A hard mask composition and method for forming a pattern
The hard mask composition prepared by crosslinking solves the problem of lack of etch resistance of spin-coated hard mask materials in the prior art, and achieves efficient pattern etching and solvent properties, which is suitable for fine pattern formation in the semiconductor industry. .
Patent Information
- Application Number
- CN202311603977.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-11-28
AI Technical Summary
The lack of spin-coated hard mask materials with good solubility and etch resistance in the prior art makes it difficult to meet the semiconductor industry's demand for fine pattern etching.
Using a hard mask composition prepared by crosslinking compound I and compound II, combined with a crosslinking agent and solvent, a thin film with high etch resistance and good solvent properties is formed. Through the optimization of specific compound ratios and preparation process, high efficiency is achieved. Pattern formation and etching.
It realizes high etching resistance in N2/O2 and CHF3/CF4 gas environments, controls the etching rate within 23 angstroms/second and 20 angstroms/second, and has good solvent properties and gap filling characteristics, which is suitable for semiconductor industry Pattern etching.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hard mask materials, and in particular to a hard mask composition and a method for forming a pattern. Background Art
[0002] In recent years, the semiconductor industry has developed ultra-fine technology with patterns ranging from a few nanometers to tens of nanometers in size. To achieve such fine patterns, on the one hand, the wavelength of the light source used for lithography is developing towards a shorter wavelength, and on the other hand, in order to prevent the fine photoresist pattern from collapsing, the thickness of the photoresist film is gradually thinning. However, the thinned photoresist pattern is difficult to provide sufficient etching resistance to etch the material layer, so it is necessary to introduce an inorganic or organic film with strong etching resistance between the photoresist and the material layer. This film is called a resist underlayer film or a hard mask.
[0003] The hard mask layer is usually prepared by chemical vapor deposition. The hard mask layer prepared by chemical vapor deposition has excellent etching resistance and etching selectivity, but there are also some problems, such as particle contamination and huge investment in startup equipment. Therefore, in recent years, chemical vapor deposition hard mask materials have gradually been replaced by spin-coated hard mask materials. Spin-coated hard mask is a material that is spin-coated on the substrate as the first layer. The substrate structure needs to be smoothed to provide a flat surface for the subsequent spin coating of SiARC and photoresist.
[0004] Therefore, it is of great significance to study a spin-on hard mask material with good solubility and etching resistance. Summary of the invention
[0005] The purpose of the present invention is to provide a hard mask composition and a scheme for forming a pattern in view of the problem that the prior art lacks a spin-on hard mask material with both good solubility and etching resistance. The hard mask composition comprises a combination of two compound monomers, has good gap filling properties and material solubility, exhibits excellent performance in terms of etching resistance, achieves unexpected technical effects, and is easy to promote and apply.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A hard mask composition is prepared from the following raw materials: compound I, compound II, a crosslinking agent and a solvent; wherein the structural formula of compound I is as shown in formula I:
[0008]
[0009] In formula I, n is an integer of 40 to 80;
[0010] The structural formula of compound II is shown in formula II:
[0011]
[0012] Wherein, n in formula II is an integer of 50-1000; R1 is a C1-C6 methylene group, R2 is a C1-C6 straight-chain or branched alkyl group, and R3 is a methyl group or hydrogen.
[0013] The present invention provides a hard mask composition and a method for forming a pattern. The hard mask composition is prepared by cross-linking a compound I and a compound II. A film formed by the prepared hard mask composition has high etching resistance, wherein the main etching rate in a N2 / O2 mixed gas environment can be controlled within 23 angstroms / second, and the main etching rate in a CHF3 / CF4 mixed gas environment can be controlled within 20 angstroms / second. At the same time, the hard mask composition has high solubility and good gap filling properties, which is convenient for promotion and application.
[0014] Further, compound I is
[0015]
[0016] Furthermore, in Formula II, n is an integer of 200-1000, and R2 is a methyl group or an ethyl group.
