Thermosetting resin composition, anisotropic conductive film and connection structure

By using a cationic curing system of tetrahydroindenediepoxide and quaternary ammonium salt compounds in the thermosetting resin composition, the problems of low storage stability and curing shrinkage of the anisotropic conductive film during the rapid curing process of low temperature are solved. Stable curing and high connection reliability at lower temperatures and short time are achieved, reducing substrate warping.

CN117659667BActive Publication Date: 2024-11-01CHANGZHOU DECHUANG HIGH TECH MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311623638.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-30
Publication Date
2024-11-01
Estimated Expiration
2043-11-30

AI Technical Summary

Technical Problem

The existing anisotropic conductive films have problems with low storage stability and curing shrinkage during the fast curing process of low temperatures, making it difficult to achieve reliable connections at lower temperatures and in a short time, resulting in circuit wiring position offset and substrate warping.

Method used

Using a cationic curing system of tetrahydroindenediepoxide and quaternary ammonium salt compounds, the curing at a lower temperature and shorter time is achieved by adding film-forming additive components to the thermosetting resin composition, and curing is reduced, and curing shrinkage is reduced. Improve connection reliability.

Benefits of technology

It realizes stable curing at a lower temperature and in a short time, improves the storage stability and connection reliability of the anisotropic conductive film, reduces substrate warping, and ensures a stable connection state under low stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present disclosure provides a thermosetting resin composition, an anisotropic conductive film and a connection structure. The thermosetting resin composition in the present disclosure includes the following components: (A) a cationic polymerizable resin, including tetrahydroindene diepoxide, the content of which accounts for 5% to 50% by weight of the thermosetting resin composition; (B) a thermal acid generating initiator, including a quaternary ammonium salt compound, the content of which accounts for 0.05% to 30% by weight of the cationic polymerizable resin; (C) a film-forming additive, the content of which accounts for 20% to 70% by weight of the thermosetting resin composition; (D) conductive particles, the content of which is 20 to 100,000 particles / mm 2 Conductive film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of bonding and connecting electronic components, and in particular to a thermosetting resin composition, an anisotropic conductive film and a connection structure. Technical Background

[0002] In the fields of semiconductors and flat panel displays, anisotropic conductive films are widely used to fix electronic components or connect circuits due to their directional conductive properties, such as chip packaging (COG) that directly mounts IC chips on glass substrates and packaging of flexible circuit substrates (FOG).

[0003] In the past, anisotropic conductive films were mainly prepared by using an epoxy curing composition with anionic curing agents or cationic curing agents as an adhesive layer and dispersing conductive particles therein. As electronic components gradually become smaller, denser, and more refined, the electrode width and electrode spacing become narrower, and IC chips and glass substrates become very thin. Due to the hot pressing during connection, problems such as component burning or circuit wiring position displacement after packaging may occur due to the relative thermal expansion difference of the circuit substrate. Especially in COG packaging, due to the curing shrinkage of the anisotropic conductive film or the thermal expansion difference between the IC chip and the glass substrate, the substrate may be warped, resulting in uneven display on the display. In addition, in terms of production costs, in order to reduce costs and improve production efficiency, it is necessary to prepare the adhesive layer material of the anisotropic conductive film to be able to complete curing at a lower temperature (e.g., 140-150°C) and in a shorter time (e.g., within 5 seconds).

[0004] In recent years, in order to achieve the storage stability and low-temperature rapid curing of the adhesive layer material of the anisotropic conductive film, the development direction is mainly towards a cationic curing system that can be cured at low temperatures. Compared with the general glycidyl ether compounds, alicyclic epoxy compounds with higher cationic polymerization reactivity and no oxygen to hinder the polymerization reaction are used as dark-reactive polymerization initiators, and the use of sulfonium salt-based thermal acid initiators that generate protons by heat is proposed. Such anisotropic conductive films containing alicyclic epoxy compounds and sulfonium salt-based thermal acid initiators show a relatively low temperature (for example, around 100°C) curing temperature.

[0005] However, there is also a problem that, for example, polymerization may start at a temperature of about 40 to 60°C, and the adhesive may also solidify during storage, resulting in a low storage stability. On the other hand, when a polymerization initiator with lower reactivity (such as an iodine salt compound) is used, although the storage stability of the anisotropic conductive film is ensured, it is difficult to solidify the adhesive layer material of the anisotropic conductive film under the conditions of a relatively low temperature (such as 140 to 150°C) and a relatively short time (such as within 5 seconds).

