process, the electric field enhancement effect occurs locally, the ionization probability of organic molecules increases, the heating rate is fast, and graphene can be obtained in a short time. Graphene, due to its huge specific surface area and high conductivity, will also absorb waves and accelerate the carbonization of organic matter on other substrate sites. In addition, graphene has many conductivity loss and dielectric loss mechanisms, including dipole polarization at defects, capacitive structure polarization between graphene sheets, conductivity loss caused by electron migration, multiple scattering of electromagnetic waves between sheets, etc. (Journal of Materials Chemistry: C, 2015, 3

[0064] (38); 10017-10022). These are conducive to the efficient heating of organic / copper composite powders and the efficient preparation of graphene / copper composite powders. After recording the experimental cycle, the average time required for preparing graphene / copper composite powders by microwave in-situ growth method is 10 minutes, and the average time required for preparing composite powders by CVD in-situ growth method at 800°C is 150 minutes. It can be seen that microwave treatment also has the advantages of fast heating and high efficiency in promoting in-situ growth. In addition, microwave treatment requires low energy consumption and simple experimental requirements.

Claims

1. A method for preparing graphene / copper composite powder using microwaves, characterized in that: The method is achieved by the following steps: The organic matter and copper powder are uniformly mixed in a certain proportion, placed in a quartz container, introduced with an inert gas, sealed, subjected to microwave treatment, and cooled to room temperature to obtain the graphene / copper composite powder; Among them, the inert gas is argon; The organic matter is one or more of polyacrylonitrile, polymethyl methacrylate, oleic acid, and oleylamine; The mass ratio of organic matter to copper powder is 1: (1-1000); the particle size of the copper powder is 20 meshes-15000 meshes; The microwave equipment is a microwave heating machine, a microwave heating box, or a household microwave oven; the microwave heating power is controlled within a range of 100 watts to 200,000 watts, and the microwave heating time is 1 minute to 30 minutes.

2. The method according to claim 1, characterized in that: Mechanical stirring, ball milling, and rotary evaporation were used for mixing.

3. The method according to claim 2, characterized in that: The solvent used for the rotary evaporation is N, N-dimethylformamide, cyclohexane or anhydrous ethanol; the process parameters of the ball milling are: the ball-to-material ratio is (10-20):1, the ball mill speed is 100r / min~600r / min, and the ball milling time is 1h~10h.

4. A graphene / copper composite powder prepared by the method according to any one of claims 1 to 3.

5. A method for preparing a graphene / copper composite material, characterized in that: The graphene / copper composite material is obtained by sintering the graphene / copper composite powder prepared by the method according to any one of claims 1 to 3, or deforming the powder after sintering.

6. The method according to claim 5, characterized in that: The sintering process includes spark plasma sintering, vacuum hot pressing sintering and vacuum sintering; the sintering process is carried out at a temperature of 400°C to 1050°C and a pressure of 0 MPa to 200 MPa; the deformation process is carried out by rolling or extrusion; The deformation temperature is controlled at 0-900℃ and the deformation ratio is 0-95%.

7. A graphene / copper composite material prepared by the method according to claim 5 or 6.

Citation Information

Patent Citations

  • Preparation method for polyaniline-coated graphene loaded copper-nickel solid solution composite material

    CN109559899A

  • Preparation method of grapheme-like or graphene metal composite powder

    CN110744052A

  • Method of synthesizing thickness-controlled graphene through chemical vapor deposition using cu-ni thin film laminate

    US20180346338A1