[0017] Further, compound II is
[0018]
[0019] Furthermore, the hard mask composition is prepared by the following method:
[0020] Compound I, compound II and a solvent are mixed, heated to above 80° C., a crosslinking agent is added under stirring, and stirring is maintained for 1-3 hours to obtain a hard mask composition; wherein the mass content of the compound in the hard mask composition is 1% to 50%.
[0021] Furthermore, the weight ratio of the compound I to the compound II is 0.3 to 0.8:1. The inventors have found through research that the addition ratio of the two compounds is a key factor affecting the hard mask composition. Too large or too small a ratio will reduce the product performance. Preferably, the weight ratio of the compound I to the compound II is 0.3 to 0.6:1.
[0022] Furthermore, the cross-linking agent is isobutyltriethoxysilane.
[0023] Furthermore, the solvent is at least one of propylene glycol, hexane, methoxypropylene glycol, propylene glycol diacetate, diethylene glycol butyl ether, propylene glycol monomethyl ether, γ-butyrolactone, cyclohexanone, N,N-dimethylformamide, N,N-dimethylacetamide, nitromethane, methyl pyrrolidone and acetylacetone.
[0024] Another object of the present invention is to provide a method for using the hard mask composition.
[0025] A method for forming a pattern using the hard mask composition comprises the following steps:
[0026] Step 1, spin coating a hard mask composition on a material layer of a substrate, and performing a heat treatment to form a hard mask layer;
[0027] Step 2, forming a photoresist layer on the hard mask layer;
[0028] Step 3, exposing and developing the photoresist layer to form a photoresist pattern;
[0029] Step 4: selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer, and etching the exposed portion of the material layer.
[0030] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0031] The present invention provides a hard mask composition and a method for forming a pattern. The hard mask composition is prepared by cross-linking a compound I and a compound II. A film formed by the prepared hard mask composition has high etching resistance, wherein the main etching rate in a N2 / O2 mixed gas environment can be controlled within 23 angstroms / second, and the main etching rate in a CHF3 / CF4 mixed gas environment can be controlled within 20 angstroms / second. At the same time, the hard mask composition has high solubility and good gap filling properties, which is convenient for promotion and application. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0033] Example 1
[0034] Preparation of compounds I
[0035] Benzyl alcohol, p-nitroacetophenone, sodium hydroxide, ammonium acetate and γ-MnO2 nanoparticles (molar ratio of 1:1:1:1:0.1) were mixed and then heated under 450 W microwave irradiation for 5 min. The product was cooled to room temperature, washed with ethanol, centrifuged, and then the crude product was recrystallized in a mixture of n-hexane and ethyl acetate (volume ratio of 1:1), filtered, and dried to obtain a monomer.
[0036] Mix 48 mmol of iron powder and a hydrochloric acid solution containing 125 mmol of hydrochloric acid (50:125), heat and boil for 8 minutes; take 10 mmol of the monomer and dissolve it in 200 mmol of ethanol; transfer the two solutions into a constant pressure dropping funnel, add them dropwise into the device at a rate of 0.6 mL / min, and reflux at 80°C for redox reaction for 8 hours; then filter while hot to remove the iron powder, collect the filtrate, concentrate it, recrystallize it with ethanol, and dry it to obtain the diamine monomer.
[0037] 6 mmol of dimethoxymethane and 1 mmol of the diamine monomer prepared above were mixed and dissolved, and 110 mmol of trifluoroacetic acid was added dropwise to the reverse solution at 0°C; after the addition, the reaction was continued at 25°C for 24 hours under nitrogen protection; then, ammonia water was added to the product until pH = 8, filtered, and washed; the obtained solid product was dissolved in chloroform, n-hexane was added, a solid was precipitated, filtered, and dried to obtain compound I, wherein the specific structure of compound I is n is 40-80.
[0038] Preparation of Compound II
[0039] First, 14 g of 2-(methylthio)ethanol and 22 g of triethylamine were dissolved in 200 mL of anhydrous dichloromethane to obtain a mixed solution I; then, 18 g of acryloyl chloride was dissolved in 50 mL of dichloromethane solution to obtain a mixed solution II; under ice bath conditions, the mixed solution II was added dropwise to the mixed solution I, and the reaction was maintained for 18 hours. Then, the filtrate was filtered, and the filtrate was washed twice with a saturated sodium bicarbonate solution, 1M HCl, and a saturated sodium chloride solution, dried with anhydrous magnesium sulfate, and concentrated to obtain a crude product.