[0006] In summary, there is a need to provide an adhesive material that has excellent storage stability, can be cured at a lower temperature and in a shorter time, and can make the resulting anisotropic conductive film have good connection reliability. Summary of the invention

[0007] In view of this, in order to overcome any of the above and at least one of other defects in the prior art, the present disclosure proposes a thermosetting resin composition, which uses tetrahydroindene diepoxide and quaternary ammonium salt compounds in its film-forming additive components, so that the thermosetting resin composition has storage stability and can be cured at a lower temperature and in a shorter time, and an anisotropic conductive film with good connection reliability is successfully prepared. .

[0008] In addition, the present disclosure proposes a connection structure that performs anisotropic conductive connection between a first electronic component and a second electronic component through a cured anisotropic conductive film, thereby achieving a stable connection state under low stress and reducing warping of the substrate.

[0009] In order to achieve the above object, in one aspect of the present disclosure, a thermosetting resin composition is provided, which is suitable for thermal curing to prepare an anisotropic conductive film, and the composition comprises the following components:

[0010] (A) a cationic polymerizable resin comprising tetrahydroindene diepoxide, wherein the content of the tetrahydroindene diepoxide is 5 wt % to 50 wt % of the thermosetting resin composition;

[0011] (B) a thermal acid generating initiator, comprising a quaternary ammonium salt compound, wherein the content of the quaternary ammonium salt compound accounts for 0.05 wt % to 30 wt % of the cationic polymerizable resin;

[0012] (C) a film-forming additive component, wherein the content of the film-forming additive component accounts for 20% to 70% by weight of the thermosetting resin composition;

[0013] (D) conductive particles, the content of the conductive particles is 20 to 100,000 particles / mm 2 Conductive film.

[0014] According to an embodiment of the present disclosure, the content of tetrahydroindene diepoxide accounts for 10 wt % to 40 wt % of the thermosetting resin composition.

[0015] According to an embodiment of the present disclosure, the quaternary ammonium salt compound is a salt composed of a quaternary ammonium cation and a borate anion.

[0016] According to an embodiment of the present disclosure, the above-mentioned quaternary ammonium salt compound is selected from at least one of dimethylphenyl (4-methoxybenzyl) ammonium tetrakis (pentafluorophenyl) borate, dimethylphenyl (4-methylbenzyl) ammonium hexafluorotetrakis (pentafluorophenyl) borate, methylphenyl dibenzyl ammonium tetrakis (pentafluorophenyl) borate, phenyl tribenzyl ammonium tetrakis (pentafluorophenyl) borate, dimethylphenyl (3, 4-dimethylbenzyl) ammonium tetrakis (pentafluorophenyl) borate, and N, N-diethyl-N-benzylaniline boron tetrafluoride.

[0017] According to an embodiment of the present disclosure, the content of the quaternary ammonium salt compound accounts for 2 to 15 weight % of the cationic polymerizable resin.

[0018] According to an embodiment of the present disclosure, the content of the film-forming additive component accounts for 30 wt % to 60 wt % of the thermosetting resin composition.

[0019] According to an embodiment of the present disclosure, the film-forming additive component includes an epoxy resin or a phenoxy resin that is solid at room temperature.

[0020] According to an embodiment of the present disclosure, the epoxy resin is selected from at least one of bisphenol epoxy resin, novolac epoxy resin, naphthalene epoxy resin, and biphenyl epoxy resin.

[0021] According to an embodiment of the present disclosure, the phenoxy resin is selected from at least one of fluorene-type phenoxy resin, bisphenol-type phenoxy resin, novolac-type phenoxy resin, naphthalene-type phenoxy resin, and biphenyl-type phenoxy resin.

[0022] According to an embodiment of the present disclosure, the conductive particles are selected from at least one of nickel, cobalt, silver, copper, gold, palladium, solder, and metal-plated resin particles.

[0023] According to the embodiment of the present disclosure, the content of the above conductive particles is 200 to 70,000 particles / mm 2 Conductive film.

[0024] According to an embodiment of the present disclosure, the cationic polymerizable resin further includes dimeroxydicyclohexyl groups, and the content of the dimeroxydicyclohexyl groups accounts for 0 to 50 weight % of the cationic polymerizable resin.

[0025] In another aspect of the present disclosure, there is provided an anisotropic conductive film, which is made by thermally curing the above-mentioned thermosetting resin composition;

[0026] According to an embodiment of the present disclosure, the temperature of thermal curing is 140-160° C., and the curing time is within 5 seconds.

[0027] In another aspect of the present disclosure, a connection structure is provided, which is formed by anisotropically conductively connecting a first electronic component and a second electronic component using the anisotropic conductive film.