[0040] Then, 3 g of the crude product was added to a mixed solution of 30 mL of water and 30 mL of acetone, and 55 mg of molybdenum dioxide dichloride was added and stirred to obtain a mixed solution III; 25 mmol of a 33% hydrogen peroxide solution was added dropwise to the mixed solution III under ice bath conditions, and the mixture was reacted for 2 h until the solution became clear. The clear solution was then concentrated, extracted with dichloromethane, dried, and concentrated to obtain a monomer.
[0041] Finally, 1 g of monomer and 30 g of BCSPA, a RAFT chain transfer agent, were dissolved in 3 mL of DMF and placed in a 70 °C oil bath for reaction for 30 h. The reaction was then terminated by quick freezing with liquid nitrogen. The product was precipitated with icy ether and dried under reduced pressure to obtain compound II.
[0042] n is 500-1000.
[0043] Preparation of hard mask composition
[0044] Compound I, compound II and methoxypropylene glycol are mixed, wherein the weight addition ratio of compound I to compound II is 0.5:1, heated to 80°C, and isobutyltriethoxysilane is added under stirring conditions, and stirring is maintained for 2 hours to obtain a hard mask composition; wherein the mass content of the compound in the hard mask composition is 10%.
[0045] Forming a pattern
[0046] Spin coating the hard mask composition on the material layer of the substrate and performing a heat treatment to form a hard mask layer;
[0047] forming a photoresist layer on the hard mask layer;
[0048] exposing and developing the photoresist layer to form a photoresist pattern;
[0049] selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer, and
[0050] The exposed portion of the material layer is etched.
[0051] Example 2
[0052] Preparation of Compound I
[0053] Methylbenzyl alcohol, p-nitroacetophenone, sodium hydroxide, ammonium acetate and γ-MnO2 nanoparticles (molar ratio of 1:1:1:1:0.1) were mixed and then heated under 450 W microwave irradiation for 5 min. The product was cooled to room temperature, washed with ethanol, centrifuged, and then the crude product was recrystallized in a mixture of n-hexane and ethyl acetate (volume ratio of 1:1), filtered, and dried to obtain a monomer.
[0054] Mix 48 mmol of iron powder and a hydrochloric acid solution containing 125 mmol of hydrochloric acid (50:125), heat and boil for 8 minutes; take 10 mmol of the monomer and dissolve it in 200 mmol of ethanol; transfer the two solutions into a constant pressure dropping funnel, add them dropwise into the device at a rate of 0.6 mL / min, and reflux at 80°C for redox reaction for 8 hours; then filter while hot to remove the iron powder, collect the filtrate, concentrate it, recrystallize it with ethanol, and dry it to obtain the diamine monomer.
[0055] 6 mmol of dimethoxymethane and 1 mmol of the diamine monomer prepared above were mixed and dissolved, and 110 mmol of trifluoroacetic acid was added dropwise to the reverse solution at 0°C; after the addition was completed, the reaction was continued at 25°C under nitrogen protection for 24 hours; then, ammonia water was added to the product until pH = 8, filtered, and washed; the obtained solid product was dissolved in chloroform, n-hexane was added, the solid was precipitated, filtered, and dried to obtain compound I,
[0056] Among them, the specific structure of compound I is n is 40-80.
[0057] Preparation of Compound II
[0058] First, 14 g of 2-hydroxyethyl ethyl sulfide and 22 g of triethylamine were dissolved in 200 mL of anhydrous dichloromethane to obtain a mixed solution I; then, 18 g of acryloyl chloride was dissolved in 50 mL of dichloromethane solution to obtain a mixed solution II; under ice bath conditions, the mixed solution II was added dropwise to the mixed solution I, and the reaction was maintained for 18 hours. Then, the filtrate was filtered, and the filtrate was washed twice with a saturated sodium bicarbonate solution, 1M HCl, and a saturated sodium chloride solution, dried with anhydrous magnesium sulfate, and concentrated to obtain a crude product.
[0059] Then, 3 g of the crude product was added to a mixed solution of 30 mL of water and 30 mL of acetone, and 55 mg of molybdenum dioxide dichloride was added and stirred to obtain a mixed solution III; 25 mmol of a 33% hydrogen peroxide solution was added dropwise to the mixed solution III under ice bath conditions, and the mixture was reacted for 2 h until the solution became clear. The clear solution was then concentrated, extracted with dichloromethane, dried, and concentrated to obtain a monomer.
[0060] Finally, 1 g of monomer and 30 g of BCSPA, a RAFT chain transfer agent, were dissolved in 3 mL of DMF and placed in a 70 °C oil bath for reaction for 30 h. The reaction was then terminated by quick freezing with liquid nitrogen. The product was precipitated with icy ether and dried under reduced pressure to obtain compound II.
[0061] n is 500-1000.
[0062] Preparation of hard mask composition
[0063] Compound I, compound II and nitromethane are mixed, wherein the weight ratio of compound I to compound II is 0.6:1, heated to 85° C., isobutyltriethoxysilane is added under stirring, and stirring is maintained for 1 hour to obtain a hard mask composition; wherein the mass content of the compound in the hard mask composition is 10%.
[0064] Forming a pattern
[0065] Spin coating the hard mask composition on the material layer of the substrate and performing a heat treatment to form a hard mask layer;
[0066] forming a photoresist layer on the hard mask layer;
[0067] exposing and developing the photoresist layer to form a photoresist pattern;
[0068] selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer, and
[0069] The exposed portion of the material layer is etched.
[0070] Example 3
[0071] Preparation of Compound I
[0072] Trifluoromethylbenzyl alcohol, p-nitroacetophenone, sodium hydroxide, ammonium acetate and γ-MnO2 nanoparticles (molar ratio of 1:1:1:1:0.1) were mixed and then heated under 450 W microwave irradiation for 5 min. The product was cooled to room temperature, washed with ethanol, centrifuged, and then the crude product was recrystallized in a mixture of n-hexane and ethyl acetate (volume ratio of 1:1), filtered, and dried to obtain a monomer.
[0073] Mix 48 mmol of iron powder and a hydrochloric acid solution containing 125 mmol of hydrochloric acid (50:125), heat and boil for 8 minutes; take 10 mmol of the monomer and dissolve it in 200 mmol of ethanol; transfer the two solutions into a constant pressure dropping funnel, add them dropwise into the device at a rate of 0.6 mL / min, and reflux at 80°C for redox reaction for 8 hours; then filter while hot to remove the iron powder, collect the filtrate, concentrate it, recrystallize it with ethanol, and dry it to obtain the diamine monomer.
[0074] 6 mmol of dimethoxymethane and 1 mmol of the diamine monomer prepared above were mixed and dissolved, and 110 mmol of trifluoroacetic acid was added dropwise to the reverse solution at 0°C; after the addition, the reaction was continued at 25°C for 24 hours under nitrogen protection; then, ammonia water was added to the product until pH = 8, filtered, and washed; the obtained solid product was dissolved in chloroform, n-hexane was added, a solid was precipitated, filtered, and dried to obtain compound I, wherein the specific structure of compound I is
[0075] n is 40-80.
[0076] Preparation of Compound II
[0077] First, 14 g of 2-(pentylthio)ethanol and 22 g of triethylamine were dissolved in 200 mL of anhydrous dichloromethane to obtain a mixed solution I; then, 18 g of acryloyl chloride was dissolved in 50 mL of dichloromethane solution to obtain a mixed solution II; under ice bath conditions, the mixed solution II was added dropwise to the mixed solution I, and the reaction was maintained for 18 hours. Then, the filtrate was filtered, and the filtrate was washed twice with a saturated sodium bicarbonate solution, 1M HCl, and a saturated sodium chloride solution, dried with anhydrous magnesium sulfate, and concentrated to obtain a crude product.