[0028] The thermosetting resin composition provided by the present disclosure can achieve curing at a lower temperature (for example) and in a shorter time by adding tetrahydroindene diepoxide and quaternary ammonium salt compounds to the film-forming additive components. The two cooperate with each other; at the same time, due to the presence of a rigid indene skeleton, there is no steric hindrance, so the curing shrinkage is small and the glass transition temperature (Tg) is high, thereby improving the storage stability and achieving low-temperature rapid curing.

[0029] The connection state of the connection structure provided by the present disclosure after curing is stable under low stress, which can reduce the warping of the substrate and greatly increase the connection reliability. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the present disclosure more clear, the present disclosure is further described in detail below in conjunction with specific embodiments. However, the present disclosure is not limited to the following embodiments.

[0031] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "including", "comprising", etc. used herein indicate the presence of features, steps, operations and / or components, but do not exclude the presence or addition of one or more other features, steps, operations or components. All terms (including technical and scientific terms) used herein have the meanings commonly understood by those skilled in the art, unless otherwise defined. It should be noted that the terms used herein should be interpreted as having meanings consistent with the context of this specification and should not be interpreted in an idealized or overly rigid manner.

[0032] In the process of realizing the present disclosure, it is found that a cationic curing system of tetrahydroindene diepoxide and a quaternary ammonium salt compound is used in the film-forming additive of the thermosetting resin composition. The indene skeleton in the tetrahydroindene diepoxide has no steric hindrance and the curing shrinkage is very small. Moreover, due to its rigid skeleton, its cured product Tg is relatively high. Therefore, the connection reliability of the anisotropic conductive film obtained by thermal curing of the composition can be improved, and storage stability and curing at a relatively low temperature and in a relatively short time can be achieved. Based on the above-mentioned anisotropic conductive film, a connection structure with high connection reliability that suppresses the warping of the substrate as much as possible under relatively low stress can be obtained.

[0033] In one aspect of the present disclosure, the thermosetting resin composition of the present disclosure is mainly composed of tetrahydroindene diepoxide, quaternary ammonium salt compound, film-forming additive and conductive particles as essential components. More specifically, a thermosetting resin composition is provided, which is suitable for thermal curing to prepare an anisotropic conductive film, and the composition includes the following components:

[0034] (A) a cationic polymerizable resin, comprising tetrahydroindene diepoxide, wherein the content of the tetrahydroindene diepoxide accounts for 5% to 50% by weight of the thermosetting resin composition, for example, 5%, 10%, 20%, 30%, 40%, 50% by weight, etc.;

[0035] (B) a thermal acid generating initiator, including a quaternary ammonium salt compound, wherein the content of the quaternary ammonium salt compound is 0.05% to 30% by weight of the cationic polymerizable resin, for example, 0.05%, 1%, 10%, 15%, 20%, 35%, 30% by weight, etc.;

[0036] (C) a film-forming additive component, wherein the content of the film-forming additive component accounts for 20% to 70% by weight of the thermosetting resin composition, for example, 20%, 30%, 40%, 50%, 60%, 70% by weight, etc.;

[0037] (D) Conductive particles, the content of the conductive particles is 20 to 100,000 particles / mm 2 Conductive film, for example, can be 20 / mm 2 , 50 pieces / mm 2 , 80 pieces / mm 2 , 100 pieces / mm 2 , 1000 pieces / mm 2 , 10000pcs / mm 2 , 100000 pieces / mm 2 wait.

[0038] According to the embodiments of the present disclosure, a cationic curing system of tetrahydroindene diepoxide and quaternary ammonium salt compounds is used in the film-forming additive component, and the two cooperate to fully cure at a relatively low temperature (e.g., 140-160° C.) and in a relatively short time (e.g., within 5 seconds). The formed cured product has a rigid indene skeleton without steric hindrance, has a relatively high Tg and a relatively small curing shrinkage compared to other alicyclic epoxy resins, so that the anisotropic conductive film containing conductive particles formed therefrom exhibits a stable connection state under low stress, and can minimize the warping of the substrate.

[0039] According to the embodiments of the present disclosure, the cationic polymerizable resin used in the present disclosure refers to a resin or resin monomer having at least one cationic polymerizable functional group, and the cationic ring-opening polymerizable functional group may be exemplified by cyclic ether, cyclic imine, lactone, etc. Examples of the cationic polymerizable resin include not only tetrahydroindene diepoxide monomers, but also other epoxy resins.

[0040] According to the embodiments of the present disclosure, when other epoxy resins are used in combination, an epoxy resin having the same reactivity as tetrahydroindene diepoxide is selected as much as possible, for example, alicyclic epoxy resins can be used, and dimeroxydicyclohexyl is preferably used.

[0041] According to an embodiment of the present disclosure, the cationic polymerizable resin also includes dicyclohexyl oxide, and the content of dicyclohexyl oxide accounts for 0 to 50 weight % of the cationic polymerizable resin, for example, it can be 0 weight %, 10 weight %, 20 weight %, 30 weight %, 40 weight %, 50 weight %, etc.

[0042] According to the embodiments of the present disclosure, tetrahydroindene diepoxide is an alicyclic epoxy resin having an indene skeleton, which can be prepared by a conventionally known method. For example, tetrahydroindene diepoxide (a compound represented by the following formula (T)) can be prepared by epoxidizing a corresponding cyclic polyolefin compound (a compound represented by the following formula (I)) with an oxidizing agent.

[0043]

[0044] Examples of the oxidizing agent include hydrogen peroxide, aliphatic percarboxylic acid, organic peroxide, etc. The amount of the oxidizing agent used is 1 equivalent or more, preferably 1 to 2 equivalents, relative to the unsaturated bonds of the cyclic polyolefin compound.

[0045] The epoxidation reaction is preferably carried out in a solvent. Examples of the solvent include aliphatic hydrocarbons such as hexane and cyclohexane, aromatic hydrocarbons such as toluene, and esters such as ethyl acetate and methyl acetate.

[0046] The reaction temperature is preferably 20 to 70° C., for example, 20° C., 30° C., 40° C., 50° C., 60° C., 70° C., etc. The reaction time depends on the reaction scale, etc., and ranges from 1 to 100 hours, for example, 1 hour, 10 hours, 20 hours, 30 hours, 50 hours, 70 hours, 90 hours, 100 hours, etc.

[0047] After the reaction is completed, the target tetrahydroindene diepoxide can be obtained by a method such as precipitation with a poor solvent, a method of putting the epoxide into hot water under stirring and distilling off the solvent, a direct desolvation method, etc. There are four stereoisomers based on the stereo configuration of two epoxy rings in tetrahydroindene diepoxide, but their ratios have little effect on the characteristics of the anisotropic conductive film disclosed in the present invention.

[0048] According to an embodiment of the present disclosure, the content of tetrahydroindene diepoxide accounts for 10 wt % to 40 wt % of the thermosetting resin composition.

[0049] According to the embodiments of the present disclosure, if the content of tetrahydroindene diepoxide is too little, the expected effect cannot be achieved, and if the content is too much, the membrane performance cannot be maintained.

[0050] According to an embodiment of the present disclosure, the quaternary ammonium salt compound may be a salt composed of a quaternary ammonium cation and a borate anion;

[0051] Quaternary ammonium salt compounds are used as thermal acid initiators for curing epoxy resins such as tetrahydroindene diepoxide, and can act on curing at a relatively low temperature and in a short time, thereby improving storage stability. The borate anion is preferably BF4- or (BX4)-, wherein X represents a phenyl group substituted with at least two or more fluorine or trifluoromethyl groups.

[0052] Preferably, the quaternary ammonium salt compound is selected from at least one of dimethylphenyl (4-methoxybenzyl) ammonium tetrakis (pentafluorophenyl) borate, dimethylphenyl (4-methylbenzyl) ammonium hexafluorotetrakis (pentafluorophenyl) borate, methylphenyldibenzyl ammonium tetrakis (pentafluorophenyl) borate, phenyltribenzyl ammonium tetrakis (pentafluorophenyl) borate, dimethylphenyl (3,4-dimethylbenzyl) ammonium tetrakis (pentafluorophenyl) borate, and N,N-diethyl-N-benzylaniline boron tetrafluoride.

[0053] According to an embodiment of the present disclosure, the content of the quaternary ammonium salt compound accounts for 2 to 15 weight % of the cationic polymerizable resin, for example, it can be 2 weight %, 5 weight %, 8 weight %, 10 weight %, 13 weight %, 15 weight %, etc. When the content of the quaternary ammonium salt compound is within this range, the obtained anisotropic conductive film has excellent low-temperature and short-time curing properties and storage stability.

[0054] According to the embodiments of the present disclosure, the film-forming additive component is a component for forming an anisotropic conductive film into a film, and an epoxy resin or a phenoxy resin that is solid at room temperature is used as an essential component, and can be used alone or in combination.

[0055] According to the embodiments of the present disclosure, the solid epoxy resin and phenoxy resin have excellent film-forming properties, processability, and connection reliability at room temperature, do not hinder the cationic polymerization reaction, and can complete the curing reaction at low temperature and in a short time. In addition, even after the reliability test in a high temperature and high humidity environment, it can significantly inhibit the peeling of the connection part of the connection structure.