[0078] Then, 3 g of the crude product was added to a mixed solution of 30 mL of water and 30 mL of acetone, and 55 mg of molybdenum dioxide dichloride was added and stirred to obtain a mixed solution III; 25 mmol of a 33% hydrogen peroxide solution was added dropwise to the mixed solution III under ice bath conditions, and the mixture was reacted for 2 h until the solution became clear. The clear solution was then concentrated, extracted with dichloromethane, dried, and concentrated to obtain a monomer.
[0079] Finally, 1 g of monomer and 30 g of BCSPA, a RAFT chain transfer agent, were dissolved in 3 mL of DMF and placed in a 70 °C oil bath for reaction for 30 h. The reaction was then terminated by quick freezing with liquid nitrogen. The product was precipitated with icy ether and dried under reduced pressure to obtain compound II.
[0080] n is 500-1000.
[0081] Preparation of hard mask composition
[0082] Compound I, compound II and γ-butyrolactone are mixed, wherein the weight addition ratio of compound I to compound II is 0.3:1, heated to 80°C, and isobutyltriethoxysilane is added under stirring conditions, and stirring is maintained for 2 hours to obtain a hard mask composition; wherein the mass content of the compound in the hard mask composition is 10%.
[0083] Forming a pattern
[0084] Spin coating the hard mask composition on the material layer of the substrate and performing a heat treatment to form a hard mask layer;
[0085] forming a photoresist layer on the hard mask layer;
[0086] exposing and developing the photoresist layer to form a photoresist pattern;
[0087] selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer, and
[0088] The exposed portion of the material layer is etched.
[0089] Example 4
[0090] Preparation of Compound I
[0091] Benzyl alcohol, p-nitroacetophenone, sodium hydroxide, ammonium acetate and γ-MnO2 nanoparticles (molar ratio of 1:1:1:1:0.1) were mixed and then heated under 450 W microwave irradiation for 5 min. The product was cooled to room temperature, washed with ethanol, centrifuged, and then the crude product was recrystallized in a mixture of n-hexane and ethyl acetate (volume ratio of 1:1), filtered, and dried to obtain a monomer.
[0092] Mix 48 mmol of iron powder and a hydrochloric acid solution containing 125 mmol of hydrochloric acid (50:125), heat and boil for 8 minutes; take 10 mmol of the monomer and dissolve it in 200 mmol of ethanol; transfer the two solutions into a constant pressure dropping funnel, add them dropwise into the device at a rate of 0.6 mL / min, and reflux at 80°C for redox reaction for 8 hours; then filter while hot to remove the iron powder, collect the filtrate, concentrate it, recrystallize it with ethanol, and dry it to obtain the diamine monomer.
[0093] 6 mmol of dimethoxymethane and 1 mmol of the diamine monomer prepared above were mixed and dissolved, and 110 mmol of trifluoroacetic acid was added dropwise to the reverse solution at 0°C; after the addition, the reaction was continued at 25°C for 24 hours under nitrogen protection; then, ammonia water was added to the product until pH = 8, filtered, and washed; the obtained solid product was dissolved in chloroform, n-hexane was added, a solid was precipitated, filtered, and dried to obtain compound I, wherein the specific structure of compound I is n is 40-80.
[0094] Preparation of Compound II
[0095] First, 14 g of 2-(pentylthio)ethanol and 22 g of triethylamine were dissolved in 200 mL of anhydrous dichloromethane to obtain a mixed solution I; then, 18 g of acryloyl chloride was dissolved in 50 mL of dichloromethane solution to obtain a mixed solution II; under ice bath conditions, the mixed solution II was added dropwise to the mixed solution I, and the reaction was maintained for 18 hours. Then, the filtrate was filtered, and the filtrate was washed twice with a saturated sodium bicarbonate solution, 1M HCl, and a saturated sodium chloride solution, dried with anhydrous magnesium sulfate, and concentrated to obtain a crude product.
[0096] Then, 3 g of the crude product was added to a mixed solution of 30 mL of water and 30 mL of acetone, and 55 mg of molybdenum dioxide dichloride was added and stirred to obtain a mixed solution III; 25 mmol of a 33% hydrogen peroxide solution was added dropwise to the mixed solution III under ice bath conditions, and the mixture was reacted for 2 h until the solution became clear. The clear solution was then concentrated, extracted with dichloromethane, dried, and concentrated to obtain a monomer.