[0056] According to the embodiments of the present disclosure, the epoxy resin solid at room temperature may be at least one of bisphenol epoxy resin, novolac epoxy resin, naphthalene epoxy resin, and biphenyl epoxy resin. From the viewpoint of film forming properties and processability, bisphenol epoxy resin is preferably used.

[0057] Examples of the phenoxy resin that is solid at room temperature include at least one of fluorene-type phenoxy resins, bisphenol-type phenoxy resins, novolac-type phenoxy resins, naphthalene-type phenoxy resins, and biphenyl-type phenoxy resins.

[0058] According to the embodiments of the present disclosure, further, the following film-forming auxiliary components may also be used: unsaturated polyester resin, saturated polyester resin, polyurethane resin, butadiene resin, polyimide resin, polyamide resin, polyolefin resin, etc.

[0059] According to an embodiment of the present disclosure, the content of the film-forming additive component is preferably 30% to 60% by weight of the thermosetting resin composition, for example, it can be 30%, 35%, 40%, 45%, 50%, 55%, 60% by weight, etc.

[0060] According to the embodiments of the present disclosure, the film-forming additive component can fully exert its film-forming ability within this range.

[0061] According to an embodiment of the present disclosure, the conductive particles may be selected from at least one of nickel, cobalt, silver, copper, gold, palladium, solder, and metal-plated resin particles;

[0062] Preferably, the content of conductive particles is 200 to 70,000 particles / mm 2 Conductive film, for example, can be 200 / mm 2 , 500 pieces / mm 2 , 1000 pieces / mm 2 , 5000pcs / mm 2 , 10000pcs / mm 2 , 30000pcs / mm 2 , 50000pcs / mm 2 , 70000 pieces / mm 2 The content can be measured by counting under an optical microscope.

[0063] According to the embodiments of the present disclosure, the average particle size of the conductive particles should be able to cope with the deviation of the wiring height. In addition, in order to suppress the increase of the on-resistance and the occurrence of short circuits, the average particle size of the conductive particles is preferably 2.5 μm to 30 μm, and more preferably 3 μm to 20 μm. The particle size of the conductive particles can be measured by a general particle size distribution measuring device, and the average particle size can also be measured using a particle size distribution measuring device.

[0064] According to the embodiments of the present disclosure, the thermosetting resin composition may contain inorganic fillers such as silica, stress relaxants such as rubber components, or additives such as coupling agents and leveling agents, depending on the type of circuit board to be connected.

[0065] According to the embodiments of the present disclosure, the amount of inorganic filler can be 1-30wt%, for example, 1wt%, 5wt%, 15wt%, 20wt%, 25wt%, 30wt%, etc. The addition of inorganic filler can reduce the thermal expansion coefficient and stabilize the connection state.

[0066] According to the embodiments of the present disclosure, the amount of stress relaxant can be 5-20wt%, for example, 5wt%, 8wt%, 10wt%, 15wt%, 20wt%, etc. The stress relaxant can reduce the shrinkage stress generated during the curing process to stabilize the connection state.

[0067] According to the embodiments of the present disclosure, the coupling agent is a general term for compounds having both a part that reacts with an organic compound and a part that reacts with an inorganic compound, in particular, the part that reacts with the organic compound is an epoxy group, and the part that reacts with the inorganic substance is a silane (silicon), and a silane coupling agent is preferably used. The amount of the coupling agent can be 0.01 to 5wt%, preferably 0.5 to 2.0wt%, for example, 0.5wt%, 1wt%, 2wt%, 4wt%, 5wt%, etc. The coupling agent can be used to improve the adhesion to the glass interface. Especially under the reliability of high temperature and high humidity, it has the effect of preventing the glass interface from peeling off.

[0068] According to the embodiments of the present disclosure, the amount of the leveling agent can be 0.1-1.0wt%, for example, 0.1wt%, 0.3wt%, 0.6wt%, 0.8wt%, 1.0wt%, etc. The leveling agent has the effect of making the anisotropic conductive film easier to peel off from the release film, and also can make the anisotropic conductive film have a good pre-lamination effect when it is temporarily attached to the circuit board.

[0069] In another aspect of the present disclosure, an anisotropic conductive film is provided, which is prepared by thermally curing the above-mentioned thermal curable resin composition.

[0070] According to the embodiments of the present disclosure, when the anisotropic conductive film is used for conductive connection of electronic components, the connection state after curing can be stabilized under low stress, and the warping of the substrate can be minimized.

[0071] According to an embodiment of the present disclosure, preferably, the temperature of thermal curing is 140-160°C, for example, it can be 140°C, 145°C, 150°C, 155°C, 160°C, etc., and the curing time is within 5 seconds, for example, it can be 1 second, 2 seconds, 3 seconds, 4 seconds, 5 seconds, etc.