[0097] Finally, 1 g of monomer and 30 g of BCSPA, a RAFT chain transfer agent, were dissolved in 3 mL of DMF and placed in a 70 °C oil bath for reaction for 30 h. The reaction was then terminated by quick freezing with liquid nitrogen. The product was precipitated with icy ether and dried under reduced pressure to obtain compound II.
[0098] n is 500-1000.
[0099] Preparation of hard mask composition
[0100] Compound I, compound II and γ-butyrolactone are mixed, wherein the weight addition ratio of compound I to compound II is 0.3:1, heated to 80°C, and isobutyltriethoxysilane is added under stirring conditions, and stirring is maintained for 2 hours to obtain a hard mask composition; wherein the mass content of the compound in the hard mask composition is 10%.
[0101] Forming a pattern
[0102] Spin coating the hard mask composition on the material layer of the substrate and performing a heat treatment to form a hard mask layer;
[0103] forming a photoresist layer on the hard mask layer;
[0104] exposing and developing the photoresist layer to form a photoresist pattern;
[0105] selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer, and
[0106] The exposed portion of the material layer is etched.
[0107] Example 5
[0108] Preparation of Compound I
[0109] Trifluoromethylbenzyl alcohol, p-nitroacetophenone, sodium hydroxide, ammonium acetate and γ-MnO2 nanoparticles (molar ratio of 1:1:1:1:0.1) were mixed and then heated under 450 W microwave irradiation for 5 min. The product was cooled to room temperature, washed with ethanol, centrifuged, and then the crude product was recrystallized in a mixture of n-hexane and ethyl acetate (volume ratio of 1:1), filtered, and dried to obtain a monomer.
[0110] Mix 48 mmol of iron powder and a hydrochloric acid solution containing 125 mmol of hydrochloric acid (50:125), heat and boil for 8 minutes; take 10 mmol of the monomer and dissolve it in 200 mmol of ethanol; transfer the two solutions into a constant pressure dropping funnel, add them dropwise into the device at a rate of 0.6 mL / min, and reflux at 80°C for redox reaction for 8 hours; then filter while hot to remove the iron powder, collect the filtrate, concentrate it, recrystallize it with ethanol, and dry it to obtain the diamine monomer.
[0111] 6 mmol of dimethoxymethane and 1 mmol of the diamine monomer prepared above were mixed and dissolved, and 110 mmol of trifluoroacetic acid was added dropwise to the reverse solution at 0°C; after the addition, the reaction was continued at 25°C for 24 hours under nitrogen protection; then, ammonia water was added to the product until pH = 8, filtered, and washed; the obtained solid product was dissolved in chloroform, n-hexane was added, a solid was precipitated, filtered, and dried to obtain compound I, wherein the specific structure of compound I is
[0112] n is 40-80.
[0113] Preparation of Compound II
[0114] First, 14 g of 2-(methylthio)ethanol and 22 g of triethylamine were dissolved in 200 mL of anhydrous dichloromethane to obtain a mixed solution I; then, 18 g of acryloyl chloride was dissolved in 50 mL of dichloromethane solution to obtain a mixed solution II; under ice bath conditions, the mixed solution II was added dropwise to the mixed solution I, and the reaction was maintained for 18 hours. Then, the filtrate was filtered, and the filtrate was washed twice with a saturated sodium bicarbonate solution, 1M HCl, and a saturated sodium chloride solution, dried with anhydrous magnesium sulfate, and concentrated to obtain a crude product.
[0115] Then, 3 g of the crude product was added to a mixed solution of 30 mL of water and 30 mL of acetone, and 55 mg of molybdenum dioxide dichloride was added and stirred to obtain a mixed solution III; 25 mmol of a 33% hydrogen peroxide solution was added dropwise to the mixed solution III under ice bath conditions, and the mixture was reacted for 2 h until the solution became clear. The clear solution was then concentrated, extracted with dichloromethane, dried, and concentrated to obtain a monomer.
[0116] Finally, 1 g of monomer and 30 g of BCSPA, a RAFT chain transfer agent, were dissolved in 3 mL of DMF and placed in a 70 °C oil bath for reaction for 30 h. The reaction was then terminated by quick freezing with liquid nitrogen. The product was precipitated with icy ether and dried under reduced pressure to obtain compound II.
[0117] n is 500-1000.
[0118] Preparation of hard mask composition
[0119] Compound I, compound II and methoxypropylene glycol are mixed, wherein the weight addition ratio of compound I to compound II is 0.5:1, heated to 80°C, and isobutyltriethoxysilane is added under stirring conditions, and stirring is maintained for 2 hours to obtain a hard mask composition; wherein the mass content of the compound in the hard mask composition is 10%.
[0120] Forming a pattern
[0121] Spin coating the hard mask composition on the material layer of the substrate and performing a heat treatment to form a hard mask layer;
[0122] forming a photoresist layer on the hard mask layer;
[0123] exposing and developing the photoresist layer to form a photoresist pattern;
[0124] selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer, and
[0125] The exposed portion of the material layer is etched.
[0126] Comparative Example 1
[0127] Comparative Example 1 Compared with Example 1, Compound I was not added, and only Compound II prepared in Example 1 was used to prepare a hard mask composition.
[0128] Mix compound II and methoxypropylene glycol, wherein the amount of compound II added is the total weight of compound I and compound II in Example 1, heat to 80°C, add isobutyltriethoxysilane under stirring conditions, and keep stirring for 2 hours to obtain a hard mask composition; wherein the mass content of the compound in the hard mask composition is 10%.
[0129] Comparative Example 2
[0130] Comparative Example 2 Compared with Example 1, Compound II was not added, and only Compound I prepared in Example 1 was used to prepare a hard mask composition.
[0131] Compound I and methoxypropylene glycol are mixed, wherein the amount of compound I added is the total weight of compound I and compound II in Example 1, heated to 80° C., isobutyltriethoxysilane is added under stirring, and stirring is maintained for 2 hours to obtain a hard mask composition; wherein the mass content of the compound in the hard mask composition is 10%.
[0132] Comparative Example 3
[0133] Comparative Example 3 changes the preparation process of the hard mask composition compared to Example 1, and both Compound I and Compound II are prepared using Example 1. The specific operation is as follows:
[0134] Preparation of hard mask composition
[0135] Compound I, compound II and methoxypropylene glycol are mixed, wherein the weight addition ratio of compound I to compound II is 0.5:1, to obtain a hard mask composition; wherein the mass content of the compound in the hard mask composition is 10%.
[0136] Comparative Example 4
[0137] In Comparative Example 4, the addition ratio of Compound I and Compound II in the hard mask composition is changed compared with Example 1, as follows:
[0138] Preparation of hard mask composition
[0139] Compound I, compound II and methoxypropylene glycol are mixed, wherein the weight addition ratio of compound I to compound II is 0.2:1, heated to 80°C, and isobutyltriethoxysilane is added under stirring conditions, and stirring is maintained for 2 hours to obtain a hard mask composition; wherein the mass content of the compound in the hard mask composition is 10%.
[0140] Comparative Example 5
[0141] Compared with Example 1, the addition ratio of Compound I and Compound II in the hard mask composition is changed in Comparative Example 5, as follows:
[0142] Preparation of hard mask composition
[0143] Compound I, compound II and methoxypropylene glycol are mixed, wherein the weight addition ratio of compound I to compound II is 1:1, heated to 80° C., isobutyltriethoxysilane is added under stirring conditions, and stirring is maintained for 2 hours to obtain a hard mask composition; wherein the mass content of the compound in the hard mask composition is 10%.