[0072] According to an embodiment of the present disclosure, the present disclosure provides a method for manufacturing an anisotropic conductive film, which comprises firstly dispersing an inorganic filler evenly in an organic solvent such as toluene, then dissolving a film-forming additive in the dispersed solution, and mixing and dispersing tetrahydroindene diepoxide, a quaternary ammonium salt compound and conductive particles therein to form a coating, forming the coating into a film by a known film-forming method, and then thermally curing the coating to manufacture the anisotropic conductive film.

[0073] According to the embodiments of the present disclosure, the anisotropic conductive film of the present disclosure can be a single layer or a double layer structure of a layer containing conductive particles and a layer not containing conductive particles. By forming a double layer structure, the particle capture efficiency during connection can be improved, thereby reducing the use of high-priced conductive particles and reducing manufacturing costs.

[0074] According to the disclosed embodiment, the thickness of the anisotropic conductive film can be coated to a thickness that can fully fill the electrode portion of the circuit substrate, and also depends on the size and number of the electrodes. Generally, it can be 3 to 10 μmm thicker than the height of the electrode.

[0075] In another aspect of the present disclosure, a connection structure is provided, which is formed by anisotropically conductively connecting a first electronic component and a second electronic component using the anisotropic conductive film.

[0076] According to the embodiment of the present disclosure, the first electronic component may be, for example, an electrode portion of a first circuit board, and the second electronic component may be, for example, a connection portion of a second printed circuit board.

[0077] According to the embodiments of the present disclosure, the anisotropic conductive film can be preferably used when an anisotropic conductive connection is performed between a first circuit substrate such as an IC chip, COF, or FPC and a second circuit substrate such as a glass circuit substrate, a plastic circuit substrate, a rigid circuit substrate, a ceramic circuit substrate, or a polyimide circuit substrate. In addition, a known method can be used as a method for connecting electronic components of the anisotropic conductive film.

[0078] The thermosetting resin composition, anisotropic conductive film and connection structure disclosed in the present invention provide a method with excellent storage stability and cost-effectiveness for the research of anisotropic conductive film, which has far-reaching significance for the development of adhesive materials in electronic products.

[0079] In order to make the purpose, technical scheme and advantages of the present disclosure more clear, the present disclosure is further described in detail below in conjunction with specific examples. The test materials and reagents used in the following examples, unless otherwise specified, can be obtained from commercial sources. If no specific techniques or conditions are specified in the examples, they are all conventional methods and can be carried out according to the techniques or conditions described in the literature in the field or according to the product instructions.

[0080] Example 1: Thermosetting resin composition

[0081] Tetrahydroindene diepoxide was used as component (A); a quaternary ammonium salt compound (product name CXC-1821, manufactured by King Industries) was used as component (B); and a phenoxy resin (product name YP-50, manufactured by Nippon Steel Chemical Materials Co., Ltd.) was used as component (C). The mixing ratio of each component is shown in Table 1. In addition, conductive particles (C) having an average particle size of 4 μm (trade name: Micropearl, manufactured by Sekisui Chemical Co., Ltd., Ni-plated resin particles) were used and dispersed in an amount of 60,000 particles / mm 2 , a thermosetting resin composition, i.e., an adhesive composition, was obtained. Further, the adhesive composition was applied on a 50 μm thick peeling PET film using a coating device, and hot air dried at 60° C. for 5 minutes to obtain an adhesive layer with a thickness of 18 μm. The mixing ratio of each component is shown in Table 1.

[0082] Example 2: Thermosetting resin composition

[0083] Compared with Example 1, component (A) was changed to tetrahydroindene diepoxide and alicyclic epoxy resin (product name: CELLOXIDE 8000, manufactured by Daicel Corporation), and an adhesive layer was obtained in the same manner as in Example 1. The mixing ratio of each component is shown in Table 1.

[0084] Example 3: Thermosetting resin composition

[0085] Compared with Example 1, the component (C) was changed to a solid epoxy resin (product name YD-020, manufactured by KUKDO CHEMICAL Co., Ltd.), and an adhesive layer was obtained by the same method as in Example 1. Table 1 shows the mixing ratio of each component.

[0086] Comparative Example 1

[0087] Compared with Example 1, component (A) was changed to an alicyclic epoxy resin (product name: CELLOXIDE 8000, manufactured by Daicel Corporation), and an adhesive layer was obtained by the same method as Example 1. The mixing ratio of each component is shown in Table 1.