[0144] Test 1
[0145] The hard mask compositions according to Examples 1-5 and Comparative Examples 1-5 were spin-coated on silicon chips, and then heated at 300°C for 3 minutes to prepare a 3500 angstrom thick film. Then, the film was dry-etched for 60 seconds and 100 seconds using N2 / O2 mixed gas and CFx mixed gas, respectively, and the thickness of the film was then measured to calculate the etching rate. The test results are shown in Table 1. Main etching rate = (initial film thickness - film thickness after etching) / etching time (angstrom / second)
[0146] Table 1 Test results
[0147]
[0148]
[0149] It can be seen from the test results in Table 1 that the film formed by the hard mask composition provided in the present application has high etching resistance. The study found that the selection, dosage and preparation process of the compound are all important factors affecting the etching resistance of the hard mask composition. If the above factors are changed, the etching resistance will decrease.
[0150] Test 2
[0151] At room temperature (25° C.), the hard mask compositions prepared in Examples 1-5 and Comparative Examples 1-5 were placed in 100 mL of propylene glycol monomethyl ether acetate (PGMEA) solvent until saturated, and then fully stirred to prepare each solution. The solution was filtered and the solid obtained by filtration was measured. The solubility test results are shown in Table 2.
[0152] The hard mask compositions prepared in Examples 1-5 and Comparative Examples 1-5 were spin-coated on patterned silicon chips, dried at 350° C. for 3 min, and then the gap filling characteristics were detected using a FE-SEM device. Specifically, the gap filling characteristics were determined by using an electron scanning microscope to check the cross section of the pattern to see if there was a gap, and the detection results are shown in Table 2.
[0153] Table 2 Test results
[0154]
[0155]
[0156] It can be seen from the test results in Table 2 that the hard mask composition provided by the present application has high solubility and good gap filling properties. The study found that the selection of compounds, dosage and preparation process are all important factors affecting the solubility and gap filling properties of the hard mask composition. If the above factors are changed, the solubility and gap filling properties will decrease.
[0157] The present invention provides a hard mask composition and a method for forming a pattern. The hard mask composition is prepared by cross-linking a compound I and a compound II. A film formed by the prepared hard mask composition has high etching resistance, wherein the main etching rate in a N2 / O2 mixed gas environment can be controlled within 23 angstroms / second, and the main etching rate in a CHF3 / CF4 mixed gas environment can be controlled within 20 angstroms / second. At the same time, the hard mask composition has high solubility and good gap filling properties, which is convenient for promotion and application.
[0158] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A hard mask composition, characterized in that The method comprises the following raw materials: compound I, compound II, a cross-linking agent and a solvent; Wherein, compound I is: , or ; n in compound I is an integer of 40 to 80; Compound II is: , or ; n in compound II is an integer of 500-1000; The hard mask composition is prepared by the following method: mixing compound I, compound II and a solvent, heating to above 80° C., adding a crosslinking agent under stirring conditions, and maintaining stirring for 1-3 hours to obtain a hard mask composition; wherein the mass content of the compound in the hard mask composition is 1% to 50%; The added weight ratio of the compound I to the compound II is 0.3-0.6:
1.
2. The hard mask composition according to claim 1, characterized in that The crosslinking agent is isobutyltriethoxysilane.
3. The hard mask composition according to claim 1, characterized in that The solvent is at least one of propylene glycol, hexane, methoxypropylene glycol, propylene glycol diacetate, diethylene glycol butyl ether, propylene glycol monomethyl ether, γ-butyrolactone, cyclohexanone, N,N-dimethylformamide, N,N-dimethylacetamide, nitromethane, methyl pyrrolidone and acetylacetone.
4. A method for forming a pattern using the hard mask composition according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1, spin coating a hard mask composition on a material layer of a substrate, and performing a heat treatment to form a hard mask layer; Step 2, forming a photoresist layer on the hard mask layer; Step 3, exposing and developing the photoresist layer to form a photoresist pattern; Step 4: selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer, and etching the exposed portion of the material layer.
Citation Information
Patent Citations
Acrylate film-forming resin containing cubane, ArF photoresist, preparation method of ArF photoresist and photoetching method
CN109679020A
High etch resistance spin-on carbon hard mask composition and patterning method using same
CN109844639A
Hard mask composition, hard mask layer, and pattern forming method
CN114424122A
Hardmask composition and method of forming patterns using the hardmask composition
KR1020160008930A
KR20210070812A