[0088] Comparative Example 2

[0089] Compared with Example 1, component (B) was changed to a sulfonate compound (product name: SAN-Aid SI-60L, manufactured by Sanshin Chemical Industry Co., Ltd.), and an adhesive layer was obtained in the same manner as in Example 1. Table 1 shows the mixing ratio of each component.

[0090] The performance of the thermosetting resin compositions of the above-mentioned Examples 1 to 3 and Comparative Examples 1 to 2 was tested, and the specific testing method is as follows:

[0091] 1. Differential Scanning Calorimeter (DSC) Measurement

[0092] The adhesive layer obtained in each embodiment and comparative example was measured using differential scanning calorimetry (DSC250, manufactured by TA Corporation). The sample amount was 5 mg, the measurement temperature range was 50-250°C, and the heating rate was 10°C / min. The heat start temperature, heat end temperature, and heat value were measured. The results are shown in Table 1.

[0093] 2. Storage stability evaluation

[0094] The adhesive layer obtained in each example and comparative example was placed in a constant temperature device at 40°C for 24 hours. The adhesive layer after being placed at 40°C was subjected to DSC measurement, and the storage stability was determined based on the calorific value reduction rate. A reduction rate of less than 10% was ○, and a reduction rate of more than 10% was ×. The results are shown in Table 1.

[0095] Heat value reduction rate (%) = [(heat value before 40°C storage - heat value after 40°C storage) / heat value before 40°C storage]

[0096] Example 4: Connection structure preparation

[0097] An IC chip (shape: 1.6mm×15.1mm, bump height: 12μm), a glass substrate (OA-10G manufactured by Nippon Electric Glass Co., Ltd., shape 40mm×20mm, thickness 0.5mm, surface ITO (indium tin oxide) wiring spacing (wiring width 22μm, line spacing width 8μm)), the adhesive layer obtained in each embodiment and comparative example is cut into a size of 2×20mm, and attached to the glass substrate, and heated and pressed under the connection conditions of temperature 140°C and 160°C, pressure and time 60MPa for 5 seconds, and the cured anisotropic conductive film connects the IC chip and the glass substrate to obtain a connected structure.

[0098] The performance test of the connection structure of the above-mentioned embodiment 4 is carried out, and the specific test method is as follows:

[0099] 1. Determination of connection resistance

[0100] The connection resistance after the connection structure is connected is measured, and the connection resistance after exposure to high temperature and high humidity environment (85°C / 85%RH / 500 hours) is measured. The function tester (model: RM3545, manufactured by HIOKI) is used for measurement, and the resistance value when 1mA current flows is measured by the 4-terminal method. After exposure to high temperature and high humidity, the connection resistance value is judged as ○ if it is less than 10Ω, and × if it is greater than 10Ω. The results are shown in Table 1.

[0101] 2. Evaluation of warpage

[0102] The warpage of the glass substrate side of the connected structure connected at 160°C / 60 MPa / 5 seconds was measured. The surface roughness measuring machine (trade name: SE500A, manufactured by Kosaka Laboratory Co., Ltd.) was used to move the contact needle on the back side of the glass substrate to which the IC chip was not connected. The results are shown in Table 1.

[0103] Table 1

[0104]

[0105] ※CELLOXIDE 8000: alicyclic epoxy resin (structure name: diepoxydicyclohexyl)

[0106] ※CXC-1821: Quaternary ammonium salt (structure name: dimethylphenyl (4-methoxybenzyl) ammonium tetrakis (pentafluorophenyl) borate)

[0107] ※SI-60L: Sulfonium salt (structure name: methyl (4-hydroxyphenyl) benzylsulfonium hexafluoroantimonate)

[0108] ※YP-50: Phenoxy resin (bisphenol A type phenoxy resin)

[0109] ※YD-020: Epoxy resin (bisphenol A type epoxy resin)

[0110] As can be seen from Table 1 above, the composition of tetrahydroindene diepoxide and quaternary ammonium salt in Example 1 has a heat generation reduction rate of less than 10% after being stored at 40°C for 24 hours, indicating good storage stability; and in Example 2, another alicyclic epoxy resin is used as a cationic polymerizable resin, and this storage stability can still be maintained. In Example 3, a solid epoxy resin is used as a film-forming additive component, and this storage stability can still be maintained. In Comparative Example 2, since a sulfonate compound is used as a thermal acid generating initiator, the heat generation is greatly reduced after being stored at 40°C for 24 hours, and the storage stability is deteriorated.

[0111] In Example 4, the connection structure obtained by using the thermosetting resin composition of Examples 1 to 3 has a connection resistance value of less than 10Ω after exposure to high temperature and high humidity, even if the connection temperature is a low temperature connection of 140°C, indicating that the connection state is stable and the warping amount of the connection structure is small. The thermosetting resin composition of Comparative Example 1 was used to make a connection structure at a connection temperature of 140°C. Since tetrahydroindene diepoxide was not used, the resistance value was more than 10Ω after 85°C / 85%RH / 500 hours, and the connection state became unstable. The thermosetting resin composition of Comparative Example 2 was used. Although tetrahydroindene diepoxide was used, since a sulfonate compound was used as a thermal acid initiator; when the connection structure was made at connection temperatures of 140°C and 160°C, the resistance value was more than 10Ω after 85°C / 85%RH / 500 hours, and the connection state became unstable.

[0112] In summary, the thermosetting resin composition disclosed in the present invention has excellent storage stability and can be cured at a relatively low temperature (e.g., 140-150°C) and in a short time (e.g., within 5 seconds). Therefore, the connection state of the anisotropic conductive film after curing is stable under low stress, and the warping of the substrate can be minimized, so that a connection structure with good connection reliability can be produced.

[0113] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.

Claims

1. A thermosetting resin composition suitable for thermal curing to prepare an anisotropic conductive film, the composition comprising the following components: (A) a cationic polymerizable resin, comprising tetrahydroindene diepoxide, wherein the content of the tetrahydroindene diepoxide accounts for 10 wt % to 50 wt % of the thermosetting resin composition; (B) a thermal acid generating initiator, comprising a quaternary ammonium salt compound, wherein the content of the quaternary ammonium salt compound accounts for 0.05% to 30% by weight of the cationic polymerizable resin, and the quaternary ammonium salt compound is a salt composed of a quaternary ammonium cation and a borate anion; (C) a film-forming additive component, wherein the content of the film-forming additive component accounts for 20% to 70% by weight of the thermosetting resin composition; (D) conductive particles, wherein the content of the conductive particles is 20 to 100,000 particles / mm 2 Conductive film.

2. The thermosetting resin composition according to claim 1, wherein The content of the tetrahydroindene diepoxide accounts for 10 wt % to 40 wt % of the thermosetting resin composition.

3. The thermosetting resin composition according to claim 1, wherein The quaternary ammonium salt compound is selected from at least one of dimethylphenyl (4-methoxybenzyl) ammonium tetrakis (pentafluorophenyl) borate, dimethylphenyl (4-methylbenzyl) ammonium hexafluorotetrakis (pentafluorophenyl) borate, methylphenyl dibenzylammonium tetrakis (pentafluorophenyl) borate, phenyl tribenzyl ammonium tetrakis (pentafluorophenyl) borate, dimethylphenyl (3, 4-dimethylbenzyl) ammonium tetrakis (pentafluorophenyl) borate, and N, N-diethyl-N-benzylaniline boron tetrafluoride.

4. The thermosetting resin composition according to claim 1 or 3, wherein The content of the quaternary ammonium salt compound accounts for 2 to 15 weight % of the cationic polymerizable resin.

5. The thermosetting resin composition according to claim 1, wherein The content of the film-forming additive component accounts for 30% to 60% by weight of the thermosetting resin composition.

6. The thermosetting resin composition according to claim 1 or 5, wherein The film-forming additive component includes epoxy resin or phenoxy resin which is solid at room temperature.

7. The thermosetting resin composition according to claim 6, wherein The epoxy resin is selected from at least one of bisphenol epoxy resin, novolac epoxy resin, naphthalene epoxy resin and biphenyl epoxy resin; The phenoxy resin is selected from at least one of fluorene-type phenoxy resin, bisphenol-type phenoxy resin, novolac-type phenoxy resin, naphthalene-type phenoxy resin and biphenyl-type phenoxy resin.

8. The thermosetting resin composition according to claim 1, wherein The conductive particles are selected from at least one of nickel, cobalt, silver, copper, gold, palladium, solder, and metal-plated resin particles.

9. The thermosetting resin composition according to claim 8, wherein The content of the conductive particles is 200-70,000 / mm 2 Conductive film.

10. The thermosetting resin composition according to claim 1, wherein The cationic polymerizable resin further includes dicyclohexyl oxide, and the content of the dicyclohexyl oxide accounts for 0 to 50 weight % of the cationic polymerizable resin. 11 . An anisotropic conductive film, produced by thermally curing the thermosetting resin composition according to claim 1 . 12 . The anisotropic conductive film according to claim 11 , wherein the thermal curing temperature is 140-160° C. and the curing time is within 5 seconds.

13. A connection structure, wherein a first electronic component and a second electronic component are anisotropically conductively connected using the anisotropic conductive film according to claim 11 or 12.